Silver-coated copper powder and preparation method and application thereof

Through the method of dropping silver ammonia solution and reducing agent at a differential speed, the problem of poor coating effect of traditional silver-coated copper powder is solved, and the preparation of high-density and uniform silver-coated copper powder is achieved, which is suitable for large-scale production and Significantly improves electromagnetic shielding performance.

CN118832162AInactive Publication Date: 2024-10-25HANGZHOU DIANZI UNIV

Patent Information

Application Number
CN202411313866.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The traditional preparation method of silver-coated copper powder results in poor coating effect, complex process and high cost, making it difficult to meet the needs of industrial production.

Method used

The method of adding silver ammonia solution and reducing agent at a differential speed is used to form fine silver nuclei through the electrode potential difference between metallic copper and silver, and the silver ammonia solution and reducing agent are added dropwise at a specific speed to promote the epitaxial continuity of the silver nuclei. Uniform growth to achieve dense and uniform silver-coated copper powder particles.

Benefits of technology

It improves the coating density and uniformity of the silver-coated copper powder, simplifies the process, reduces the cost, is suitable for large-scale production, and improves the electromagnetic shielding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118832162A_ABST
    Figure CN118832162A_ABST
Patent Text Reader

Abstract

The invention relates to silver-coated copper powder and a preparation method and application thereof. The preparation method comprises the following steps that hydrophilic modified copper powder and a complexing agent are mixed, a first silver-ammonia solution is dropwise added at a first speed, then a second silver-ammonia solution and a reducing agent are dropwise added at the same time at a second speed, and silver-coated copper powder is obtained through solid-liquid separation, cleaning and drying; wherein the ratio of the first speed to the second speed is 1: 3-1: 16. According to the preparation method, the coating compactness and uniformity of the silver-coated copper powder can be improved, meanwhile, the process is simple, safety is high, cost is low, the method is suitable for large-scale production, and the silver-coated copper powder prepared through the preparation method is continuous and smooth in surface, excellent in electromagnetic shielding performance and wide in application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal powders, in particular to silver-coated copper powder and a preparation method and application thereof. Background Art

[0002] Silver-coated copper powder has excellent electromagnetic isolation effect and chemical stability, and is widely favored in the field of electromagnetic shielding materials. At present, the chemical reduction and replacement method is mainly used to prepare silver-coated copper powder, and the surface of the copper powder is silver-plated by reacting with silver coordination ion solution, reducing agent and dispersant. However, the coating effect of silver-coated copper powder obtained by traditional preparation method is poor, which limits the application of silver-coated copper powder.

[0003] In order to improve the coating effect of silver-coated copper powder, the existing technology performs silver coating treatment on copper powder at least twice to improve the density and uniformity of the silver-coated copper powder. However, the preparation process requires repeated switching of the plating solution environment, and the product needs to be repeatedly cleaned in each link, resulting in complex process and high cost, which is difficult to meet the needs of industrial production.

[0004] Therefore, there is an urgent need for a preparation method that can improve the coating density and uniformity of silver-coated copper powder while simplifying the process and reducing costs. Summary of the invention

[0005] Based on this, it is necessary to provide a silver-coated copper powder and a preparation method and application thereof to address the above problems. The preparation method of the present invention can improve the coating density and uniformity of the silver-coated copper powder, and at the same time, the process is simple, the safety is high, the cost is low, and it is suitable for large-scale production. The silver-coated copper powder prepared by the preparation method has a dense and smooth surface, excellent electromagnetic shielding performance, and broad application prospects.

[0006] A method for preparing silver-coated copper powder comprises the following steps: The hydrophilic modified copper powder is mixed with a complexing agent, a first silver ammonia solution is added dropwise at a first speed, and then a second silver ammonia solution and a reducing agent are added dropwise at a second speed, and silver-coated copper powder is obtained through solid-liquid separation, washing, and drying; wherein the ratio of the first speed to the second speed is 1:3-1:16.

[0007] In one embodiment, the first speed is 0.8 mmol / min to 100 mmol / min; And / or, the second speed is 12mmol / min~300mmol / min.

[0008] In one embodiment, the molar ratio of the hydrophilically modified copper powder to the solute in the complexing agent is 1:1.5 to 1:6.5; and / or, the molar ratio of the solute in the first silver ammonia solution to the solute in the complexing agent is 1:12 to 1:40; And / or, the molar ratio of the solute in the second silver ammonia solution to the solute in the reducing agent is 1:1~6.5:1.

[0009] In one embodiment, the molar ratio of the solute in the first silver ammonia solution to the solute in the second silver ammonia solution is 1:2.5 to 1:3.5; And / or, the concentration of the first silver ammonia solution is 0.2 mol / L to 0.4 mol / L; And / or, the concentration ratio of the first silver ammonia solution to the second silver ammonia solution is 1:1~1:3.

[0010] In one embodiment, the complexing agent is selected from at least one of trisodium citrate solution, ethylenediaminetetraacetic acid solution and disodium ethylenediaminetetraacetic acid solution; And / or, the reducing agent is selected from at least one of a fructose solution, a glucose solution and an ascorbic acid solution.

[0011] In one embodiment, the concentration of the complexing agent is 0.1wt%~4wt%; And / or, the concentration of the reducing agent is 3mmol / L~18mmol / L.

[0012] In one embodiment, the reaction time after the first silver ammonia solution is added dropwise is 5 min to 8 min; And / or, the reaction time after the second silver ammonia solution and the reducing agent are added dropwise is 20 min to 40 min.

[0013] In one embodiment, the hydrophilic modified copper powder is prepared by mixing an emulsifier with copper powder, and the mixing reaction satisfies at least one of the following conditions: (1) The particle size of the copper powder is 1 μm to 50 μm; (2) The mass ratio of the copper powder to the emulsifier is 1:30 to 1:500; (3) The concentration of the emulsifier is 0.01wt%~0.15wt%; (4) The emulsifier is selected from at least one of gelatin solution, gum arabic solution, fish glue solution and alkylphenol polyoxyethylene ether solution.

[0014] A silver-coated copper powder prepared by the preparation method as described above.

[0015] An electromagnetic shielding sheet comprises an organic matrix and the above-mentioned silver-coated copper powder distributed in the organic matrix.

[0016] The preparation method adopts a differential titration strategy when adding silver ammonia solution twice. First, the electrode potential difference between metallic copper and silver is utilized to induce uniform displacement of the copper powder surface by slowly adding silver ammonia solution to form fine silver cores. Subsequently, the silver ammonia solution and a reducing agent are added at a specific speed to effectively increase the driving force for silver growth and promote continuous and uniform epitaxial growth of the silver core, thereby achieving dense and uniform coating of core-shell type silver-coated copper powder particles.

[0017] Therefore, the preparation method provided by the present invention can improve the coating density and uniformity of the silver-coated copper powder, and has a simple process, high safety, low cost, and is suitable for large-scale production. The silver-coated copper powder prepared by the present invention has high surface coating density and uniformity, excellent electromagnetic shielding performance, and broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0019] Figure 1 The X-ray diffraction pattern of the silver-coated copper powder prepared in Example 1 of the present invention; Figure 2 This is a scanning electron microscope image of the silver-coated copper powder prepared in Example 1 of the present invention; Figure 3 This is a scanning electron microscope image of the silver-coated copper powder prepared in Example 4 of the present invention; Figure 4 This is a scanning electron microscope image of the silver-coated copper powder prepared in Comparative Example 1 of the present invention; Figure 5 This is a scanning electron microscope image of the silver-coated copper powder prepared in Comparative Example 2 of the present invention; Figure 6 This is a characterization diagram of the electromagnetic shielding performance of the electromagnetic shielding sheet prepared in Application Example 1 of the present invention in the X-band and Ku-band. DETAILED DESCRIPTION

[0020] For ease of understanding of the present invention, the present invention will be described in more detail below. However, it should be understood that the present invention can be implemented in many different forms and is not limited to the embodiments or examples described herein. On the contrary, the purpose of providing these embodiments or examples is to make the understanding of the disclosure of the present invention more thorough and comprehensive.

[0021] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific implementation methods or embodiments, and are not intended to limit the present invention. The optional scope of the term "and / or" used herein includes any one of two or more related listed items, and also includes any and all combinations of related listed items, and the combinations include any two related listed items, any more related listed items, or all related listed items.

[0022] A method for preparing silver-coated copper powder comprises the following steps: S1, mixing the hydrophilic modified copper powder with a complexing agent, and adding a first silver ammonia solution dropwise at a first speed; S2, simultaneously adding a second silver ammonia solution and a reducing agent at a second speed, and obtaining silver-coated copper powder through solid-liquid separation, washing, and drying; wherein the ratio of the first speed to the second speed is 1:3-1:16.

[0023] The ratio of the first speed to the second speed includes but is not limited to any point value among 1:3.1, 1:3.5, 1:4, 1:5, 1:7, 1:9, 1:10, 1:12, 1:14, 1:16 or a range value between any two of them.

[0024] Preferably, the ratio of the first speed to the second speed is 1:5-1:8.

[0025] In step S1, the electrode potential difference between metallic copper and silver is utilized to induce uniform replacement of the copper powder surface by slowly dropping a silver ammonia solution, thereby forming fine silver nuclei on the copper powder surface; at this time, the growth rate of the silver nuclei is slow, and as the reaction time increases, the effective sites on the copper powder surface gradually decrease, resulting in a decrease in the efficiency of the replacement reaction, and the silver ammonia ions are enriched on the copper powder surface. The complexing agent added in the present invention can form a structurally stable complex with the enriched silver ammonia ions, thereby reducing the precipitation of impurities such as silver nitride and silver imide generated by the decomposition of the silver ammonia ions.

[0026] It should be noted that the present invention hydrophilizes the copper powder by an existing method to obtain hydrophilically modified copper powder, which effectively improves the dispersibility of the copper powder and is conducive to improving the efficiency of the replacement reaction. Specifically, the copper powder is mixed with an emulsifier, filtered to obtain the hydrophilically modified copper powder, and stirred for 10 min to 30 min after mixing to improve the modification effect.

[0027] In one embodiment, the particle size of the copper powder is 1 μm to 50 μm, which is beneficial to increase the specific surface area, increase the adsorption sites on the copper powder surface, promote the replacement reaction, and further improve the coating density and uniformity of the silver-coated copper powder.

[0028] In one embodiment, the mass ratio of the copper powder to the emulsifier is 1:30 to 1:500.

[0029] Specifically, the concentration of the emulsifier is 0.01wt%~0.15wt%.

[0030] Specifically, the emulsifier is selected from at least one of a gelatin solution, an arabic gum solution, an isinglass solution, and an alkylphenol polyoxyethylene ether (OP-10) solution.

[0031] In order to increase the number and uniformity of silver nuclei grown on the copper powder surface and reduce the detachment of silver from the copper powder surface, the first speed is preferably 0.01mmol / min~100mmol / min, including but not limited to any point value among 0.01mmol / min, 0.05mmol / min, 0.1mmol / min, 0.5mmol / min, 1mmol / min, 5mmol / min, 10mmol / min, 20mmol / min, 30mmol / min, 50mmol / min, 80mmol / min, 100mmol / min or any range value between two thereof.

[0032] More preferably, the first speed is 0.8 mmol / min to 100 mmol / min.

[0033] More preferably, the first speed is 0.8 mmol / min to 50 mmol / min.

[0034] In one embodiment, the molar ratio of the hydrophilically modified copper powder to the solute in the complexing agent is 1:1.5~1:6.5, which is beneficial to reduce the concentration of silver ammonium ions in the reaction system, promote the slow reduction of silver ammonium ions on the surface of the copper powder, thereby promoting the formation of uniform and fine silver nuclei on the surface of the copper powder, and at the same time, it is beneficial to draw the silver ammonium ions to the surface of the copper powder, avoid the free growth of silver element, and thus improve the density and uniformity of the silver shell.

[0035] In one embodiment, the molar ratio of the first silver ammonia solution to the solute in the complexing agent is 1:12-1:40, which is conducive to forming a structurally stable complex with the silver ammonia ions enriched on the surface of the copper powder, reducing the precipitation of impurities such as silver nitride and silver imide produced by the decomposition of the enriched silver ammonia ions, further improving the density and uniformity of the silver shell layer, and improving the performance stability of the silver-coated copper powder.

[0036] Specifically, the concentration of the complexing agent is 0.1wt%~4wt%.

[0037] The prior art improves the smoothness and uniformity of the surface of the silver-coated copper powder by adding strong complexing agents such as thiourea and thiosemicarbazide into the plating solution. However, the strong complexing agents are highly toxic and easily cause environmental pollution. The complexing agent of the present invention is preferably at least one of trisodium citrate solution, ethylenediaminetetraacetic acid (EDTA) solution and disodium ethylenediaminetetraacetic acid (EDTA-2Na) solution. The carboxylic acid in the complexing agent effectively improves the reaction with the silver ammonium ions enriched on the surface of the copper powder, reduces the precipitation of impurities such as silver nitride and silver imide produced by the decomposition of the silver ammonium ions, and has good safety and environmental protection.

[0038] Specifically, the concentration of the first silver ammonia solution is 0.2 mol / L to 0.4 mol / L.

[0039] In one embodiment, the reaction time after the first silver ammonia solution is added dropwise is 5 min to 8 min.

[0040] It should be noted that the present invention has no special restrictions on the temperature of the above-mentioned replacement reaction. Those skilled in the art can select and adjust it according to actual production conditions or product requirements. In order to improve production efficiency and reduce costs, the present invention makes the process more suitable for industrial production. The temperature of the reduction reaction is room temperature; the efficiency of the replacement reaction can be improved by stirring, oscillating, etc., and the present invention has no special restrictions on this.

[0041] In step S2, the silver ammonia solution and the reducing agent are added dropwise at a specific speed. At this time, the dropping speed is relatively fast, which is not only conducive to improving the driving force for silver growth and promoting the epitaxial continuous densification growth of the silver shell along the silver core formed in step S1, but also can ensure the smooth progress of the reduction reaction, and effectively avoid defects such as agglomeration of the silver shell, loose and sparse silver shell, and separation of the silver element from the copper powder surface due to excessively fast reduction reaction, thereby obtaining densely and uniformly coated core-shell type silver-coated copper powder particles.

[0042] Preferably, the second speed is 12mmol / min~300mmol / min, which effectively promotes the epitaxial continuous densification growth of the silver core, and prevents the local reaction from being accelerated due to excessive drop acceleration, so that the locally generated silver particles are more concentrated and agglomerate and agglomerate, which is conducive to achieving a silver-coated copper powder with a continuous and smooth surface. The second speed includes but is not limited to any point value of 12mmol / min, 13mmol / min, 15mmol / min, 20mmol / min, 30mmol / min, 40mmol / min, 50mmol / min, 80mmol / min, 120mmol / min, 150mmol / min, 200mmol / min, 220mmol / min, 250mmol / min, 300mmol / min or any range value between two of them.

[0043] More preferably, the second speed is 15 mmol / min to 300 mmol / min.

[0044] More preferably, the second speed is 15 mmol / min to 150 mmol / min.

[0045] In one embodiment, the molar ratio of the second silver ammonia solution to the solute in the complexing agent is 1:1.8-1:15, including but not limited to any point value of 1:1.8, 1:2.5, 1:3, 1:4, 1:5, 1:7, 1:9, 1:10, 1:12, and 1:15, or a range value between any two of them, which is beneficial to promote the reduction reaction of silver ammonia ions on the surface of the copper powder, and is beneficial to avoid defects such as loose and sparse silver shells and the separation of silver from the surface of the copper powder, thereby improving the density and uniformity of the silver shell.

[0046] In order to further improve the driving force of silver growth, improve the utilization rate of silver ammonium ions, promote the epitaxial continuous densification growth of the silver shell along the silver core, and at the same time ensure the smooth progress of the reduction reaction, avoid the reduction reaction too fast and cause the silver shell to agglomerate, the silver shell is loose and sparse, and the silver element is separated from the copper powder surface and other defects, so as to achieve a silver-coated copper powder with a continuous and smooth surface, the molar ratio of the solute in the second silver ammonia solution to the solute in the reducing agent is 1:1~6.5:1, including but not limited to any point value of 1:1, 1.5:1, 2:1, 3:1, 3.5:1, 5:1, 6.5:1 or any range value between two of them.

[0047] In one embodiment, the reducing agent is selected from an organic reducing agent. The present invention adopts an organic reducing agent with weaker reducing property to effectively increase the driving force of silver growth. While ensuring the reduction reaction, it avoids the defects such as the loose and sparse silver shell layer generated due to the rapid acceleration of the reduction process and the separation of the silver element from the copper powder surface. In addition, the reducing agent has good safety, effectively avoids environmental pollution and reduces wastewater discharge costs, which is conducive to simplifying the process, improving safety and reducing costs.

[0048] Specifically, the reducing agent is selected from at least one of a fructose solution, a glucose solution and an ascorbic acid solution.

[0049] More preferably, the reducing agent is selected from a glucose solution, wherein glucose contains a molecular structure of a monoaldehyde group and multiple hydroxy groups, wherein the aldehyde group is conducive to promoting the reduction reaction, while the hydroxyl group is conducive to stabilizing the alkaline environment of the liquid phase, thereby ensuring the smooth progress of the reduction process.

[0050] Specifically, the concentration of the reducing agent is 3mmol / L~18mmol / L.

[0051] In one embodiment, the ratio of the concentration of the first silver ammonia solution to the concentration of the second silver ammonia solution is 1:1 to 1:3.

[0052] It should be noted that the first silver ammonia solution and the second silver ammonia solution used in the present invention can be homemade or commercially available, and the present invention has no particular limitation on this.

[0053] In order to ensure stable adsorption and growth of the silver shell particles at each stage of the reaction, the molar ratio of the solute in the first silver ammonia solution to the solute in the second silver ammonia solution is 1:2.5~1:3.5.

[0054] In one embodiment, the reaction time after the second silver ammonia solution and the reducing agent are added dropwise is 20 min to 40 min.

[0055] It should be noted that the present invention has no special restrictions on the temperature of the above-mentioned reduction reaction. Those skilled in the art can select and adjust it according to actual production conditions or product requirements. In order to improve production efficiency and reduce costs, the present invention makes the process more suitable for industrial production. The temperature of the reduction reaction is room temperature; the efficiency of the reduction reaction can be improved by stirring, oscillating, etc., and the present invention has no special restrictions on this.

[0056] In one embodiment, after the reduction reaction is completed, solid-liquid separation is performed by filtering, the obtained solid is washed with deionized water 2 to 3 times, and vacuum dried at 40° C. to 60° C. for 6 h to 12 h.

[0057] In summary, the preparation method provided by the present invention optimizes the preparation process of traditional silver-coated copper powder through the synergistic effect of the liquid phase components and the differential dripping method, realizes the efficient preparation of silver-coated copper powder under a green and streamlined process, effectively improves the coating density and uniformity of the silver-coated copper powder, and has a simple process, high safety, and low cost, and is suitable for large-scale production.

[0058] The present invention also provides a silver-coated copper powder prepared by the preparation method as described above. The silver-coated copper powder has high surface coating density and uniformity, excellent electromagnetic shielding performance, and broad application prospects.

[0059] The present invention also provides an electromagnetic shielding sheet, comprising an organic matrix and the silver-coated copper powder as described above distributed in the organic matrix. The electromagnetic shielding sheet has excellent electromagnetic shielding performance and strong performance stability, and has great commercial application and promotion value.

[0060] The method for preparing the electromagnetic shielding sheet of the present invention adopts the existing technology in the field, and the present invention has no special restrictions on this. For example, an organic matrix is ​​mixed with the above-mentioned silver-coated copper powder, and the electromagnetic shielding sheet is obtained by calendering, casting, spin coating and curing. The present invention has no special restrictions on the thickness of the electromagnetic shielding sheet, such as 0.8mm, 1mm, 1.5mm, etc.

[0061] Specifically, the organic matrix is ​​selected from at least one of epoxy resin, polyethylene resin, silicone oil and silicone gel.

[0062] Specifically, the mass ratio of the organic matrix to the silver-coated copper powder is 1:2-1:3.

[0063] Hereinafter, the silver-coated copper powder and its preparation method and application will be further described through the following specific examples.

[0064] Example 1 30 g of spherical copper powder with a particle size of 15 μm was placed in 240 mL of 0.02 wt% gum arabic solution and stirred for 15 min, and hydrophilically modified copper powder was obtained after filtration; under stirring conditions, the hydrophilically modified copper powder was placed in 300 mL of 0.5 wt% trisodium citrate solution, and then, silver ammonia solution (concentration of 0.4 mol / L) was added dropwise at a rate of 5 mmol / min, and the reaction was carried out for 5 min after the addition was completed; wherein, the molar ratio of the silver ammonia ions added in this step to trisodium citrate was 1:40, and the molar ratio of the hydrophilically modified copper powder to trisodium citrate was 1:4.5.

[0065] Under stirring conditions, silver ammonia solution (concentration of 0.6 mol / L) and glucose solution (concentration of 0.3 mol / L) are simultaneously added dropwise to the solution of the previous step at a speed of 50 mmol / min, the ratio of the first speed to the second speed is 1:10, and the reaction is carried out for 25 minutes after the addition is completed to obtain a silver-coated copper powder suspension; wherein the molar ratio of the silver ammonia ions added dropwise in the previous step to the silver ammonia ions added dropwise in this step is 1:3, and the molar ratio of the silver ammonia ions added dropwise in this step to the glucose is 1:1.

[0066] The obtained silver-coated copper powder suspension was filtered, and the obtained solid matter was washed with deionized water for 3 times, and then placed at 40° C. for 6 hours in vacuum drying to obtain silver-coated copper powder.

[0067] The X-ray diffraction pattern of the silver-coated copper powder obtained in Example 1 is as follows: Figure 1 As shown, it can be seen that the obtained particles only have diffraction peaks of silver and copper elements, and no impurity phase is generated; the scanning electron microscope image of the silver-coated copper powder obtained in Example 1 is as follows Figure 2 As shown, it can be seen that the surface of the spherical copper powder particles is continuously and evenly coated with nano silver particles.

[0068] Example 2 20 g of spherical copper powder with a particle size of 15 μm was placed in 150 mL of 0.10 wt% gum arabic solution and stirred for 15 min, and hydrophilically modified copper powder was obtained after filtration; under stirring conditions, the hydrophilically modified copper powder was placed in 200 mL of 2.5 wt% trisodium citrate solution, and then, silver ammonia solution (concentration of 0.3 mol / L) was added dropwise at a rate of 0.8 mmol / min, and the reaction was carried out for 6 min after the addition was completed; wherein, the molar ratio of the silver ammonia ions added in this step to trisodium citrate was 1:35, and the molar ratio of the hydrophilically modified copper powder to trisodium citrate was 1:2.

[0069] Under stirring conditions, a silver ammonia solution (with a concentration of 0.9 mol / L) and an ascorbic acid solution (with a concentration of 0.3 mol / L) are simultaneously added dropwise to the solution of the previous step at a speed of 12 mmol / min, the ratio of the first speed to the second speed is 1:15, and the reaction is carried out for 30 minutes after the addition is completed to obtain a silver-coated copper powder suspension; wherein the molar ratio of the silver ammonia ions added dropwise in the previous step to the silver ammonia ions added dropwise in this step is 1:2.5, and the molar ratio of the silver ammonia ions added dropwise in this step to the ascorbic acid is 1:3.

[0070] The obtained silver-coated copper powder suspension was filtered, and the obtained solid matter was washed with deionized water for 3 times, and then placed at 50° C. for vacuum drying for 10 h to obtain silver-coated copper powder.

[0071] Example 3 6 g of spherical copper powder with a particle size of 5 μm was placed in 150 mL of 0.12 wt% gelatin solution and stirred for 12 min, and hydrophilically modified copper powder was obtained after filtration; under stirring conditions, the hydrophilically modified copper powder was placed in 150 mL of 3.0 wt% EDTA solution, and then silver ammonia solution (concentration of 0.2 mol / L) was added dropwise at a rate of 50 mmol / min, and the reaction was carried out for 5 min after the addition was completed; wherein, the molar ratio of the silver ammonia ions added in this step to EDTA was 1:200, and the molar ratio of the hydrophilically modified copper powder to EDTA was 1:40.

[0072] Under stirring conditions, silver ammonia solution (concentration of 0.25 mol / L) and glucose solution (concentration of 0.25 mol / L) are simultaneously added dropwise to the solution of the previous step at a speed of 150 mmol / min, the ratio of the first speed to the second speed is 1:3, and the reaction is carried out for 35 minutes after the addition is completed to obtain a silver-coated copper powder suspension; wherein the molar ratio of the silver ammonia ions added dropwise in the previous step to the silver ammonia ions added dropwise in this step is 1:3.5, and the molar ratio of the silver ammonia ions added dropwise in this step to the glucose is 1:2.5.

[0073] The obtained silver-coated copper powder suspension was filtered, and the obtained solid matter was washed twice with deionized water and then dried under vacuum at 50° C. for 12 h to obtain silver-coated copper powder.

[0074] Example 4 The difference between Example 4 and Example 1 is that an equal amount of hydrazine hydrate solution is used instead of glucose solution.

[0075] The scanning electron microscope image of the silver-coated copper powder obtained in Example 4 is as follows: Figure 3 As shown, it can be seen that the silver shell layer on the surface of the spherical copper powder particles is relatively loose. This is because the reducing property of hydrazine hydrate is strong, which makes the epitaxial growth rate of the silver particles faster, resulting in the subsequent generated silver particles unable to form close contact with the previously generated silver particles in time.

[0076] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that the first speed is 200 mmol / min, the second speed is 50 mmol / min, and the ratio of the first speed to the second speed is 4:1.

[0077] The scanning electron microscope image of the silver-coated copper powder prepared in Comparative Example 1 is as follows: Figure 4 As shown, it can be seen that there are fewer silver particles on the surface of the copper powder, and the coating density of the silver shell is low and relatively rough. This is because the droplet acceleration of the first silver ammonia solution is too fast, causing part of the silver element to detach from the surface of the copper powder, thereby reducing the number of silver nuclei formed on the surface of the copper powder, resulting in the final silver-coated copper powder containing some free silver element and a rough silver shell.

[0078] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the first speed is 1 mmol / min, the second speed is 20 mmol / min, and the ratio of the first speed to the second speed is 1:20.

[0079] The scanning electron microscope image of the silver-coated copper powder prepared in Comparative Example 2 is as follows: Figure 5 As shown in the figure, due to the high ratio of the second speed, when the second silver ammonia solution is added, the growth sites of the newly generated silver particles are relatively reduced, and some shell particles grow abnormally, resulting in uneven morphology of the composite particles and loose packaging.

[0080] Application Examples The silver-coated copper powder obtained in all the embodiments and comparative examples is evenly mixed with an organic matrix, and an electromagnetic shielding sheet is obtained after calendering, wherein the organic matrix of Application Example 2 adopts silicone oil, and the organic matrix of the other application examples and application comparative examples adopts epoxy resin; the mass ratio of the silver-coated copper powder to the organic matrix in Application Example 3 is 1.5:1, and the mass ratio of the silver-coated copper powder to the organic matrix in the other application examples and application comparative examples is 2:1; the thickness of the electromagnetic shielding sheet obtained in Application Example 2 is 0.8 mm, the thickness of the electromagnetic shielding sheet obtained in Application Example 3 is 0.8 mm, and the thickness of the electromagnetic shielding sheet obtained in the other application examples and application comparative examples is 1.5 mm.

[0081] The electromagnetic shielding sheets prepared in all application examples were subjected to electromagnetic shielding tests in the 8.2 GHz to 18 GHz band by the waveguide method. The electromagnetic shielding performance characterization results of the electromagnetic shielding sheet prepared in Example 1 are as follows: Figure 6 As shown, it can be seen that the electromagnetic shielding sheet has excellent shielding performance in the 8.2GHz~18GHz band, and the highest shielding effectiveness reaches 106.5dB; under the same test conditions, the highest shielding effectiveness of application examples 2 to 4 are 102dB, 100dB, and 105dB respectively, while the highest shielding effectiveness of application examples 1 to 3 are 78dB, 83dB, and 66dB respectively, which are significantly lower than the highest shielding effectiveness of all application examples. In summary, the silver-coated copper powder prepared by the preparation method of the present invention has a continuous and smooth surface, excellent electromagnetic shielding performance, and broad application prospects.

[0082] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0083] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing silver-coated copper powder, characterized in that: The preparation method comprises the following steps: The hydrophilically modified copper powder is mixed with a complexing agent, a first silver ammonia solution is added dropwise at a first speed, and then a second silver ammonia solution and a reducing agent are added dropwise simultaneously at a second speed. Silver-coated copper powder is obtained through solid-liquid separation, washing, and drying; wherein the ratio of the first speed to the second speed is 1:3 to 1:

16.

2. The method for preparing silver-coated copper powder according to claim 1, wherein The first speed is 0.8mmol / min~100mmol / min; And / or, the second speed is 12 mmol / min to 300 mmol / min.

3. The method for preparing silver-coated copper powder according to claim 1, wherein The molar ratio of the hydrophilically modified copper powder to the solute in the complexing agent is 1:1.5 to 1:6.5; and / or, the molar ratio of the solute in the first silver ammonia solution to the solute in the complexing agent is 1:12 to 1:40; And / or, the molar ratio of the solute in the second silver ammonia solution to the solute in the reducing agent is 1:1 to 6.5:

1.

4. The method for preparing the silver-coated copper powder according to claim 1 or claim 3, wherein: The molar ratio of the solute in the first silver ammonia solution to the solute in the second silver ammonia solution is 1:2.5 to 1:3.5; And / or, the concentration of the first silver ammonia solution is 0.2 mol / L to 0.4 mol / L; And / or, the ratio of the concentration of the first silver ammonia solution to the concentration of the second silver ammonia solution is 1:1 to 1:

3.

5. The method for preparing silver-coated copper powder according to claim 1, wherein The complexing agent is selected from at least one of trisodium citrate solution, ethylenediaminetetraacetic acid solution and disodium ethylenediaminetetraacetic acid solution; And / or, the reducing agent is at least one selected from fructose solution, glucose solution and ascorbic acid solution.

6. The method for preparing the silver-coated copper powder according to claim 1 or claim 5, wherein: The concentration of the complexing agent is 0.1wt%~4wt%; And / or, the concentration of the reducing agent is 3 mmol / L to 18 mmol / L.

7. The method for preparing silver-coated copper powder according to claim 1, wherein After the first silver ammonia solution is added dropwise, the reaction time is 5 min to 8 min; And / or, the reaction time after the second silver ammonia solution and the reducing agent are added dropwise is 20 min to 40 min.

8. The method for preparing silver-coated copper powder according to claim 1, wherein The hydrophilically modified copper powder is prepared by a mixing reaction between an emulsifier and copper powder, and the mixing reaction satisfies at least one of the following conditions: (1) The particle size of the copper powder is 1 μm to 50 μm; (2) The mass ratio of the copper powder to the emulsifier is 1:30 to 1:500; (3) The concentration of the emulsifier is 0.01wt%~0.15wt%; (4) The emulsifier is selected from at least one of gelatin solution, gum arabic solution, fish glue solution and alkylphenol polyoxyethylene ether solution.

9. Silver-coated copper powder prepared by the preparation method according to any one of claims 1 to 8.

10. An electromagnetic shielding sheet, characterized in that: The invention comprises an organic matrix and the silver-coated copper powder as claimed in claim 9 distributed in the organic matrix.

Citation Information

Patent Citations

  • Preparation method of silver coated copper powder for electronic slurry

    CN102328076A

  • Preparation method of silver-coated copper powder with good conductivity

    CN115971480A

  • Preparation method of silver-coated copper powder with core-shell structure and low silver content

    CN116550974A

  • Preparation method for realizing compact coating of silver-coated copper powder under low silver content

    CN117399617A

  • Preparation method of superfine silver-coated copper powder for conductive paste

    CN118080848A

Cited By

  • Corrosion-resistant flaky silver-coated copper powder, preparation method thereof and electromagnetic shielding shell

    CN119927207A

  • A corrosion-resistant flaky silver-coated copper powder, its preparation method, and an electromagnetic shielding housing

    CN119927207B

  • Method for preparing silver-coated copper adhesive by using silver methanesulfonate as silver source

    CN121379464A

  • High-density superfine silver-coated copper composite material and preparation method thereof

    CN121696391A