Laser welding method and laser welding system

By using the laser welding method when welding electrical equipment, combining the first wavelength laser from 800nm ​​to 1200nm and the second wavelength laser from 400nm to 500nm, the problem of many pores in the welding part is solved, the welding strength is improved and the cost and conductivity are reduced , achieving efficient welding effects.

CN118832291AInactive Publication Date: 2024-10-25HONDA MOTOR CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410435857.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-25
Filing Date
2024-04-11
Publication Date
2024-10-25
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

In the existing technology, when welding electrical equipment, the copper conductor with high oxygen content causes more pores to be formed in the welding part, resulting in insufficient strength and increased resistance. When deoxidizing materials are used to suppress the generation of pores, the cycle time is prolonged, the cost is increased, and the conductivity is reduced. problem.

Method used

The laser welding method is used to irradiate the processing object with a first wavelength laser of 800nm ​​to 1200nm and a second wavelength laser of 400nm to 500nm respectively. The first wavelength laser is used to perform preliminary melting, and the second wavelength laser is used to maintain the melting amount of the melted area. , control the laser output power to reduce the generation of pores.

Benefits of technology

It effectively reduces the number of pores in the welding part, improves the welding strength, avoids the cost increase and decrease in conductivity caused by the use of deoxidized materials, and improves the welding efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118832291A_ABST
    Figure CN118832291A_ABST
Patent Text Reader

Abstract

The present invention provides a laser welding method for performing welding by irradiating a laser beam to a workpiece. The method includes a first step of irradiating a first laser beam to a processing object to melt the processing object, and a second step of irradiating a second laser beam different from the first laser beam to a melting region melted by the first step to maintain the melting amount of the melting region. The laser light is irradiated by a first laser light configuration in which the output power of the first laser light is reduced by a predetermined amount and the output power of the second laser light is set to be smaller than the output power of the first laser light after a predetermined time has elapsed from the start of irradiation of the first laser light, or a second laser light configuration in which the output power of the second laser light is set to be smaller than the output power of the first laser light. The first laser comprises IR laser of a first output power, and the second laser comprises IR laser of which the output power is smaller than that of the first output power and / or is in a defocused state.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a laser welding method and a laser welding system. Background Art

[0002] Electrical equipment such as rotating motors and power conversion devices require a large current to flow through with low resistance, and use thick conductors such as flat wires and conductor plates, which are joined together for use (for example, see Patent Document 1). When such conductors and conductor plates are made of copper with a relatively high oxygen content, many pores are formed in the welded portion, resulting in problems such as insufficient strength and increased resistance. Therefore, in the welding method described in Patent Document 1, by melting the conductor to be joined and adding a phosphorus-containing filler (deoxidizing material), welding with suppressed pores can be performed.

[0003] However, in the case of bonding using a deoxidizing material, the bonding cycle time is prolonged and the material cost of the deoxidizing material is increased, which leads to an increase in processing cost. In addition, the deoxidizing material also causes a decrease in electrical conductivity.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent document 1: Patent publication No. 7162144 (JP7162144B2). Summary of the invention

[0007] A laser welding method according to a technical solution of the present invention is a laser welding method for performing welding by irradiating a processing object with a laser, and includes a first step and a second step. In the first step, a first laser is irradiated onto the processing object to melt the processing object. In the second step, a second laser different from the first laser is irradiated onto a molten area melted by the first step to maintain the melting amount of the molten area. The method includes a first laser configuration (A) or a second laser configuration (B). In the first laser configuration (A), after a predetermined time has passed since the irradiation of the first laser began, the output power of the first laser is reduced by a predetermined amount, and the output power of the second laser is set to be smaller than the output power of the first laser. In the second laser configuration (B), the first laser includes a laser having a first wavelength of greater than 800 nm and less than 1200 nm and a first output power, and the second laser includes a laser having the first wavelength and an output power smaller than the first output power and / or being in a defocused state.

[0008] A laser welding system according to another technical solution of the present invention comprises: a first laser generating device that generates a first laser; a second laser generating device that generates a second laser different from the first laser; an optical device that irradiates the first laser and the second laser onto a processing object; and a control device that controls the operation of the first laser generating device, the second laser generating device, and the optical device. The control device controls the operation of the first laser generating device, the second laser generating device, and the optical device so that the first laser is irradiated onto the processing object to melt the processing object, and then the second laser is irradiated onto the melted molten area to maintain the melting amount of the molten area. BRIEF DESCRIPTION OF THE DRAWINGS

[0009] The objects, features and advantages of the present invention will be further clarified through the following description of the embodiments in conjunction with the accompanying drawings.

[0010] Figure 1 This is a block diagram showing a schematic configuration of a laser welding system according to the present embodiment.

[0011] Figure 2 This is a diagram showing an example of a processing target of laser welding.

[0012] Figure 3 This is a flowchart for explaining the control of laser welding in the embodiment.

[0013] Figure 4 is a schematic diagram showing the first scanning method.

[0014] Figure 5 This is a diagram showing an end portion where a molten region is formed, as viewed from the side of the conductor.

[0015] Figure 6 is a schematic diagram showing the second scanning method.

[0016] Figure 7 This is a diagram showing an end portion where a merged fused region is formed, as viewed from the side of the conductor.

[0017] Figure 8 This is a graph qualitatively illustrating the relationship between laser irradiation and the amount of melting and the amount of pores.

[0018] Fig. 9 It is a diagram for explaining the discharge of air into the atmosphere from the pores.

[0019] Fig.10 It is a diagram for explaining modification example 1.

[0020] Fig.11 This is a diagram for explaining Modification Example 2.

[0021] Fig.12This is a diagram showing an example of reducing the output power in multiple stages.

[0022] Fig.13 This is a diagram showing an example of continuously reducing the output power.

[0023] Fig.14 This is a diagram for explaining Modification Example 3.

[0024] Fig.15 This is a flowchart for explaining Modification Example 4.

[0025] Fig.16 This is a diagram showing a state where plate materials are overlapped and welded. DETAILED DESCRIPTION

[0026] The specific implementation of the present invention is described below with reference to the accompanying drawings. The following description and the accompanying drawings are examples for illustrating the present invention. In order to make the description clear, they are appropriately omitted and simplified. In addition, in the following description, the same or similar elements and processes are sometimes marked with the same figure numbers, and repeated descriptions are omitted. It should be noted that the content described below is only an example of an implementation of the present invention, and the present invention is not limited to the following implementation, and can also be implemented in various other ways.

[0027] Figure 1 1 is a block diagram showing a schematic structure of a laser welding system 1 according to the present embodiment. The laser welding system 1 includes a first laser generator 10, a second laser generator 11, an optical device 12, a control device 13, and an optical fiber 14. The laser generators 10 and 11 each include a laser oscillator. The laser generator 10 generates a first wavelength laser having a wavelength of 800 nm or more and 1200 nm or less. The laser generator 11 generates a second wavelength laser having a wavelength of 400 nm or more and 500 nm or less.

[0028] The optical fiber 14 conducts the laser light output from the laser generating devices 10 and 11 to the optical device 12. The optical device 12 is an optical system for irradiating the laser light input from the laser generating devices 10 and 11 to the processing object 15. Although not shown in the figure, the optical device 12 includes a collimating lens, a focusing lens, a reflecting mirror, a filter, etc. The optical device 12 is configured to be able to scan the laser light on the processing object 15.

[0029] The control device 13 controls the operation of the laser generators 10 and 11 and the optical device 12. The control device 13 includes a CPU, a memory (RAM (random access memory) and a ROM (read only memory)), etc., and controls the laser welding system 1 by executing a program stored in the memory by the CPU. The control device 13 controls the output power of the lasers of the laser generators 10 and 11. The control device 13 controls the focal position of the laser and the scanning trajectory of the optical device 12.

[0030] The first wavelength laser having a wavelength of 800 nm or more and 1200 nm or less is a laser of a wavelength region generally referred to as an IR laser. In addition, the second wavelength laser having a wavelength of 400 nm or more and 500 nm or less is a laser of a wavelength region referred to as a BLUE laser. When comparing the first wavelength laser and the second wavelength laser, the first wavelength laser has a small spot diameter and a high power density, but a low absorptivity at the processing object 15. On the other hand, the second wavelength laser has a large spot diameter and a low power density, but a high absorptivity at the processing object 15.

[0031] Therefore, when the processing object is scanned by the laser including the first wavelength laser and the second wavelength laser, the area on the scanning path is irradiated by the first wavelength laser after being irradiated by the second wavelength laser having a larger spot diameter. That is, by irradiating the first wavelength laser having a high power density after irradiating the second wavelength laser having a low power density but a high absorption rate, the generation of spatter and pores can be improved. In this embodiment, the processing object 15 is melted by using the laser including the first wavelength laser and the second wavelength laser, and a welding method as described later is adopted to further reduce the generation of pores.

[0032] Figure 2 This is a diagram showing an example of a processing object 15 to be laser welded. Figure 2 2 is a diagram showing a portion of a stator coil 21 provided in a stator core 20 of a motor. The stator core 20 is formed by stacking electromagnetic steel sheets. A plurality of slots 200 are formed in the stator core 20. A stator coil 21 is arranged in each slot 200. The stator coil 21 is formed by connecting a plurality of segment coils. Figure 2 In the illustrated example, a pair of segment coils 21A and 21B that are connected to each other among the plurality of segment coils constituting the stator coil 21 is illustrated.

[0033] Segment coil 21A is inserted into slot 200a, and segment coil 21B is inserted into slot 200b. End 211a of segment coil 21A is arranged in parallel to be adjacent to end 211b of segment coil 21B. End 211a and end 211b are joined to each other by laser welding. Laser is irradiated on end surfaces of end 211a and end 211b.

[0034] The stator coil 21 generally uses oxygen-free copper with a low oxygen content. When red copper is used instead of oxygen-free copper in order to reduce costs, there is a problem of forming many pores in the welded portion, as described in Patent Document 1. Red copper has a higher oxygen content than oxygen-free copper. For example, the oxygen content in oxygen-free copper is less than 10 ppm, but red copper contains about 300 to 500 ppm of oxygen. When red copper is melted, the oxygen contained in it combines with hydrogen to generate water vapor, which is considered to be the cause of the pores. In this embodiment, laser welding is performed using the method described below to suppress the generation of pores.

[0035] Figure 3 10 is a flowchart illustrating the control of laser welding by the control device 13. In step S101, the control device 13 sets the irradiation condition of the laser irradiated to the processing object 15 to the first irradiation condition. Under the first irradiation condition in the embodiment, the first wavelength laser of the laser generating device 10 and the second wavelength laser of the laser generating device 11 are irradiated simultaneously. In addition, as described later, the output power of the second wavelength laser is set to an output power that maintains the melting amount M of the combined melting area S3 at a specified melting amount Mth. On the other hand, the output power of the first wavelength laser is set to an output power that can melt the processing object 15 (coil conductor) when the first wavelength laser and the second wavelength laser with the above-mentioned output power are irradiated. For example, it is set to an output power that can melt the coil conductor only with the first wavelength laser. Hereinafter, the laser of the first irradiation condition is referred to as the first laser LL1.

[0036] In step S102, Figure 4 In the first scanning mode shown, the first laser light LL1 is irradiated onto the end surfaces of the end portions 211 a and 211 b of the segment coils 21A and 21B. Figure 4 Schematic diagram showing the first scanning method, showing a diagram (top view) when the end surfaces of the end portions 211a and 211b are viewed from above. Arrows R1 and R2 show the scanning trajectory of the first laser beam LL1.

[0037] In the first scanning mode, first, as shown by the scanning trajectories R1 and R2, the spot of the first laser LL1 is reciprocated on the end surface of one end 211a. As a result, the conductor at the end 211a is melted to form a molten area S1. Next, as shown by the scanning trajectories R1 and R2, the spot of the first laser LL1 is reciprocated on the end surface of the other end 211b. As a result, the conductor at the end 211b is melted to form another molten area S2 on the end surface of the end 211b.

[0038] It should be noted that, as a method of alternately scanning the end portions 211a and 211b, the end portions 211a and 211b may be alternately scanned back and forth once in the manner of 211a → 211b → 211a → 211b ..., or may be alternately scanned back and forth multiple times in the manner of 211a → 211a → 211b → 211b → 211a → 211a → 211b .... In addition, a combination of a single reciprocating scan and a multiple reciprocating scan may be performed.

[0039] Figure 5 This is a diagram of the end portions 211a and 211b formed with the molten regions S1 and S2, as viewed from the side of the conductor. By reciprocatingly scanning the end surface of the end portion 211a with the first laser LL1, a portion of the end portion 211a melts to form the molten region S1. Next, by reciprocatingly scanning the end surface of the end portion 211b with the first laser LL1, a portion of the end portion 211b melts to form the molten region S2. Each time the laser irradiation to each end portion 211a and 211b is repeated, the amount of melting of the molten regions S1 and S2 increases. As the ends 211a and 211b melt, pores BH are generated. It should be noted that in this embodiment, bubbles generated in the molten region and pores generated in the weld are collectively referred to as pores.

[0040] Back to Figure 3 In step S103, the control device 13 determines whether the number of reciprocating scans N1 in the first scanning mode (reciprocating scanning) for each end portion 211a, 211b has reached a predetermined number of times N1th set in advance. Figure 5 The melting amount of each melting region S1, S2 shown increases with the increase of the number of scans N1, and the separated melting regions S1, S2 are merged into one. The melting region S3 shown by the double-dotted line shows the merged melting region, which is hereinafter referred to as the merged melting region S3. The merged melting region S3 is formed across the end surface of the end 211a and the end surface of the end 211b.

[0041] The predetermined number of times N1 in step S103 is set in consideration of the timing when the melting amount of each melting region S1, S2 formed at each end 211a, 211b increases and the melting regions S1, S2 merge to form a merged melting region S3. That is, the predetermined number of times N1th is set to the number of times that the merged melting region S3 is necessarily formed when the predetermined number of reciprocating scans N1th are performed.

[0042] The processing of step S103 is repeatedly performed until the number of scans of each end 211a, 211b reaches the specified number N1th. When it is determined in step S103 that N1 ≥ N1th, the process proceeds to step S104. In step S104, the entire combined molten region S3 is scanned. Figure 6 The first laser LL1 is irradiated in the second scanning mode shown. In the second scanning mode, the first laser LL1 is irradiated to each end 211a, 211b in a circular scanning trajectory as shown by the dotted line R3 in a manner that crosses the boundary of the adjacent end 211a, 211b. With the irradiation of the first laser LL1, the melting amount of the combined melting area S3 increases. Figure 7 This is a diagram of the end portions 211a and 211b where the combined molten region S3 is formed, as viewed from the side of the conductor. As the amount of molten metal M of the combined molten region S3 increases, the amount of pores BH generated also increases.

[0043] exist Figure 3 In step S105, the control device 13 determines whether the number of scans N2 using the second scanning method has reached a predetermined number N2th. The predetermined number N2th in this case is set to the number of times the melting amount M of the combined melting area S3 reaches a predetermined melting amount Mth. The process of step S105 is repeatedly performed until the number of scans N2 reaches the predetermined number N2th. When it is determined in step S105 that N2 ≥ N2th, the process proceeds to step S106.

[0044] In step S106, the control device 13 changes the irradiation condition of the irradiated laser from the first irradiation condition to the second irradiation condition. It should be noted that the second scanning mode is continued with respect to the scanning mode. Under the second irradiation condition in the embodiment, the first wavelength laser of the laser generating device 10 is stopped, and irradiation with only the second wavelength laser of the laser generating device 11 is implemented. It should be noted that the output power of the second wavelength laser is set to be the same as that of the first irradiation condition (an output power that maintains the melting amount M of the combined melting area S3 at a specified melting amount Mth). Hereinafter, the laser of the second irradiation condition is referred to as the second laser LL2.

[0045] Here, the output power of the combined melting area S3 is equivalent to Figure 6 The second scanning method shown maintains the output power of not increasing the melting amount M of the combined melting area S3 when irradiating the combined melting area S3 with the second laser LL2. In this case, no new melting occurs at each end 211a, 211b, and the melting amount M of the combined melting area S3 is maintained at a predetermined melting amount Mth.

[0046] In step S107, the control device 13 determines whether the number of scans N3 of the second laser LL2 has reached the specified number of times N3th. Then, the process of step S107 is repeatedly performed until the number of scans N3 reaches the specified number of times N3th. When it is determined in step S107 that N3 ≥ N3th, the process proceeds to step S108. In step S108, the irradiation of the second laser LL2 is stopped, and the laser welding end process is performed, thereby ending a series of laser welding processes.

[0047] Figure 8 This is a graph that qualitatively illustrates the relationship between laser irradiation and the amount of melt and the amount of pores. The graph on the upper side of the graph shows the temporal changes in the amount of melt M and the amount of pores Vb, and the graph on the lower side of the graph shows the temporal changes in the output power W of the laser. The first laser LL1 is irradiated from time t=0 to time t2, and the second laser LL2 is irradiated from time t2 to time t3. The first laser LL1 includes a first wavelength laser IR with an output power W1 and a second wavelength laser Bu with an output power W2. On the other hand, the second laser LL2 includes only the second wavelength laser Bu with an output power W2.

[0048] Line L1 represents the melting amount M, and line L2 represents the estimated pore amount Vb. The slope of line L1 representing the melting amount M changes (increases) at time t1. It can be considered that this is because the melting area extends to substantially the entire end surface of the end portions 211a and 211b, and the laser absorption rate of the processing object increases. When the laser irradiated at time t2 is switched from the first laser LL1 to the second laser LL2, the increase in the melting amount M stops and is maintained at the specified melting amount Mth.

[0049] It can be considered that the amount of pores BH contained in the molten area (pore amount Vb) increases according to the newly melted amount M of the conductor. Therefore, from the start of welding when the melting amount M increases to approximately time t2, the pore amount Vb increases as time passes. On the other hand, when the irradiated laser is switched from the first laser LL1 to the second laser LL2, only the second wavelength laser Bu with an output power of W2 is irradiated in the molten area (combined molten area S3). The second wavelength laser Bu has a large spot diameter and a low power density, so its role is to prevent the conductor from being newly melted and to maintain the melting of the molten area.

[0050] When the conductor does not undergo new melting and the melting amount M is maintained at a certain level, no new pores BH are generated. On the other hand, pores BH that already exist in the melting region (combined melting region S3) are formed. Fig. 9 As shown in FIG. 1 , the pores BH move toward the surface of the combined molten region S3 due to the buoyancy. Then, the pores BH reaching the surface of the combined molten region S3 are discharged from the surface of the combined molten region S3 into the atmosphere. When the melt volume M is maintained at a certain level, the pores BH are discharged into the atmosphere in this way. Figure 8 The pore volume Vb of the combined molten region S3 shown by the line L2 is reduced. The irradiation time of the second laser LL2, that is, the time during which the molten volume M is maintained at a certain value (Mth), is set according to the discharge speed of the pores BH.

[0051] As described above, in this embodiment, the second laser LL2 is irradiated to the molten area to maintain the melting amount M, promote the discharge of the pores BH to the atmosphere, and thus reduce the pores BH in the combined molten area S3. As a result, the number of pores BH (pore volume Vb) remaining in the welded portion of the end portions 211a and 211b can be reduced compared to the past, and the bonding strength of the welded portion can be improved. In addition, as in the technology described in Patent Document 1, since no deoxidizing material is used, it is possible to prevent an increase in processing costs and a decrease in electrical conductivity.

[0052] In the above embodiment, the first laser LL1 includes a first wavelength laser IR having a wavelength of 800 nm to 1200 nm and a second wavelength laser Bu having a wavelength of 400 nm to 500 nm, and the second laser LL2 is a laser consisting only of the second wavelength laser Bu. However, the configuration of the first laser LL1 and the second laser LL2 is not limited thereto. Other examples (variations 1 to 4) are described below. It should be noted that in variations 1 to 3, although the description of the first laser LL1 and the second laser LL2 is omitted, Figure 3 The control flowchart shown in FIG. 1 is a flowchart of control, but the irradiation conditions and the like may be appropriately changed according to the contents of the modified example.

[0053] (Variant 1)

[0054] Fig.10 1 is a diagram illustrating the first laser LL1 and the second laser LL2 in Modification 1. In Modification 1, the second laser LL2 also adopts a structure including the first wavelength laser IR and the second wavelength laser Bu. In addition, the output power of the first wavelength laser IR is set to W1 in the first laser LL1, and the output power of the first wavelength laser IR is set to W11 (<W1) in the second laser LL2. In addition, since the first wavelength laser IR including the output power W11 is set in the second laser LL2, the output power of the second wavelength laser Bu is set to W21 (<W2). By setting in this way, the total output power of the second laser LL2 can be an output power that maintains the melting amount M of the combined melting area S3 at a specified melting amount Mth. In the case where pores are generated at a deeper position in the melting area, insufficient heat is input to the deep part of the melting area using only the second wavelength laser Bu, and the pores solidify before being discharged. Therefore, by reducing the output power of the first wavelength laser IR to a level (output power W11) at which no new pores are generated, the pores can be discharged while maintaining the melting state at a deeper position.

[0055] In addition, instead of reducing the output power of the first wavelength laser IR in the second laser LL2, the first wavelength laser IR can be irradiated in a defocused state. By irradiating in a defocused state, the spot diameter of the first wavelength laser IR is enlarged and the power density is reduced. Therefore, energy can be injected while preventing new melting of the conductor caused by the first wavelength laser IR. It should be noted that not only the first wavelength laser IR but also the second wavelength laser Bu can be defocused at the same time.

[0056] In the second laser LL2, the output power of the first wavelength laser IR can be reduced and the second wavelength laser Bu included in the second laser LL2 can be set to a defocused state. In addition, the output power of the second wavelength laser Bu included in the second laser LL2 can be set lower than the output power of the second wavelength laser Bu included in the first laser LL1.

[0057] (Variant 2)

[0058] Fig.11 1 is a diagram for explaining the first laser LL1 and the second laser LL2 in Modification 2. In Modification 2, in Modification 1 ( Fig.10 ) in the first laser LL1, the output power of the first wavelength laser IR included therein is reduced by a predetermined amount ΔW from output power W1 to W12 (W1>W12>W11) at time t1. The other structures are the same as those in the above-mentioned modification example 1.

[0059] It is known that the absorptivity of laser light increases as the temperature of copper, which is the object of processing, increases, and the absorptivity increases in a step-like manner when copper changes from a solid state to a molten state. Time t1 is a timing set in conjunction with the increase in the absorptivity of laser light, and in conjunction with this timing, the output power of the first wavelength laser light IR contained in the first laser light LL1 is reduced from W1 to W12. When the absorptivity of laser light increases, the melting caused by the first laser light LL1 increases dramatically. Therefore, in Modification 2, in order to suppress the rapid increase in pores caused by such a rapid increase in melting, the output power of the first laser light LL1 is reduced by a predetermined amount ΔW.

[0060] exist Fig.11 In the embodiment, the output power of the first laser LL1 is reduced by a predetermined amount ΔW in one stage. Fig.12 As shown in FIG. 1 , ΔW / 2 can be reduced in two stages. Of course, there can be more than three stages. Furthermore, as Fig.13 As shown, the output power of the first laser LL1 can be continuously and smoothly reduced by a predetermined amount ΔW. As a result, the output power of the first laser LL1 can be made to more appropriately follow the change in the absorption rate, and the generation of pores can be more effectively suppressed.

[0061] When the output power of the first laser LL1 is Fig.11 , Fig.12In such a phased reduction, Figure 4 The irradiation (reciprocating scanning) of the reciprocating movement of the end 211a shown in the figure and the irradiation (reciprocating scanning) of the reciprocating movement of the end 211b are combined into one cycle of irradiation as a unit, and the output power is reduced every n units (n=1, 2, 3...). In this way, by reducing the output power in units of cycles, the melting state of each end can be made equal.

[0062] It should be noted that Figure 8 The first laser LL1 and the second laser LL2 are also relative to Fig.10 of Figures 11 to 13 Similarly to the case of FIG. 1 , the output power of the first wavelength laser IR included in the first laser LL1 may be reduced stepwise or continuously from W1 to W12 at time t1 .

[0063] (Variant 3)

[0064] Fig.14 1 is a diagram for explaining the first laser LL1 and the second laser LL2 in Modification 3. In Modification 3, the first laser LL1 and the second laser LL2 are each composed of only the first wavelength laser IR. The output power of the first wavelength laser IR in the first laser LL1 is set to W13. The output power W13 can also be Figure 8 The output power W1 shown is the same as that of the first wavelength laser IR, or can be set slightly higher. The output power of the first wavelength laser IR in the second laser LL2 is set to W14. The first wavelength laser IR is irradiated in a defocused state to increase the spot diameter and reduce the power density of the first wavelength laser IR.

[0065] Thus, in the third modification, the second laser LL2 is composed of only the first wavelength laser IR, but the output power is reduced and the power density is reduced by defocusing, thereby maintaining the melting amount M of the combined melting area S3 at a constant level. It should be noted that the first wavelength laser IR of the second laser LL2 can also be a structure in which the output power is reduced only, or it can be irradiated only in a defocused state. Fig.14 In the variant 3 of Fig.10 of Figures 11 to 13 Similarly to the case of FIG. 1 , at time t1 , the output power of the first wavelength laser IR included in the first laser LL1 may be reduced stepwise or continuously from W1 to W12 .

[0066] (Variant 4)

[0067] Fig.15 This is a flowchart for explaining Modification Example 4. Fig.15 The flowchart is in Figure 3The flowchart of FIG. 1 deletes step S103, step S104, and step S105 and adds step S113. The processing of steps other than step S113 is the same as Figure 3 The processing of the steps with the same reference numerals is the same. The following mainly describes the steps after step S113.

[0068] In step S102 , as described above, irradiation of the end surfaces of the end portions 211 a and 211 b of the segment coils 21A and 21B with the first laser beam LL1 in the first scanning mode is started. Figure 5 The melting amount of each melting region S1 and S2 shown increases as the number of scans N1 increases. Furthermore, the separated melting regions S1 and S2 are merged into one, forming a merged melting region S3 spanning the end surface of the end portion 211a and the end surface of the end portion 211b.

[0069] In step S113, the control device 13 determines whether the number of scans N1 of the first scanning method has reached a predetermined number of times Nth1. The predetermined number of times Nth1 is set to the number of times the melting amount M of the combined melting area S3 reaches a predetermined melting amount Mth. The process of step S113 is repeatedly performed until the number of scans N1 reaches the predetermined number of times Nth1. When it is determined in step S113 that N1 ≥ Nth1, the process proceeds to step S106.

[0070] In step S106, the control device 13 changes the irradiation condition of the irradiated laser from the first irradiation condition (first laser LL1) to the second irradiation condition (second laser LL2). It should be noted that the first scanning mode is continued with respect to the scanning mode. In step S107, it is determined whether the number of scans N3 of the second laser LL2 has reached the prescribed number of scans N3th. When it is determined that N3 ≥ N3th, the process proceeds to step S108. In step S108, the irradiation of the second laser LL2 is stopped and the laser welding end process is performed, and a series of laser welding processes are ended.

[0071] exist Figure 3 In the laser scanning control shown, when the molten area becomes the combined molten area S3, the reciprocating scanning (first scanning mode) is switched to the circular orbit scanning (second scanning mode). On the other hand, in Modification 4, the scanning mode does not need to be switched, so the scanning control is simpler.

[0072] It should be noted that in the above embodiment, the laser welding is described by taking the case of joining the stator coils of the motor as an example, but the laser welding method of the present invention is not limited to the joining of stator coils, and can be applied to the welding of various processing objects. Fig.16As shown, it can also be applied to the case where the plates 30a and 30b are overlapped and welded. First, the first laser LL1 is irradiated to form a molten area S4 across the plate 30a and the plate 30b. Next, the second laser LL2 is irradiated to the molten area S4 to maintain a constant amount of melting. While the amount of melting is maintained, the pores BH in the molten area S4 are discharged into the atmosphere, which can reduce the pores in the weld.

[0073] According to the above-described embodiment and modified example of the present invention, the following effects are achieved.

[0074] (1) Figure 5 , 7 As shown in , 11 to 14, etc., the laser welding method includes: a first step, in which the first laser LL1 is irradiated to the ends 211a, 211b as the processing object to melt the ends 211a, 211b; and a second step, in which the second laser LL2 with irradiation conditions different from those of the first laser LL1 is irradiated to the molten area (combined molten area S3) melted by the first step to maintain the melting amount of the combined molten area S3.

[0075] The laser is irradiated by the following first laser configuration (A) or second laser configuration (B). In the first laser configuration (A), for example, Figures 11 to 13 As shown in FIG. 1 , after a predetermined time has passed since the irradiation of the first laser LL1, the output power of the first laser LL1 is reduced by a predetermined amount, and the output power of the second laser LL2 is set to be smaller than the output power of the first laser LL1. Fig.14 As shown, the first laser LL1 includes a first wavelength laser IR having a first wavelength of 800 nm to 1200 nm and an output power W13, and the second laser LL2 includes a first wavelength laser IR having a first wavelength and an output power smaller than the output power W13 and / or in a defocused state.

[0076] Thus, in the second step, since the melting amount of the combined melting area S3 is maintained, the generation of new pores accompanying the melting can be stopped. In addition, the pores in the melting area move toward the surface of the melting area due to buoyancy and are discharged from the surface of the melting area to the atmosphere. As a result, the pores in the melting area are reduced, so that the pores remaining in the weld are reduced, and the bonding strength of the weld can be improved. In addition, since no deoxidizing material is used, the cost increase and the decrease in electrical conductivity can be suppressed.

[0077] (2) In addition, Figures 4 to 7As shown in FIG. 1 , the processing object is the conductor ends (ends 211a, 211b) of a plurality of conductors (segment coils 21A, 21B) arranged in parallel, until the molten regions S1, S2 formed at the respective ends 211a, 211b merge to form a combined molten region S3, as shown in FIG. Figure 4 As shown in FIG. 1 , the laser is scanned toward the ends 211a and 211b separately, and after the merged molten area S3 is formed, as shown in FIG. Figure 6 The laser is shown being scanned across each end 211a, 211b.

[0078] Conductors such as the stator coil of the motor are coated with enamel etc. Therefore, when laser is irradiated to the end faces of the ends 211a and 211b for welding, when the laser is scanned across the ends 211a and 211b, the coating layer may be damaged by laser irradiation and may have an adverse effect.

[0079] As described above, until the molten regions S1 and S2 formed on each end face merge, Figure 4 As shown in FIG. 1 , the laser is irradiated to the end portions 211a and 211b separately, thereby preventing the laser from irradiating the cover layer. On the other hand, when the combined molten region S3 is formed, since the cover layer of the boundary region of the end portions 211a and 211b is covered by the combined molten region S3, even if Figure 6 As shown in FIG. 1 , the laser is scanned across each end 211a, 211b, and the cover layer may also be irradiated with the laser. As a result, damage to the cover layer caused by the laser can be prevented. It should be noted that in order to make scanning control simpler, as shown in FIG. Fig.15 As shown in FIG. 1 and FIG. 2 , after the combined molten region S3 is formed, the ends 211a and 211b may be irradiated with laser light separately. That is, in both the first step and the second step, the ends of the conductor may be scanned with laser light separately.

[0080] (3) In addition, Figure 8 As shown in FIG. 1 , the first laser LL1 in the first laser configuration (A) includes a laser having a first wavelength and an output power W1 and a laser having a second wavelength of 400 nm or more and 500 nm or less and an output power W2 smaller than the output power W1. The second laser LL2 in the first laser configuration (A) includes a laser having a second wavelength and an output power W2. By setting the output power in this way, the number of pores BH (pore volume Vb) remaining in the welded portion at each end can be reduced compared to the past, and the bonding strength of the welded portion can be improved.

[0081] (4) In addition, Fig.14 As shown in the first laser configuration (A), the output power of the first laser LL1 is continuously and gradually reduced as the irradiation time passes, so that the output power of the first laser LL1 is reduced by the predetermined amount. Fig.11 , 12 As shown in the figure, in the first laser configuration (A), the output power of the first laser LL1 is reduced in stages, and the output power of the first laser LL1 is reduced by the specified amount. When the processing object is the conductor end (end 211a, 211b), when the first laser LL1 is irradiated to each conductor end (end 211a, 211b), the output power is reduced in units of a specified number (n units (n=1, 2, 3...)) of reciprocating scans (irradiation (reciprocating scan) of the reciprocating movement of the end 211a and irradiation (reciprocating scan) of the reciprocating movement of the end 211b are combined into one cycle of irradiation), and the output power of the first laser LL1 is reduced in stages. In more detail, each time the reciprocating scan of the first laser LL1 including the reciprocating movement of the end 211a and the reciprocating movement of the end 211b is performed a specified number of times, the output power of the first laser is reduced. By reducing the output power in units of cycles in this way, the melting state of each end can be made uniform.

[0082] The various embodiments and modifications described above are merely examples, and the present invention is not limited to those contents unless the characteristics of the invention are impaired. Other forms that can be conceived within the scope of the technical concept of the present invention are also included in the scope of the present invention.

[0083] By adopting the present invention, it is possible to prevent the increase of processing cost and the decrease of electrical conductivity while reducing pores.

[0084] The present invention has been described above in conjunction with preferred embodiments, but it should be understood by those skilled in the art that various modifications and changes can be made without departing from the scope of the disclosure of the claims set forth below.

Claims

1. A laser welding method, which is a laser welding method for welding by irradiating a laser to a processing object, characterized in that: The process includes executing the following steps by a computer: a first step of irradiating the processing object with a first laser to melt the processing object; and a second step of irradiating the molten region melted in the first step with a second laser beam different from the first laser beam to maintain the amount of the molten region; The laser is irradiated by the first laser configuration or the second laser configuration, wherein In the first laser configuration, after a predetermined time has passed since the irradiation of the first laser, the output power of the first laser is reduced by a predetermined amount, and the output power of the second laser is set to be smaller than the output power of the first laser. In the second laser configuration, the first laser includes laser light having a first wavelength of 800 nm to 1200 nm and a first output, and the second laser includes laser light having the first wavelength and having a power lower than the first output and / or being in a defocused state.

2. The laser welding method according to claim 1, characterized in that: In the first laser configuration, the output power of the first laser is continuously and gradually reduced as the irradiation time elapses, and the output power of the first laser is reduced by the predetermined amount.

3. The laser welding method according to claim 1, characterized in that: The processing object is the conductor ends of a plurality of conductors arranged in parallel, In the first laser configuration, reducing the output power of the first laser in stages so as to reduce the output power of the first laser by the predetermined amount, When irradiating each of the plurality of conductor ends with the first laser beam, the output power of the first laser beam is reduced in units of a predetermined number of reciprocating scans, so that the output power of the first laser beam is reduced in stages.

4. The laser welding method according to claim 3, characterized in that: The plurality of conductor ends include a first conductor end and a second conductor end, In the first laser configuration, whenever the reciprocating scan including the reciprocating irradiation of the first conductor end and the reciprocating irradiation of the second conductor end is performed the predetermined number of times, the output power of the first laser is reduced in stages.

5. The laser welding method according to claim 1, characterized in that: The first laser in the first laser configuration includes a laser having the first wavelength and a second output power and a laser having a second wavelength of 400 nm to 500 nm and a third output power lower than the second output power, The second laser light in the first laser configuration includes laser light having the second wavelength and the third output power.

6. The laser welding method according to any one of claims 1 to 5, characterized in that: The processing object is the conductor end portions of a plurality of conductors arranged in parallel, In the first step and the second step, the laser beam is scanned toward the conductor end alone.

7. The laser welding method according to any one of claims 1 to 5, characterized in that: The processing object is the conductor end portions of a plurality of conductors arranged in parallel, until the molten regions formed at the ends of the conductors merge to form a combined molten region, scanning the laser light toward the ends of the conductors individually, After the merged molten region is formed, the laser is scanned across each of the conductor ends.

8. A laser welding system, characterized in that: have: A first laser generating device (10) which generates a first laser; A second laser generating device (11) which generates a second laser different from the first laser; an optical device (12) for irradiating the first laser light and the second laser light to a processing object; and a control device (13) for controlling the operation of the first laser generating device (10), the second laser generating device (11) and the optical device (12), The control device (13) controls the operation of the first laser generating device, the second laser generating device and the optical device so that the first laser is irradiated onto the processing object to melt the processing object, and then the second laser is irradiated onto the melted molten area to maintain the melting amount of the molten area.