Preparation method of magnesium cobaltate and magnesium cobaltate
Through the high-energy ball milling method and the use of water as a process control agent, the problems of high-temperature calcination and high energy consumption in the preparation of magnesium cobalt oxide are solved, and the low-cost large-scale preparation of magnesium cobalt ate and the production of high-capacitance materials are achieved.
Patent Information
- Application Number
- CN202411236121.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-10-25
AI Technical Summary
The existing preparation method of magnesium cobaltate has problems such as complicated production process, high temperature calcination, high energy consumption, high cost and small output, which limits its industrial application.
Adopt high-energy ball milling method and use water as process control agent to inhibit powder solidification, improve solid-phase reaction efficiency, and convert magnesium oxide into magnesium hydroxide with lower bond energy, making it easier for magnesium atoms and oxygen atoms to enter cobalt trioxide The crystal lattice enables large-scale preparation of magnesium cobaltate at room temperature.
The preparation of magnesium cobaltate with a simple, efficient and low-cost process is realized, which is suitable for industrial production and improves the mass specific capacitance of the magnesium cobaltate electrode material.
Smart Images

Figure CN118833871A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material preparation, and in particular to a preparation method of magnesium cobaltate and the magnesium cobaltate. Background Art
[0002] In order to solve the energy crisis, electrochemical energy storage and energy conversion devices have become hot spots in the field of research and application. Supercapacitors are a common electrochemical energy storage material, and common supercapacitors are divided into double-layer capacitors and pseudocapacitor materials. Magnesium cobaltate is an emerging pseudocapacitor material. The existing methods for preparing magnesium cobaltate mainly include the following: combustion method, electrochemical deposition method, molten salt method, electrospinning method, microwave-assisted liquid phase method, precipitation method, hydrothermal method and solvent thermal method. However, these methods either have complex production processes, require high-temperature calcination, have low yields, or produce waste and have high production costs, thereby limiting the industrial application of these methods. For example, a Chinese patent with publication number CN107335437A discloses a magnesium cobaltate catalyst, a preparation method and an application thereof, wherein the method first prepares an intermediate product, magnesium cobalt hydroxide, and then calcines the intermediate at 500°C to obtain magnesium cobaltate. The method has complex steps, uses high-temperature calcination, and has high energy consumption, resulting in a high overall cost, which is not conducive to its large-scale application. The Chinese patent with publication number CN113845149A discloses a nano magnesium cobaltate and its preparation method and application, wherein the method obtains a precursor by hydrothermal reaction, and the precursor is calcined to obtain the final product magnesium cobaltate. However, the method uses ammonium fluoride with relatively large toxicity as a structural synthesis agent, and the single batch output of magnesium cobaltate is only 0.2g. Therefore, the low-cost, large-scale and high-quality preparation of magnesium cobaltate is a problem to be solved.
[0003] During mechanical ball milling, the long-term impact and collision between the powder and the ball milling beads and the tank wall causes the powder to repeatedly undergo cold welding, fracture, and re-welding. This series of processes promotes the mutual diffusion or reaction of atoms among the powder particles in the solid phase. Therefore, mechanical ball milling makes the solid-phase reaction that was originally difficult to carry out possible. et al. (The Journal of Physical Chemistry C 2007, 111 (13), 5026-5033) successfully prepared nickel ferrite by ball milling α-iron oxide and nickel oxide powders at a molar ratio of 1:1 at 600 rpm for 8 hours. However, the method of preparing magnesium cobalt oxide by mechanical ball milling has not been reported so far. Summary of the invention
[0004] In order to overcome the defects of the above-mentioned prior art, the present invention provides a method for preparing magnesium cobaltate at low cost with simple process and easy scale-up. The present invention adopts high-energy ball milling as a solid-phase reaction, and innovatively adopts water as a process control agent, which greatly inhibits the occurrence of powder solidification during ball milling and improves the efficiency of solid-phase reaction; and the added deionized water can convert magnesium oxide into magnesium hydroxide with lower bond energy, making it easier for magnesium atoms and oxygen atoms to enter the cobalt trioxide lattice. Thereby, large-scale preparation of magnesium cobaltate material at room temperature is successfully achieved. This method is simple in process, efficient, low in cost, easy to scale up, and can be used for the industrial preparation of magnesium cobaltate electrode materials.
[0005] The objective of the present invention is achieved through the following technical solutions:
[0006] <First aspect>
[0007] The present invention provides a method for preparing magnesium cobaltate, comprising the following steps:
[0008] (1) mixing magnesium oxide and cobalt trioxide to obtain a reaction mixture, wherein the theoretical molar ratio of magnesium oxide to cobalt trioxide is 1:1;
[0009] (2) adding deionized water to the reaction mixture;
[0010] (3) ball milling, separating the reaction product, and drying to obtain magnesium cobaltate.
[0011] As an embodiment of the present invention, in step (2), the mass ratio of the volume of the deionized water to the reaction mixture is 1 to 3 mL / g.
[0012] As an embodiment of the present invention, in step (3), the ball-to-material ratio during ball milling is 10:1 to 8:1.
[0013] As an embodiment of the present invention, in step (3), the rotation speed of the ball mill is 300-350 rpm.
[0014] As an embodiment of the present invention, in step (3), the ball milling time is 64 to 96 hours.
[0015] As an embodiment of the present invention, in step (3), the ball milling is carried out in a ball mill kettle.
[0016] As an embodiment of the present invention, in step (3), the ball milling beads used in the ball milling are one or more of stainless steel balls, zirconium oxide, aluminum oxide, and agate.
[0017] As an embodiment of the present invention, in step (3), the separation method is at least one of sieve separation, centrifugal separation or filtration separation.
[0018] As an embodiment of the present invention, in step (3), the drying is oven drying or vacuum drying.
[0019] Furthermore, the drying is carried out in an oven, and the reaction product is dried in the oven to a constant weight to obtain magnesium cobaltate.
[0020] Furthermore, the drying temperature is 100-110°C.
[0021] Preferably, the drying temperature is 105°C.
[0022] As some specific embodiments of the present invention, the preparation method specifically comprises the following steps:
[0023] (1) putting magnesium oxide and cobalt trioxide into a ball mill in a molar ratio of 1:1 as reactants, and putting ball mill beads into the ball mill;
[0024] (2) Add deionized water to the ball mill, cover it with a lid, press it tightly, and fix the ball mill on the ball milling equipment;
[0025] (3) Start the ball milling equipment to fully mill the reactants. After the operation is completed, turn off the power supply, open the kettle cover, and take out the reaction product and ball milling beads;
[0026] (4) separating the ball milling beads and the reaction product, and drying the latter to obtain magnesium cobaltate.
[0027] As some specific embodiments of the present invention, the present invention relates to a method for preparing magnesium cobaltate, the method specifically comprising: placing a certain amount of magnesium oxide and cobalt trioxide into a ball mill of a certain volume according to a stoichiometric ratio, then adding a certain amount of deionized water and a certain amount of ball milling beads to the ball mill, then covering the lid and pressing it, and then placing the ball mill containing the material into a ball mill; starting the ball mill, running it at a certain ball milling speed, and stopping the machine after the running time reaches a preset value, taking out the reaction product and ball milling beads from the ball mill, and separating them through a sieve, and then placing the reaction product in an oven to dry to constant weight to obtain magnesium cobaltate. The electrode material prepared using it as a raw material has a mass specific capacitance of up to 665.8F / g. The method is simple in process, efficient, low in cost, easy to scale up, and can be used for industrial preparation.
[0028] <Second Aspect>
[0029] The present invention provides magnesium cobaltate, which is prepared by any of the methods described above.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1) The preparation method of the present invention is simple, efficient, low-cost, easy to scale up, and can be used for industrial preparation;
[0032] 2) The preparation method of the present invention adopts a mechanochemical reaction with an atomic utilization rate of 100%, and no toxic or harmful reagents are used in the process, so the preparation method is green and environmentally friendly;
[0033] 3) The method of the present invention has high reaction efficiency and can completely convert cobalt trioxide and magnesium oxide into magnesium cobaltate through solid phase reaction;
[0034] 4) The magnesium cobalt oxide electrode material prepared by the present invention has a mass specific capacitance of up to 665.8 F / g. BRIEF DESCRIPTION OF THE DRAWINGS
[0035] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:
[0036] Figure 1 This is a schematic diagram of the process for preparing magnesium cobaltate according to the present invention;
[0037] Figure 2 This is an X-ray diffraction characterization diagram of the magnesium cobalt oxide prepared in Example 1;
[0038] Figure 3 This is an X-ray diffraction characterization diagram of the magnesium cobalt oxide prepared in Example 2;
[0039] Figure 4 This is an X-ray diffraction characterization diagram of the magnesium cobalt oxide prepared in Example 3;
[0040] Figure 5 This is a charge and discharge test diagram of the magnesium cobalt oxide electrode prepared in Example 3;
[0041] Figure 6 This is an X-ray diffraction characterization diagram of the magnesium cobalt oxide prepared in Comparative Example 1;
[0042] Figure 7 This is an X-ray diffraction characterization diagram of the magnesium cobalt oxide prepared in Comparative Example 2;
[0043] Figure 8 This is an X-ray diffraction characterization diagram of the magnesium cobalt oxide prepared in Comparative Example 3;
[0044] Fig. 9 This is an X-ray diffraction characterization diagram of the magnesium cobalt oxide prepared in Comparative Example 4;
[0045] Fig.10 This is an X-ray diffraction characterization diagram of the magnesium cobalt oxide prepared in Comparative Example 5;
[0046] Fig.11 This is an X-ray diffraction characterization diagram of the magnesium cobalt oxide prepared in Comparative Example 6;
[0047] Fig.12 This is an X-ray diffraction characterization diagram of the magnesium cobalt oxide prepared in Comparative Example 7;
[0048] Fig.13 This is the charge and discharge test diagram of the magnesium cobalt oxide electrode prepared in Comparative Example 7. DETAILED DESCRIPTION
[0049] The present invention is described in detail below in conjunction with specific embodiments. The following embodiments will help those skilled in the art to further understand the present invention, but are not intended to limit the present invention in any form. It should be noted that, for those of ordinary skill in the art, several variations and improvements may be made without departing from the concept of the present invention. These all belong to the protection scope of the present invention.
[0050] In the present invention, unless otherwise specified, all raw materials are commercially available products well known to those skilled in the art.
[0051] In order to further illustrate the present invention, a method for preparing magnesium cobaltate provided by the present invention is described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0052] Example 1
[0053] like Figure 1 As shown, the preparation method of magnesium cobaltate in the present application includes the following steps: (1) adding a certain amount of cobalt trioxide, magnesium oxide, deionized water, and ball milling beads into a ball milling kettle, and pressing the kettle cover; (2) placing the ball milling kettle on a ball mill, and after running for a period of time, a mixture of the product and the ball milling beads is obtained; (3) separating and drying through a sieve to obtain the final magnesium cobaltate powder. The details are as follows:
[0054] Take 80.45g of cobalt trioxide, 19.55g of magnesium oxide and 200mL of deionized water and add them into a stainless steel ball mill with a volume of 1000mL, add 1000g of zirconium oxide ball milling beads, and press the lid of the kettle; adjust the ball mill speed to 350rpm, after ball milling for 48h, take out the reaction product and ball milling beads; after separation through a sieve, put the reaction product into an oven and dry it to constant weight at 105℃; this is the prepared magnesium cobaltate, a total of 98.1g. Characterize with an X-ray diffractometer, the analysis instrument is Rigaku Mini Flex 600, and the scanning rate in the analysis conditions is 10° / min. Figure 2 As shown, the obtained sample is magnesium cobaltate.
[0055] Example 2
[0056] Take 80.45g of cobalt trioxide, 19.55g of magnesium oxide and 200mL of deionized water and add them into a stainless steel ball mill with a volume of 1000mL, add 1000g of zirconium oxide ball milling beads, and press the lid of the kettle; adjust the ball mill speed to 300rpm, after ball milling for 96h, take out the reaction product and ball milling beads; after separation through a sieve, put the reaction product into an oven and dry it at 105℃ to constant weight; this is the prepared magnesium cobaltate, a total of 99.2g. Characterize with an X-ray diffractometer, the analysis instrument is Rigaku Mini Flex 600, and the scanning rate in the analysis conditions is 10° / min. Figure 3 As shown, the obtained sample is magnesium cobaltate.
[0057] Example 3
[0058] Take 80.45g of cobalt trioxide, 19.55g of magnesium oxide and 200mL of deionized water and add them into a stainless steel ball mill with a volume of 1000mL, add 1000g of zirconium oxide ball milling beads, and press the lid of the kettle; adjust the ball mill speed to 350rpm, after ball milling for 80h, take out the reaction product and ball milling beads; after separation through a sieve, put the reaction product into an oven and dry it at 105℃ to constant weight; this is the prepared magnesium cobaltate, a total of 98.9g. Characterize with an X-ray diffractometer, the analysis instrument is Rigaku Mini Flex 600, and the scanning rate in the analysis conditions is 10° / min. Figure 4 As shown, the obtained sample is magnesium cobaltate.
[0059] The magnesium cobalt oxide prepared in Example 3 was subjected to an electrochemical performance test, specifically as follows: The electrochemical performance test was carried out using a three-electrode system, and the prepared magnesium cobalt oxide, conductive carbon black, and polyvinylidene fluoride were mixed in N-methylpyrrolidone at a mass ratio of 80:15:5, coated on the cleaned nickel foam, and dried as a working electrode. A mercury oxide electrode was used as a reference electrode, and a platinum wire was used as a counter electrode; the electrolyte solution was 3 mol / L potassium hydroxide. The charge and discharge voltage range was 0.1 to 0.5 V, and the current density was 0.1 A / g. The results are as follows Figure 5 As shown. The electrode has high electrochemical performance, and the mass specific capacitance is as high as 665.8F / g. This shows that the magnesium cobalt oxide prepared by this method can be used as an electrode material in supercapacitors.
[0060] Comparative Example 1
[0061] Magnesium cobaltate was prepared in the same manner as in Example 1, except that deionized water was not added during the mechanical ball milling process. Specifically,
[0062] Take 80.45g of cobalt trioxide and 19.55g of magnesium oxide and add them to a stainless steel ball mill with a volume of 1000mL, add 1000g of zirconium oxide ball milling beads, and press the lid of the kettle; adjust the ball mill speed to 350rpm. After 48h of ball milling, the sample has serious agglomeration phenomenon. Take out the reaction product and ball milling beads; after separation through a sieve, a powder sample of 98.4g is obtained. Characterize with an X-ray diffractometer, the analysis instrument is Rigaku Mini Flex 600, and the scanning rate is 10° / min in the analysis conditions. Figure 6 As shown, the obtained sample has obvious magnesium oxide impurity phase in addition to the magnesium cobaltate phase.
[0063] The magnesium cobaltate obtained in this comparative example has an obvious impurity phase, indicating that in the process of preparing magnesium cobaltate by mechanical ball milling, magnesium oxide and cobalt trioxide are directly ball milled, and magnesium cobaltate without impurities cannot be obtained. This is because the cold welding during the ball milling process causes serious agglomeration of the sample, which greatly reduces the rate of solid-phase reaction during the ball milling process. Deionized water, as a process inhibitor, can significantly reduce the occurrence of cold welding and agglomeration during the ball milling process. Therefore, the synthesis of single crystalline magnesium cobaltate in Example 1 is because the addition of deionized water greatly increases the reaction rate, so that cobalt trioxide and magnesium oxide are completely converted into magnesium cobaltate.
[0064] Comparative Example 2
[0065] Magnesium cobaltate was prepared in the same manner as in Example 1, the only difference from Example 1 being that the time of the mechanical ball milling process was reduced, specifically:
[0066] Take 80.45g of cobalt trioxide, 19.55g of magnesium oxide and 200mL of deionized water and add them into a stainless steel ball mill with a volume of 1000mL, add 1000g of zirconium oxide ball milling beads, and press the lid of the kettle; adjust the ball mill speed to 350rpm, after ball milling for 16h, take out the reaction product and ball milling beads; after separation through a sieve, put the reaction product into an oven and dry it at 105℃ to constant weight; obtain a powder sample, a total of 99.3g. Characterize with an X-ray diffractometer, the analysis instrument is Rigaku Mini Flex 600, and the scanning rate in the analysis conditions is 10° / min. Figure 7 As shown, the obtained sample has obvious magnesium hydroxide and magnesium oxide impurity phases in addition to the magnesium cobaltate phase.
[0067] It can be seen that if the mechanical ball milling time is too short, the reactants cannot be completely converted into the reaction product magnesium cobaltate.
[0068] Further, from Figure 7It can be seen that when the reaction time is insufficient, the product sample obtained in this comparative example has magnesium hydroxide and magnesium oxide impurity phases, indicating that in the reaction process of the present invention, magnesium oxide and water generate magnesium hydroxide, which reduces the bond energy of the magnesium precursor, making it easier for magnesium atoms and oxygen atoms to enter the cobalt trioxide lattice, thereby generating magnesium cobaltate.
[0069] Comparative Example 3
[0070] Magnesium cobaltate was prepared in the manner of Example 3, the only difference from Example 1 being that the deionized water added during the mechanical ball milling process was replaced with ethanol, specifically:
[0071] Take 80.45g of cobalt trioxide, 19.55g of magnesium oxide and 200mL of ethanol and add them to a stainless steel ball mill with a volume of 1000mL, add 1000g of zirconium oxide ball milling beads, and press the lid of the kettle; adjust the ball mill speed to 350rpm, after ball milling for 48h, take out the reaction product and ball milling beads; after separation through a sieve, put the reaction product into an oven and dry it at 105℃ to constant weight; obtain a powder sample, a total of 99.3g. Characterize with an X-ray diffractometer, the analysis instrument is Rigaku Mini Flex 600, and the scanning rate in the analysis conditions is 10° / min. Figure 8 As shown, the obtained sample has obvious magnesium oxide impurity phase in addition to the magnesium cobaltate phase.
[0072] The sample obtained in this comparative example has an obvious magnesium oxide impurity phase, and there is no magnesium hydroxide phase. This shows that when ethanol is used as a process inhibitor, the conversion of magnesium oxide to magnesium hydroxide cannot be achieved like water. In addition to reducing the cold welding and agglomeration phenomena during the ball milling process, adding deionized water can also convert magnesium oxide into magnesium hydroxide, thereby reducing the bond energy of the magnesium precursor, making it easier for magnesium atoms and oxygen atoms to enter the cobalt trioxide lattice.
[0073] Comparative Example 4
[0074] Magnesium cobaltate was prepared in the manner of Example 1, the only difference from Example 1 being that the ratio of the volume of deionized water to the mass of the reaction mixture during the mechanical ball milling process was increased, specifically:
[0075] Take 80.45g of cobalt trioxide, 19.55g of magnesium oxide and 400mL of deionized water and add them into a stainless steel ball mill with a volume of 1000mL, add 1000g of zirconium oxide ball milling beads, and press the lid of the kettle; adjust the ball mill speed to 350rpm, after ball milling for 48h, take out the reaction product and ball milling beads; after separation through a sieve, put the reaction product into an oven and dry it at 105℃ to constant weight; obtain a powder sample, a total of 98.8g. Characterize with an X-ray diffractometer, the analysis instrument is Rigaku Mini Flex 600, and the scanning rate in the analysis conditions is 10° / min. Fig. 9 As shown, the obtained sample has an obvious magnesium hydroxide impurity phase in addition to the magnesium cobaltate phase.
[0076] The magnesium cobalt oxide obtained in this comparative example has obvious impurity phase, indicating that when the amount of deionized water is high, excessive deionized water inhibits the collision between the powder and the ball milling beads during the ball milling process, resulting in lower energy transferred to the powder during the ball milling process and lower reaction efficiency.
[0077] Comparative Example 5
[0078] Magnesium cobaltate was prepared in the manner of Example 1, the only difference from Example 1 being that the ratio of the volume of deionized water to the mass of the reaction mixture during the mechanical ball milling process was reduced, specifically:
[0079] Take 80.45g of cobalt trioxide, 19.55g of magnesium oxide and 50mL of deionized water and add them to a stainless steel ball mill with a volume of 1000mL, add 1000g of zirconium oxide ball milling beads, and press the lid of the kettle; adjust the ball mill speed to 350rpm, after ball milling for 48h, take out the reaction product and ball milling beads; after separation through a sieve, put the reaction product into an oven and dry it at 105℃ to constant weight; obtain a powder sample, a total of 99.3g. Characterize with an X-ray diffractometer, the analysis instrument is Rigaku Mini Flex 600, and the scanning rate in the analysis conditions is 10° / min. Fig.10 As shown, the obtained sample has obvious magnesium oxide and magnesium hydroxide impurity phases in addition to the magnesium cobaltate phase.
[0080] The magnesium cobalt oxide obtained in this comparative example has obvious impurity phases, indicating that when less deionized water is added, the effect of preparing magnesium cobalt oxide by mechanical ball milling is not good. This is because when the amount of deionized water added is too small, its inhibitory effect on cold welding and solidification is limited, and it is not enough to convert magnesium oxide into magnesium hydroxide, and cannot effectively promote the reaction in the process.
[0081] Comparative Example 6
[0082] Magnesium cobaltate was prepared in the manner of Example 1, the only difference from Example 1 being that the rotation speed during the mechanical ball milling process was reduced, specifically:
[0083] Take 80.45g of cobalt trioxide, 19.55g of magnesium oxide and 200mL of deionized water and add them into a stainless steel ball mill with a volume of 1000mL, add 1000g of zirconium oxide ball milling beads, and press the lid of the kettle; adjust the ball mill speed to 150rpm, after ball milling for 48h, take out the reaction product and ball milling beads; after separation through a sieve, put the reaction product into an oven and dry it at 105℃ to constant weight; obtain a powder sample, a total of 99.1g. Characterize with an X-ray diffractometer, the analysis instrument is Rigaku Mini Flex 600, and the scanning rate in the analysis conditions is 10° / min. Fig.11 As shown, the obtained sample has obvious magnesium oxide and magnesium hydroxide impurity phases in addition to the magnesium cobaltate phase.
[0084] The magnesium cobalt oxide obtained in this comparative example has obvious impurity phase, indicating that when the rotation speed is low, the mechanical ball milling is not effective in preparing magnesium cobalt oxide. This is because when the rotation speed is low, the energy transferred to the powder through the collision of the balls during the ball milling process is low, and the reaction efficiency is low.
[0085] Comparative Example 7
[0086] Comparative Example 7 uses a common precipitation method to prepare a magnesium cobaltate sample. Specifically, 1.164g of cobalt nitrate hexahydrate and 0.512g of magnesium nitrate hexahydrate are dissolved in deionized water and stirred for 30 minutes to obtain a purple-red solution. Subsequently, a 3 mol / L sodium hydroxide solution is added to the solution until the pH value is 14, and a purple-red precipitate is obtained. The purple-red precipitate is filtered and sintered at 350°C for 2h to obtain 0.361g of black powder. The X-ray diffractometer is used for characterization. The analysis instrument is Rigaku Mini Flex 600, and the scanning rate in the analysis conditions is 10° / min. Fig.12 As shown, the obtained sample is magnesium cobaltate. Compared with Example 3, the method for preparing magnesium cobaltate has a lower yield and requires high-temperature sintering of the obtained intermediate, which is not conducive to industrial production.
[0087] The electrochemical performance of magnesium cobalt oxide prepared in comparative example 7 was tested as follows: The electrochemical performance was tested using a three-electrode system. The prepared magnesium cobalt oxide, conductive carbon black, and polyvinylidene fluoride were mixed in N-methylpyrrolidone at a mass ratio of 80:15:5, coated on the cleaned nickel foam, and dried as a working electrode. A mercury oxide electrode was used as a reference electrode, and a platinum wire was used as a counter electrode; the electrolyte solution was 3 mol / L potassium hydroxide. The charge and discharge voltage range was 0.1 to 0.5 V, and the current density was 0.1 A / g. The results are as follows: Fig.13As shown. The mass specific capacitance of the electrode is 389.0F / g. Compared with Example 3, the mass specific capacitance of the electrode is lower, which is because the magnesium cobaltate particles are broken during the ball milling process, and the smaller particles have a higher specific surface area. In the precipitation method, the magnesium cobaltate particles finally obtained are larger and have a smaller specific surface area, so the mass specific capacitance is also smaller.
[0088] This comparative example shows that, compared with the traditional method for preparing magnesium cobaltate, the method of the present invention can significantly increase the single batch output of magnesium cobaltate material, and the prepared magnesium cobaltate material has good electrochemical properties. Therefore, the present method is conducive to the large-scale application of magnesium cobaltate material in electrochemical energy storage.
[0089] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.
Claims
1. A method for preparing magnesium cobaltate, characterized in that: The steps include: (1) mixing magnesium oxide and cobalt trioxide to obtain a reaction mixture, wherein the theoretical molar ratio of magnesium oxide to cobalt trioxide is 1:1; (2) adding deionized water to the reaction mixture; (3) ball milling, separating the reaction product, and drying to obtain magnesium cobaltate.
2. The preparation method according to claim 1, characterized in that: In step (2), the mass ratio of the volume of the deionized water to the reaction mixture is 1 to 3 mL / g.
3. The preparation method according to claim 1, characterized in that: In step (3), the ball-to-material ratio during ball milling is 10:1 to 8:
1.
4. The preparation method according to claim 1, characterized in that: In step (3), the rotation speed of the ball mill is 300-350 rpm.
5. The preparation method according to claim 1, characterized in that: In step (3), the ball milling time is 64 to 96 hours.
6. The preparation method according to claim 1, characterized in that: In step (3), the ball milling is carried out in a ball milling kettle.
7. The preparation method according to claim 1, characterized in that: In step (3), the ball milling beads used in the ball milling are one or more of stainless steel balls, zirconium oxide, aluminum oxide, and agate.
8. The preparation method according to claim 1, characterized in that: In step (3), the separation method is at least one of sieve separation, centrifugal separation or filtration separation.
9. The preparation method according to claim 1, characterized in that: In step (3), the drying is oven drying or vacuum drying.
10. A magnesium cobaltate, characterized in that: The method is prepared by the method according to any one of claims 1 to 9.