Silicon-based composite material containing organic flexible coating layer and preparation method thereof
By forming an organic flexible cladding layer on the silicon-based material, the problem that the inorganic carbon cladding layer cannot alleviate the expansion of the silicon-based material is solved, and the conductivity and specific capacity are improved, achieving good electrochemical performance of the negative electrode of the lithium battery.
Patent Information
- Application Number
- CN202411312424.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-20
AI Technical Summary
In the prior art, the inorganic carbon cladding layer cannot fully and effectively alleviate the volume expansion problem of silicon-based materials during charging and discharging, and the modified cladding layer containing organic polymers has an adverse effect on electrical conductivity and specific capacity.
Aniline silane is used to modify the surface of the silicon-based material containing an inorganic carbon coating layer, and form an organic flexible coating layer through in-situ polymerization to form a silicon-based composite material with a three-layer core-shell structure, including silicon-based materials and inorganic Carbon cladding and organic flexible cladding.
It effectively alleviates the volume expansion and particle rupture of the electrode material during charging and discharging, improves the circulation performance and conductivity, and achieves good comprehensive electrochemical performance.
Smart Images

Figure CN118841556B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of lithium batteries, and in particular relates to a silicon-based composite material containing an organic flexible coating layer and a preparation method thereof. Background Art
[0002] Lithium-ion batteries are one of the most attractive energy storage devices at present because of their high energy density, long life, and environmental friendliness. Traditional graphite negative electrodes have high stability, but their capacity has reached its upper limit and cannot meet the market demand for high-energy batteries; silicon-based negative electrode materials have attracted much attention due to their high specific capacity. However, in the actual process of lithium extraction / insertion of silicon-based materials, silicon particles undergo large volume changes or even break and pulverize, and the stability of the electrode structure is destroyed, which ultimately leads to rapid capacity decay of the electrode material and a short cycle life; at the same time, silicon-based materials have poor conductivity and poor reaction kinetics, which in turn affects their electrical performance. Carbon coating on the surface of silicon-based materials is currently a commonly used solution to the above problems, such as solid-phase carbon coating and chemical vapor deposition. The carbon coating layer commonly used in the prior art is an inorganic carbon layer. Since the inorganic carbon layer is rigid and brittle, it will have a certain degree of rupture during the charge and discharge process, and the pulverization of the electrode material is difficult to effectively alleviate, and the effect of improving the long-term cycle performance of the material is not good.
[0003] Therefore, it is urgent to develop a silicon-based material with a flexible coating layer, which can provide a buffer for the expansion of the silicon-based material to effectively alleviate the impact of the volume change of the electrode during the charge and discharge process. The applicant disclosed in the previous patent CN113270586B the preparation and application of an in-situ polymerization-coated modified silicon-based negative electrode material, wherein the surface of the silicon-based material is coated with a composite coating layer of an inorganic substance and a polymer, and the silicon-based negative electrode material is subjected to the action of a deep eutectic solvent, so that the monomer of the polymer is in-situ polymerized on the surface of the silicon-based material to obtain a composite coating layer in which the inorganic substance is uniformly distributed in the polymer; the composite coating layer is constructed on the surface of the material by in-situ polymerization of a polymer monomer doped with an inorganic substance, wherein the inorganic substance is a lithium salt, and the polymer is poly-1,3-dioxolane (PDOL), polyvinylene carbonate (PVC), polyvinyl carbonate (PEC), or polyacrylonitrile (PAN). Compared with the inorganic carbon coating layer, the negative electrode material containing the coating layer forms an organic-inorganic composite artificial solid electrolyte interface (SEI) in situ during the initial lithiation / delithiation process, maintaining the structural integrity during the insertion / extraction of lithium, and the addition of lithium-rich inorganic substances reduces the irreversible consumption of lithium ions, improving the first coulombic efficiency and cycle stability of the negative electrode material. Although the inorganic lithium salt in the composite coating layer of the invention is conducive to improving the cycle performance, its excessive content will affect the conductivity of the silicon-based negative electrode material; and the excessive content of organic polymer in the composite coating layer will also have an adverse effect on the conductivity and specific capacity.
[0004] In summary, in the prior art, the inorganic carbon coating layer cannot completely and effectively alleviate the problem of silicon-based material expansion, and the modified coating layer containing organic polymers will have an adverse effect on the conductivity and specific capacity. Summary of the invention
[0005] In order to solve the problem that the inorganic carbon coating layer in the above-mentioned prior art cannot completely and effectively alleviate the expansion of the silicon-based material, and the modified coating layer containing organic polymers has an adverse effect on the conductivity and specific capacity, the present invention forms a silicon-based composite material containing an organic flexible coating layer by surface modification of the silicon-based material containing the inorganic carbon coating layer with aniline silane and in-situ polymerization. The formed flexible coating layer can effectively alleviate the volume expansion and particle rupture of the electrode material during the charge and discharge process, so that it has good cycle performance; at the same time, the organic polymer in the coating layer also contributes to the conductivity and specific capacity; that is, the silicon-based composite material of the present invention has good comprehensive electrochemical performance when used in the negative electrode of the lithium battery.
[0006] To achieve the above object, the present invention adopts the following scheme:
[0007] A silicon-based composite material containing an organic flexible coating layer is a three-layer core-shell structure, which comprises a silicon-based material, an inorganic carbon coating layer and an organic flexible coating layer from the inside to the outside. The organic flexible coating layer is an organic silicon-polyaniline layer formed by in-situ polymerization of aniline, an oxidant and a cross-linking agent octaepoxysilsesquioxane after surface modification of the silicon-based material containing the inorganic carbon coating layer with an aniline silane to form a precursor. The precursor, aniline, oxidant and cross-linking agent octaepoxysilsesquioxane have a mass ratio of 100:(10-25):(5-12):(0.2-0.5). The mass ratio of the silicon-based material containing the inorganic carbon coating layer to the aniline silane is 100:(8-15).
[0008] Furthermore, the mass ratio of the precursor, aniline, oxidant, and crosslinking agent octaepoxysilsesquioxane is 100: (15-20): (7-12): (0.2-0.5).
[0009] Furthermore, the anilinosilane is at least one of anilinomethyltrimethoxysilane, anilinomethyltriethoxysilane, 3-(phenylamino)propyltrimethoxysilane, and 3-(phenylamino)propyltriethoxysilane.
[0010] Furthermore, the oxidant is at least one of ammonium persulfate and benzoyl peroxide.
[0011] Furthermore, the surface modification is achieved by hydrolyzing anilinosilane at one end of its molecular chain to generate silanol groups, which are then subjected to a condensation reaction with hydroxyl groups on the surface of the silicon-based material containing the inorganic carbon coating layer.
[0012] Furthermore, the in-situ polymerization is achieved by subjecting the precursor to chemical oxidation polymerization with aniline under the action of an oxidant, and then subjecting the precursor to a crosslinking reaction with a crosslinking agent, octaepoxysilsesquioxane.
[0013] Furthermore, the silicon-based material is at least one of silicon, silicon dioxide, modified silicon dioxide, silicon oxide, silicon-carbon composite material, magnesium silicate, lithium silicate, sodium silicate, potassium silicate, and calcium silicate, and the particle size of the silicon-based material is 3-8 μm.
[0014] Furthermore, the thickness of the inorganic carbon coating layer is 1 to 20 nm, preferably 5 to 15 nm.
[0015] In a second aspect, the present invention provides a method for preparing the above-mentioned silicon-based composite material containing an organic flexible coating layer, comprising the following preparation steps:
[0016] (S1) Inorganic carbon coating: coating the silicon-based material with inorganic carbon to obtain a silicon-based material containing an inorganic carbon coating layer;
[0017] (S2) Surface modification: dispersing a silicon-based material containing an inorganic carbon coating layer in an alcohol aqueous solution to obtain a dispersion; dispersing anilinosilane in water and performing a hydrolysis reaction at room temperature to obtain a hydrolysis solution; adding the hydrolysis solution to the dispersion, stirring and reacting at room temperature for 2 to 5 hours to obtain a precursor;
[0018] (S3) In situ polymerization: Precursor, aniline and oxidant are added to an inorganic acid solution, and stirred to react at 2-8°C for 3-8 hours under an inert atmosphere; then, octaepoxysilsesquioxane as a crosslinking agent is added, and the temperature is raised to 60-80°C and the reaction is continued for 2-5 hours to obtain a silicone-polyaniline coated silicon-based composite material, i.e., a silicon-based composite material containing an organic flexible coating layer.
[0019] In step (S1), the method of inorganic carbon coating is well known in the art, such as chemical vapor deposition or solid phase coating; preferably, chemical vapor deposition is used, that is, a gaseous carbon source is chemically vapor deposited on the surface of a silicon-based material to form a carbon coating layer, for example, the gaseous carbon source is selected from at least one of C1-4 alkanes (such as methane, ethane, propane), C2-4 olefins (such as ethylene, propylene, 1-butene), and C2-4 alkynes (such as acetylene, propyne); the process conditions are: reaction at 800°C~1000°C in an inert atmosphere for 2h~5h.
[0020] Furthermore, in step (S2), the ratio of the amount of the silicon-based material containing the inorganic carbon coating layer to the alcohol aqueous solution is 100g: (500-1000) mL, the alcohol content in the alcohol aqueous solution is 30-60wt%, and the alcohol is selected from at least one of methanol and ethanol. The silicon-based material coated with inorganic carbon is hydrophobic, so in step (S2), dispersing the silicon-based material containing the inorganic carbon coating layer in the alcohol aqueous solution has a better dispersion effect and is more conducive to subsequent surface modification.
[0021] Furthermore, in step (S2), the ratio of the anilinosilane to water is (40-50) g:100 mL; and the conditions of the hydrolysis reaction are: stirring the reaction at room temperature for 15-30 min.
[0022] Furthermore, in step (S3), the concentration of the inorganic acid solution is 0.5-1 mol / L, and the inorganic acid is at least one of hydrochloric acid, phosphoric acid, and perchloric acid; and the dosage ratio of the aniline to the inorganic acid solution is 10 g: (300-500) mL.
[0023] Furthermore, in step (S3), the inert atmosphere is at least one of nitrogen, argon or helium.
[0024] In a third aspect, the present invention provides application of the above silicon-based composite material containing an organic flexible coating layer in a lithium-ion battery.
[0025] Compared with the prior art, the present invention has the following beneficial effects:
[0026] (1) The present invention uses an anilinosilane coupling agent to modify the surface of a silicon-based material containing an inorganic carbon coating layer. After hydrolysis, the silanol group at one end of the anilinosilane undergoes a condensation reaction with the hydroxyl group on the surface of the silicon-based material containing the inorganic carbon coating layer, and the anilinosilane is introduced into the surface of the silicon-based material containing the inorganic carbon coating layer by chemical bonds; and the active aniline group at the other end of the anilinosilane can undergo chemical oxidation polymerization with the aniline monomer under the action of an oxidant, so that polyaniline is in situ grafted onto the silicon-based material containing the inorganic carbon coating layer. The surface of the silicon-based material is formed by a uniform and stable organic silicon-polyaniline layer coated on the surface of the silicon-based material; at the same time, the cross-linking agent octa-epoxy silsesquioxane can cross-link with the polyaniline in the organic silicon-polyaniline, thereby increasing the density of the organic flexible coating layer; and because both anilinosilane and the cross-linking agent octa-epoxy silsesquioxane contain organic silicon, a layer of organic silicon mesh is formed in the structure, and the Si-O bond has high bond energy and good stability; finally, a silicon-based composite material containing a dense and stable organic flexible coating layer is obtained. The organic flexible coating layer can effectively alleviate the volume expansion and particle breakage of the electrode material during the charge and discharge process.
[0027] (2) The organic flexible coating layer of the present invention contains organosilicon groups and conductive polyaniline groups, that is, the organic flexible coating layer also plays a role in specific capacity and conductivity, so it can be used without high-temperature carbonization; and because it does not undergo high-temperature carbonization, the size of the silicon grains is controllable and is in an amorphous state, thus avoiding the problem of silicon grain growth caused by high-temperature carbonization.
[0028] (3) When the silicon-based composite material containing an organic flexible coating layer prepared by the present invention is used as the negative electrode of a lithium battery, it exhibits good electrochemical performance. Its first reversible specific capacity reaches 1800 mAh / g, its first coulombic efficiency reaches more than 93%, and its 100-cycle capacity retention rate reaches more than 93%; and in the process of preparing the negative electrode slurry, the gas production of the slurry is low. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a transmission electron microscope image of the silicon-based composite material containing an organic flexible coating layer obtained in Example 1;
[0030] Figure 2 The first cycle charge and discharge curve of a lithium battery assembled with the silicon-based composite material containing an organic flexible coating layer prepared in Example 1 at a rate of 0.1C;
[0031] Figure 3 This is a graph of cycle number-Coulomb efficiency of a lithium battery assembled from a silicon-based composite material containing an organic flexible coating layer prepared in Example 1. DETAILED DESCRIPTION
[0032] In order to better explain the present invention, the following description will be given in detail with reference to the embodiments of the present invention, and the main contents of the present invention will be further clarified in conjunction with specific examples. However, the contents of the present invention are not limited to the following examples.
[0033] Unless otherwise specified, the “parts” described in the embodiments of the present invention are all parts by mass, and the reagents used are all commercially available reagents in the art.
[0034] The particle size of the silicon-carbon composite material is 6.5 μm. It is a porous carbon particle of chemical vapor deposited silicon with a silicon content of 49.7%. It is selected from Jiangxi Yijin New Energy Technology Co., Ltd.
[0035] Example 1
[0036] (S1) Inorganic carbon coating: The silicon-carbon composite material is placed in a coating furnace, heated to 900° C. under a nitrogen atmosphere, and then acetylene gas is introduced at a flow rate of 3 L / min for carbon coating for 2.5 h to obtain a silicon-based material containing an inorganic carbon coating layer;
[0037] (S2) Surface modification: 200 g of a silicon-based material containing an inorganic carbon coating layer was dispersed in 1400 mL of an ethanol aqueous solution (ethanol content was 50 wt%) to obtain a dispersion; 16 g of anilinosilane was dispersed in 40 mL of water and subjected to a hydrolysis reaction at room temperature for 30 min to obtain a hydrolysis solution; the hydrolysis solution was added to the dispersion and stirred at room temperature for 2 h; thereafter, the precursor was obtained by suction filtration, washing with pure water, and drying in an oven at 60° C. for 12 h;
[0038] (S3) In situ polymerization: 100 g of precursor, 10 g of aniline, and 5 g of oxidant ammonium persulfate were added to 500 mL of 0.5 mol / L hydrochloric acid solution, and stirred at 5±1°C for 3 h under nitrogen atmosphere; then 0.2 g of cross-linking agent octaepoxysilsesquioxane was added, and the temperature was raised to 70°C and the reaction was continued for 3 h to obtain a mixed turbid liquid; the mixed turbid liquid was then centrifuged, washed, and dried at 60°C for 24 h to obtain an organosilicon-polyaniline-coated silicon-based composite material, that is, a silicon-based composite material containing an organic flexible coating layer.
[0039] Figure 1 It is a transmission electron microscope image of the silicon-based composite material containing an organic flexible coating layer obtained in Example 1. It can be seen from the figure that the silicon-based composite material containing an organic flexible coating layer obtained in Example 1 has an obvious layered structure, which includes a silicon-based material, an inorganic carbon coating layer and an organic flexible coating layer from the inside to the outside.
[0040] Example 2
[0041] The rest is the same as Example 1, except that in step (S2), 3-(phenylamino)propyltrimethoxysilane is used instead of anilinemethyltrimethoxysilane.
[0042] Example 3
[0043] The rest is the same as Example 1, except that, in step (S2), the material dosage and reaction conditions are as follows: 200 g of a silicon-based material containing an inorganic carbon coating layer is dispersed in 1400 mL of an ethanol aqueous solution (ethanol content is 50 wt%) to obtain a dispersion; 30 g of anilinemethyltrimethoxysilane is dispersed in 100 mL of water and subjected to a hydrolysis reaction at room temperature for 30 min to obtain a hydrolysis solution; the hydrolysis solution is added to the dispersion and stirred at room temperature for 5 h; thereafter, the precursor is obtained by suction filtration, washing with pure water, and drying in an oven at 60° C. for 12 h.
[0044] Example 4
[0045] The rest is the same as Example 1, except that in step (S3), the amount of materials used is: 100g of precursor, 15g of aniline, 7g of oxidant ammonium persulfate, and 0.3g of cross-linking agent octaepoxysilsesquioxane.
[0046] Example 5
[0047] The rest is the same as Example 1, except that in step (S3), the amount of materials used is: 100g of precursor, 20g of aniline, 9g of oxidant ammonium persulfate, and 0.4g of cross-linking agent octaepoxysilsesquioxane.
[0048] Example 6
[0049] The rest is the same as Example 1, except that in step (S3), the amount of materials used is: 100g of precursor, 25g of aniline, 12g of oxidant ammonium persulfate, and 0.5g of cross-linking agent octaepoxysilsesquioxane.
[0050] Comparative Example 1
[0051] The rest is the same as Example 1, except that step (S2) is omitted, that is, the surface modification with aniline silane is not performed.
[0052] Comparative Example 2
[0053] The rest is the same as Example 1, except that step (S3) is omitted, that is, no in-situ polymerization is performed.
[0054] Comparative Example 3
[0055] The rest is the same as Example 1, except that in step (S3), the cross-linking agent octaepoxysilsesquioxane is not used.
[0056] Testing and analysis
[0057] The silicon-based composite materials containing organic flexible coating layers prepared in the examples and comparative examples were subjected to the following electrochemical performance tests:
[0058] Charge and discharge test: The prepared silicon-based composite material containing an organic flexible coating layer, carbon black and polyacrylic acid (PAA) aqueous solution binder were mixed in a mass ratio of 80:10:10 to form a slurry (wherein the concentration of polyacrylic acid aqueous solution was 3.4wt%), and the slurry was evenly coated on the copper foil current collector with a certain thickness, and vacuum dried for 12 hours to form a working electrode; lithium sheet was used as the counter electrode, ceramic diaphragm, Shenzhen Xinzhoubang electrolyte, and button cells were assembled in an argon atmosphere Micairon inert gas glove box. The above assembled battery was charged and discharged on the LAND charge and discharge tester. The test conditions were: the charge and discharge range was 0.005-1.5 V, a three-stage discharge method was used, the discharge current density was 0.1C, 0.02C, 0.01C, and the charging current density was 0.1C.
[0059] Figure 2 This is the first cycle charge and discharge curve of a lithium battery assembled with the silicon-based composite material containing an organic flexible coating layer prepared in Example 1 at a rate of 0.1C.
[0060] Figure 3 This is a graph of cycle number-Coulomb efficiency of a lithium battery assembled from a silicon-based composite material containing an organic flexible coating layer prepared in Example 1.
[0061] The high-temperature gas production test method is as follows: the prepared silicon-based composite material containing an organic flexible coating layer, carbon black and sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber (SBR) composite binder are mixed in a mass ratio of 90:5:5 to form a slurry (wherein the mass ratio of CMC and SBR is 2:3), and an aluminum-plastic bag is used to remove air for packaging. The initial slurry density value is tested using a solid densitometer, and then the density value is tested again after being stored at 45°C for 24 hours. The gas production of the material is calculated according to v=m / ρ. The higher the gas production value, the more serious the material damage and the worse the material stability.
[0062] The above test results are shown in Table 1.
[0063] Table 1 Performance test
[0064] .
[0065] It can be seen from the data in Table 1 that when the silicon-based composite material containing an organic flexible coating layer prepared in the embodiment of the present invention is used as the negative electrode of a lithium battery, its first reversible specific capacity reaches 1800 mAh / g, the first coulombic efficiency reaches more than 93%, and the capacity retention rate after 100 cycles reaches more than 93%; and in the process of preparing the negative electrode slurry, the gas production of the slurry is low, indicating that the organic flexible coating layer of the present invention can effectively alleviate the volume expansion and particle breakage of the electrode material during the charging and discharging process.
[0066] In Comparative Example 1, the silicon-based material containing an inorganic carbon coating layer is not surface-modified with aniline silane, and only aniline is polymerized on its surface. Although the lithium battery prepared therefrom has a high first coulombic efficiency, its reversible specific capacity is low and its cycle performance is poor.
[0067] In Comparative Example 2, the silicon-based material containing an inorganic carbon coating layer was only surface-modified with aniline silane without in-situ polymerization. The lithium battery prepared therefrom not only had poor electrochemical performance but also had a large slurry gas production, indicating that an effective organic flexible coating layer could not be formed.
[0068] In Comparative Example 3, the silicon-based material containing an inorganic carbon coating layer was surface-modified with aniline silane and in-situ polymerized, but no cross-linking agent was added during the polymerization process. In particular, although the first coulombic efficiency and reversible specific capacity of the prepared lithium battery were relatively high, the cycle performance was poor.
Claims
1. A silicon-based composite material containing an organic flexible coating layer, characterized in that: It is a three-layer core-shell structure, which comprises a silicon-based material, an inorganic carbon coating layer and an organic flexible coating layer from the inside to the outside. The organic flexible coating layer is formed by using an aniline silane to modify the surface of the silicon-based material containing the inorganic carbon coating layer to form a precursor, and then in situ polymerizing with aniline, an oxidant, and a cross-linking agent octaepoxy silsesquioxane to form an organic silicon-polyaniline layer. The mass ratio of the precursor, aniline, the oxidant, and the cross-linking agent octaepoxy silsesquioxane is 100: (10-25): (5-12): (0.2-0.5); the mass ratio of the silicon-based material containing the inorganic carbon coating layer to the aniline silane is 100: (8-15). The anilinosilane is at least one of anilinomethyl trimethoxysilane, anilinomethyl triethoxysilane, 3-(phenylamino)propyl trimethoxysilane, and 3-(phenylamino)propyl triethoxysilane; The surface modification is achieved by hydrolyzing anilinosilane at one end of its molecular chain to generate silanol groups, which are then subjected to a condensation reaction with hydroxyl groups on the surface of the silicon-based material containing the inorganic carbon coating layer; The in-situ polymerization is achieved by subjecting the precursor and aniline to chemical oxidation polymerization under the action of an oxidant, and then subjecting the precursor to a crosslinking reaction with a crosslinking agent, octaepoxysilsesquioxane.
2. The silicon-based composite material containing an organic flexible coating layer according to claim 1, characterized in that: The mass ratio of the precursor, aniline, oxidant and cross-linking agent octa-epoxy-octa-epoxy-silsesquioxane is 100: (15-20): (7-12): (0.2-0.5).
3. The silicon-based composite material containing an organic flexible coating layer according to claim 1, characterized in that: The oxidant is at least one of ammonium persulfate and benzoyl peroxide.
4. The silicon-based composite material containing an organic flexible coating layer according to claim 1, characterized in that: The silicon-based material is at least one of silicon, silicon dioxide, modified silicon dioxide, silicon oxide, silicon-carbon composite material, magnesium silicate, lithium silicate, sodium silicate, potassium silicate and calcium silicate, and the particle size of the silicon-based material is 3-8 μm; the thickness of the inorganic carbon coating layer is 1-20 nm.
5. The method for preparing a silicon-based composite material containing an organic flexible coating layer according to any one of claims 1 to 4, characterized in that: The method comprises the following preparation steps: (S1) Inorganic carbon coating: coating the silicon-based material with inorganic carbon to obtain a silicon-based material containing an inorganic carbon coating layer; (S2) Surface modification: dispersing a silicon-based material containing an inorganic carbon coating layer in an alcohol aqueous solution to obtain a dispersion; dispersing anilinosilane in water and performing a hydrolysis reaction at room temperature to obtain a hydrolysis solution; The hydrolysis solution is added to the dispersion, and the reaction is stirred at room temperature for 2 to 5 hours to obtain a precursor; (S3) In situ polymerization: Precursor, aniline and oxidant are added to an inorganic acid solution, and stirred to react at 2-8°C for 3-8 hours under an inert atmosphere; then, octaepoxysilsesquioxane as a crosslinking agent is added, and the temperature is raised to 60-80°C and the reaction is continued for 2-5 hours to obtain a silicone-polyaniline coated silicon-based composite material, i.e., a silicon-based composite material containing an organic flexible coating layer.
6. The preparation method according to claim 5, characterized in that: In step (S2), the ratio of the silicon-based material containing the inorganic carbon coating layer to the alcohol aqueous solution is 100 g: (500-1000) mL, the alcohol content in the alcohol aqueous solution is 30-60 wt %, and the alcohol is selected from at least one of methanol and ethanol; and / or The ratio of the anilinosilane to water is (40-50) g:100 mL; the conditions of the hydrolysis reaction are: stirring the reaction at room temperature for 15-30 min.
7. The preparation method according to claim 5, characterized in that: In step (S3), the concentration of the inorganic acid solution is 0.5-1 mol / L, and the inorganic acid is at least one of hydrochloric acid, phosphoric acid, and perchloric acid; the dosage ratio of the aniline to the inorganic acid solution is 10 g: (300-500) mL; and the inert atmosphere is at least one of nitrogen, argon, or helium.
8. Use of the silicon-based composite material containing an organic flexible coating layer according to any one of claims 1 to 4 in lithium-ion batteries.