Hydrophilic and anticoagulant enhanced bifunctional coating and preparation method thereof
The hyaluronic acid-nitric oxide catalyst-dopamine product of glycosaminoglycan is synthesized and coated through amidation reaction to form a hydrophilic and anticoagulant coating, which solves the coagulation problem of blood-contact materials and achieves long-lasting anticoagulation and The lubrication effect significantly improves the compatibility and safety of blood contact materials.
Patent Information
- Application Number
- CN202410815038.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-24
- Publication Date
- 2024-10-29
AI Technical Summary
Existing blood-contacting materials are prone to plasma protein adsorption and coagulation cascade reactions when in contact with blood, resulting in shortened functional lifespan of materials and increased complications, and existing anticoagulation strategies are inefficient.
The hyaluronic acid-nitric oxide catalyst-dopamine product is synthesized through amidation reaction and mixed with nanoparticle-coated glycosaminoglycan to form a hydrophilic and anticoagulant dual-functional coating. The slow release of glycosaminoglycans, combined with active attack and passive defense strategies, achieves anticoagulant and lubricating effects.
Significantly inhibits surface platelet adhesion and activation, promotes endothelial cell growth and surface endothelialization, improves anticoagulant properties, prolongs the anticoagulant effect of the coating, improves the hydrophilicity and lubricity of the device surface, and reduces damage to surrounding tissues.
Smart Images

Figure CN118846262A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of medical materials, and specifically relates to a hydrophilic and anticoagulant enhanced dual-functional coating and a preparation method thereof. Background Art
[0002] Blood contact materials are a widely used class of biomedical materials, commonly used in implants such as stents and heart valves, catheters for extracorporeal life support systems, and medical devices for blood collection and storage. However, when exposed to blood, plasma protein adsorption will occur rapidly on the surface of the device, triggering a coagulation cascade reaction that regulates thrombosis. The formed blood clots not only damage the functional life of the material and block blood vessels, but also the detached blood clots will move with the blood flow, further causing complications such as pulmonary embolism, renal failure, deep vein thrombosis or stroke. Therefore, improving the compatibility of blood contact materials and inhibiting adverse reactions on the surface of the materials are crucial to maintaining the function of medical devices and ensuring patient safety.
[0003] At present, researchers have proposed many methods to improve the blood compatibility of materials, for example, by adjusting the surface hydrophilicity and hydrophobicity to inhibit the adsorption of surface proteins, platelets and other blood cells to interfere with the coagulation cascade reaction, or using bioactive molecules with anticoagulant function, such as heparin, to improve the anticoagulant properties of materials. However, coatings often have limited long-term effectiveness, and the complexity of the coagulation cascade means that a single anticoagulation strategy is usually not efficient.
[0004] Studies have found that the natural anticoagulant surface - the endothelial cell layer also achieves excellent anticoagulant function by secreting / releasing a variety of signal molecules. Glycosaminoglycans are located on the surface of endothelial cells, among which hyaluronic acid has good hydrophilicity and can inhibit the adhesion of proteins, blood cells, etc., while heparan sulfate, dermatan sulfate, etc. show excellent anticoagulant activity. In addition, nitric oxide (NO) secreted by endothelial cells also has the function of inhibiting platelet adhesion and activation and promoting surface endothelialization. Therefore, simulating the function of endothelial cells to construct an anticoagulant coating is an effective strategy to improve the blood compatibility of materials. Summary of the invention
[0005] In view of the problem that blood-contact catheters without surface modification in the prior art are prone to poor biocompatibility, the present invention provides a hydrophilic and anticoagulant enhanced dual-functional coating and a preparation method thereof. The present invention first synthesizes a dopamine-hyaluronic acid-nitric oxide catalyst product by an amidation reaction using the reaction between the carboxyl group of hyaluronic acid and the amino group of dopamine and the nitric oxide catalyst, and then dissolves the product and mixes it with the glycosaminoglycan coated with nanoparticles to obtain a coating solution. The coating solution coated on the surface of the substrate can form a hydrophilic and anticoagulant dual-functional coating on the surface of the substrate after drying.
[0006] The technical solution of the present invention is:
[0007] The present invention relates to a method for preparing a hydrophilic and anticoagulation enhanced dual-functional coating, comprising the following steps:
[0008] S1. synthesizing a hyaluronic acid-nitric oxide catalyst-dopamine product by an amidation reaction using the reaction between the carboxyl group of hyaluronic acid and the amino groups of dopamine hydrochloride and the nitric oxide catalyst;
[0009] S2, dissolving the hyaluronic acid-nitric oxide catalyst-dopamine product in a phosphate buffer solution, and then adding NaOH to alkalize the solution;
[0010] S3, continue to add PLGA-coated glycosaminoglycan to the solution obtained in step S2, and after dissolution, obtain a coating solution;
[0011] S4. Soaking the substrate in the coating solution, then washing and vacuum drying to obtain a sample with a hydrophilic and anticoagulation enhanced dual-functional coating.
[0012] Preferably, the specific preparation process of the hyaluronic acid-nitric oxide catalyst-dopamine product in step S1 comprises the following steps:
[0013] (1) dissolving sodium hyaluronate and nitric oxide catalyst in ultrapure water, and adjusting the pH of the solution to a weakly acidic pH of 5 to 5.5;
[0014] (2) adding 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide to the solution obtained in step (1), and stirring evenly for 20-30 minutes to activate the carboxyl groups;
[0015] (3) adding dopamine hydrochloride to the solution obtained in step (2), and then stirring for 10-15 hours under light-proof conditions;
[0016] (4) The reaction product obtained in step (3) is transferred into a dialysis bag for dialysis, and then freeze-dried to obtain a hyaluronic acid-nitric oxide catalyst-dopamine product, which is stored for later use.
[0017] Preferably, in step (1), sodium hyaluronate and a nitric oxide catalyst are dissolved in ultrapure water, and the mass fraction of sodium hyaluronate in the resulting solution is 0.5 to 3 wt %, and the mass fraction of the nitric oxide catalyst is 1 to 5 wt %;
[0018] The mass ratio of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, N-hydroxysuccinimide used in step (2), dopamine hydrochloride used in step (3) and sodium hyaluronate in step (1) is 0.3-0.6: 0.2-0.5: 0.2-2: 0.5-3.
[0019] Preferably, the molecular weight cut-off in step (4) is 3000 Da.
[0020] Preferably, in step S1, the nitric oxide catalyst is one or more cystamine hydrochloride compounds containing a diselenide bond, a ditellurium bond or a disulfide bond.
[0021] Preferably, the preparation process of the PLGA-coated glycosaminoglycan used in step S3 is: dissolving polylactic acid-glycolic acid copolymer in dichloromethane solvent, adding glycosaminoglycan to the above solution, ice bathing, ultrasonication for 20-30s, and then mixing with polyvinyl alcohol aqueous solution and ultrasonication, stirring the formed emulsion at room temperature for 12-24h; then centrifugation and washing to remove residual polyvinyl alcohol and unencapsulated plasmids, resuspending in ultrapure water and freeze-drying in a freeze dryer for 24-72h to obtain PLGA-coated glycosaminoglycan, which is stored for later use.
[0022] Preferably, the polylactic acid-glycolic acid copolymer is dissolved in a dichloromethane solvent, and the mass fraction of the polylactic acid-glycolic acid copolymer in the obtained solution is 1-5wt%; the mass fraction of the polyvinyl alcohol in the polyvinyl alcohol aqueous solution is 1-5wt%;
[0023] The mass ratio of polylactic acid-co-glycolic acid to glycosaminoglycan is 1-5:2-15;
[0024] Among them, the glycosaminoglycan is one or more of heparan sulfate (heparin), dermatan sulfate, keratan sulfate, and chondroitin sulfate.
[0025] Preferably, in step S2, the hyaluronic acid-nitric oxide catalyst-dopamine product is dissolved in a phosphate buffer solution, and the concentration of the resulting solution is 2-10 wt %; the mass ratio of NaOH to the hyaluronic acid-nitric oxide catalyst-dopamine product is 0.2-2:2-10;
[0026] In step S3, the mass ratio of PLGA-coated glycosaminoglycan to hyaluronic acid-nitric oxide catalyst-dopamine product is 0.2-8:2-10.
[0027] Preferably, in step S4, the substrate is a metal material or a high molecular polymer material, the metal substrate is stainless steel, magnesium sheet or titanium sheet, and the high molecular polymer substrate is polymethacrylate, polyurethane, polydimethylsiloxane, polyvinyl chloride. The coating of the present invention is simple to prepare, applicable to a variety of substrates, and can exhibit excellent and long-term stable anticoagulant performance.
[0028] Preferably, the substrate is ultrasonically cleaned with acetone, methanol and ethanol for 10-15 minutes respectively before being immersed for use.
[0029] Preferably, the substrate is immersed in the coating solution for 6-12 hours.
[0030] The present invention also relates to a hydrophilic and anticoagulation enhanced dual-functional coating, which is prepared by the above-mentioned preparation method.
[0031] The beneficial effects of the present invention are:
[0032] (1) The present invention fixes the nitric oxide catalyst through chemical action, which can catalyze the production of nitric oxide in the body for a long time. Combined with the anticoagulant effect of glycosaminoglycan and NO, the coating can achieve a better anticoagulant effect. Compared with the untreated surface, it can significantly inhibit the adhesion and activation of surface platelets, inhibit smooth muscle growth, promote endothelial cell growth, and thus promote endothelialization.
[0033] (2) The hydrophilic anticoagulant coating component prepared by the present invention has functions close to those of natural endothelial cells and has low cytotoxicity.
[0034] (3) Physically loaded glycosaminoglycans are encapsulated by nanoparticles and can be slowly released from the coating. Hyaluronic acid and nitric oxide catalysts are fixed by chemical action, which can make the anticoagulant effect of the coating more long-lasting.
[0035] (4) The present invention combines active attack (NO release and glycosaminoglycan release) and passive defense (fixed hyaluronic acid) strategies. The nitric oxide catalyst in the coating can continuously catalyze the release of NO for a long time. On this basis, the glycosaminoglycans in the degradable nanoparticles can produce an anticoagulant enhancement effect similar to that of endothelial cells in the early stage, which lasts until the surface of the device is completely covered by endothelial cells. On the other hand, the hyaluronic acid in the coating can produce a hydrophilic lubricating effect, which is beneficial to increase the lubricity of the device surface and reduce damage to surrounding tissues during device delivery.
[0036] (5) The various components in the coating work synergistically to improve the anticoagulant properties by increasing hydrophilicity, inhibiting protein and blood cell adhesion, releasing bioactive molecules, inhibiting platelet adhesion and activation, and promoting endothelialization. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:
[0038] Figure 1 The structure of a hyaluronic acid-dopamine-nitric oxide catalyst, wherein A is selenium, tellurium or sulfur;
[0039] Figure 2 Schematic diagram of the anticoagulant hydrophilic coating composition;
[0040] Figure 3 The live and dead conditions of endothelial cells on the surface modified by the PU film and the coating of Example 1, where red represents dead cells and green represents live cells;
[0041] Figure 4The platelet adhesion and activation on the surface modified by the coating of PU membrane, PLGA-coated glycosaminoglycan-coated PU membrane, hyaluronic acid-nitric oxide catalyst-dopamine-coated PU membrane and Example 1;
[0042] Figure 5 The adhesion of endothelial cells on the PU membrane and the surface modified by the coating of Example 1;
[0043] Figure 6 The smooth muscle cells adhesion between the PU membrane and the coating modified surface of Example 1. DETAILED DESCRIPTION
[0044] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings. It should be understood that these descriptions are only exemplary and are not intended to limit the scope of the present invention. In addition, in the following description, the description of well-known structures and technologies is omitted to avoid unnecessary confusion of the concept of the present invention.
[0045] Example 1
[0046] (1) Dissolve 1 part by weight of sodium hyaluronate and 3 parts by weight of selenocystamine hydrochloride in ultrapure water, wherein the mass fraction of sodium hyaluronate in the obtained solution is 1 wt %, and the mass fraction of selenocystamine hydrochloride is 3 wt %, and then adjust the pH value of the solution to 5 using 1 wt % hydrochloric acid.
[0047] (2) Slowly add 0.5 parts by mass of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) and 0.3 parts by mass of N-hydroxysuccinimide (NHS) to the above solution and stir evenly for 30 minutes to activate the carboxyl groups.
[0048] (3) Add 0.5 parts by weight of dopamine hydrochloride to the above solution, and then stir for 12 hours in a dark environment.
[0049] (4) The reaction product was transferred into a dialysis bag and dialyzed for three days (molecular weight cut-off 3000Da), and then freeze-dried in a freeze dryer. The obtained light yellow powder product was stored at -80°C for later use.
[0050] (5) 1.5 parts by weight of polylactic acid-co-glycolic acid (PLGA) was dissolved in dichloromethane solvent, and the mass fraction of PLGA in the obtained solution was 1.5 wt%. 8 parts by weight of heparan sulfate was added to the above solution in an ice bath, ultrasonicated for 30 seconds, and then mixed with an equal volume of a 2 wt% polyvinyl alcohol aqueous solution and ultrasonicated for 3 minutes. The formed emulsion was stirred at room temperature for 15 hours. The residual polyvinyl alcohol and unencapsulated plasmids were removed by centrifugation and washing, and the solution was resuspended in ultrapure water and freeze-dried in a freeze dryer for 36 hours and stored at -20°C for use.
[0051] (6) The polyurethane membrane was ultrasonically cleaned with acetone, methanol and ethanol for 10 min respectively.
[0052] (7) The hyaluronic acid-selenocystamine hydrochloride-dopamine product synthesized in step (4) is dissolved in a phosphate buffer solution (pH=5) with a content of 3 wt%, and then NaOH is added to alkalize the solution, wherein the mass ratio of NaOH to the hyaluronic acid-selenocystamine hydrochloride-dopamine product is 0.5:3.
[0053] (8) Adding the PLGA-coated glycosaminoglycan synthesized in step (5) to the solution obtained in step (7), and after dissolution, immersing the cleaned polyurethane membrane in the solution at 25° C. for 12 hours, wherein the mass ratio of the PLGA-coated glycosaminoglycan to the hyaluronic acid-selenocystamine hydrochloride-dopamine product is 1:1.
[0054] (9) The immersed sample was washed with ultrapure water and vacuum dried to obtain a sample coated with a coating.
[0055] Example 2
[0056] (1) 2 parts by weight of sodium hyaluronate and 4 parts by weight of cystamine hydrochloride are dissolved in ultrapure water, wherein the mass fraction of sodium hyaluronate in the obtained solution is 2 wt %, and the mass fraction of selenocystamine hydrochloride is 4 wt %, and then the pH value of the solution is adjusted to 5.5 using 1 wt % hydrochloric acid.
[0057] (2) Slowly add 0.5 parts by mass of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) and 0.3 parts by mass of N-hydroxysuccinimide (NHS) to the above solution and stir evenly for 30 minutes to activate the carboxyl groups.
[0058] (3) Add 1 part by mass of dopamine hydrochloride to the above solution, and then stir for 12 hours in a light-proof condition.
[0059] (4) The reaction product was transferred into a dialysis bag and dialyzed for three days (molecular weight cut-off 3000Da), and then freeze-dried in a freeze dryer. The obtained light yellow powder product was stored at -80°C for later use.
[0060] (5) 3 parts by weight of polylactic acid-co-glycolic acid (PLGA) were dissolved in dichloromethane solvent, and the mass fraction of PLGA in the resulting solution was 3 wt%. 6 parts by weight of heparan sulfate were added to the above solution in an ice bath, ultrasonicated for 30 seconds, and then mixed with an equal volume of a 3 wt % polyvinyl alcohol aqueous solution and ultrasonicated for 5 minutes. The formed emulsion was stirred at room temperature for 12 hours. The residual polyvinyl alcohol and unencapsulated plasmids were removed by centrifugation and washing, and the solution was resuspended in ultrapure water and freeze-dried in a freeze dryer for 36 hours and stored at -20°C for use.
[0061] (6) The polyvinyl chloride membrane was ultrasonically cleaned with acetone, methanol and ethanol for 10 min each.
[0062] (7) dissolving the hyaluronic acid-cystamine hydrochloride-dopamine product synthesized in step (4) in a phosphate buffer solution (pH=5) with a content of 5 wt %, and then adding NaOH to alkalize the solution, wherein the mass ratio of NaOH to the hyaluronic acid-cystamine hydrochloride-dopamine product is 0.8:5.
[0063] (8) Add the PLGA-coated glycosaminoglycan synthesized in step (5) to the solution obtained in the above step (7), and after dissolution, immerse the cleaned polyvinyl chloride in the solution at 25° C. for 6 hours, wherein the mass ratio of the PLGA-coated glycosaminoglycan to the hyaluronic acid-selenocystamine hydrochloride-dopamine product is 1:1.
[0064] (9) The immersed sample was washed with ultrapure water and vacuum dried to obtain a sample coated with a coating.
[0065] Example 3
[0066] (1) 3 parts by weight of sodium hyaluronate and 1 part by weight of selenocystamine hydrochloride are dissolved in ultrapure water, wherein the mass fraction of sodium hyaluronate in the obtained solution is 3 wt %, and the mass fraction of selenocystamine hydrochloride is 1 wt %, and then the pH value of the solution is adjusted to 5 using 1 wt % hydrochloric acid.
[0067] (2) Slowly add 0.4 parts by mass of 1-ethyl-(3-dimethylaminopropyl)carbodiimide (EDC) and 0.3 parts by mass of N-hydroxysuccinimide (NHS) to the above solution and stir evenly for 30 minutes to activate the carboxyl groups.
[0068] (3) Add 1 part by mass of dopamine hydrochloride to the above solution, and then stir for 15 hours in a light-proof condition.
[0069] (4) The reaction product was transferred into a dialysis bag and dialyzed for three days (molecular weight cut-off 3000Da), and then freeze-dried in a freeze dryer. The obtained light yellow powder product was stored at -80°C for later use.
[0070] (5) 2 parts by weight of polylactic acid-co-glycolic acid (PLGA) were dissolved in dichloromethane solvent, and the mass fraction of PLGA in the resulting solution was 2 wt%. 5 parts by weight of chondroitin sulfate were added to the above solution in an ice bath, ultrasonicated for 30 seconds, and then mixed with an equal volume of a 4 wt% polyvinyl alcohol aqueous solution and ultrasonicated for 5 minutes. The formed emulsion was stirred at room temperature for 15 hours. The residual polyvinyl alcohol and unencapsulated plasmids were removed by centrifugation and washing, and the solution was resuspended in ultrapure water and freeze-dried in a freeze dryer for 36 hours and stored at -20°C for use.
[0071] (6) Use acetone, methanol and ethanol to ultrasonically clean the titanium sheet for 10 min each.
[0072] (7) dissolving the hyaluronic acid-selenocystamine hydrochloride-dopamine product synthesized in step (4) in a phosphate buffer solution (pH=5) with a content of 5 wt %, and then adding NaOH to alkalize the solution, wherein the mass ratio of NaOH to the hyaluronic acid-cystamine hydrochloride-dopamine product is 1:5.
[0073] (8) Add the PLGA-coated glycosaminoglycan synthesized in step (5) to the above solution, and after dissolution, immerse the cleaned titanium sheet in the solution at 25° C. for 10 hours, wherein the mass ratio of the PLGA-coated glycosaminoglycan to the hyaluronic acid-selenocystamine hydrochloride-dopamine product is 2:5.
[0074] (9) The immersed sample was washed with ultrapure water and vacuum dried to obtain a sample coated with a coating.
[0075] The samples of the coating prepared by the present invention were tested, taking Example 1 as an example.
[0076] 1. Live or dead status of endothelial cells
[0077] Experimental conditions: Human umbilical vein endothelial cells were cultured at 20,000 cells / cm 2 The density of cells was planted on the sample surface and cultured in a constant temperature incubator for 24 hours according to standard cell culture conditions (5% CO2, 37°C). The fluorescent dyes 5wt% calcein acetoxymethyl ester (green fluorescence, staining live cells) and 3wt% propidium iodide (red fluorescence, staining dead cells) were used for cell death and live staining. Take out the cultured cells, mix the above two fluorescent dyes in equal volumes under light-proof conditions, then add them to the sample surface and stain them at 37°C in the dark for 15-20 minutes. After staining, the waste liquid was aspirated, the sample was placed face down on a slide, and the fluorescent image of the cells on the sample surface was taken under an inverted fluorescence microscope.
[0078] Figure 3 The figures show the live and dead status of endothelial cells on the surfaces modified with the coating of PU membrane and Example 1, where red represents dead cells and green represents live cells. Comparing the surface of the sample of Example 1 with the surface of the PU membrane, the number of live endothelial cells on the surface is more and the number of dead cells is less, indicating that the coating is friendly to endothelial cells, and the coating components have no obvious toxicity to endothelial cells and are conducive to the growth of endothelial cells.
[0079] 2. Platelet adhesion and activation
[0080] Experimental conditions: Fresh animal venous blood was collected using sodium citrate anticoagulant tubes, centrifuged twice at 800-1000r / min at 22°C, each time for 5-10min, and the supernatant was collected to obtain platelet-rich plasma (PRP) for later use. The samples were cleaned and disinfected with ethanol and phosphate buffered saline (PBS) in a clean bench, and placed in a 96-well plate after drying. PRP was added to the surface of the sample and incubated in a 37°C constant temperature incubator for 1h. After incubation, the blood cells that did not adhere to the surface were washed away with PBS, and the platelets on the surface of the sample were fixed with a 4wt% paraformaldehyde solution at room temperature for 40-60min, and the residual paraformaldehyde solution was washed with PBS, and then the samples were dehydrated step by step with 50-100wt% ethanol solutions of step concentrations. The dried samples were treated with gold spraying, and the images of platelet adhesion and activation on the surface of the samples were observed and photographed using a scanning electron microscope.
[0081] Figure 4 The platelet adhesion and activation conditions of the PU membrane, the PLGA-coated glycosaminoglycan-coated PU membrane, the hyaluronic acid-nitric oxide catalyst-dopamine-coated PU membrane and the coating-modified surface of Example 1 are shown.
[0082] The preparation process of the PLGA-coated glycosaminoglycan coated PU film is as follows: the PLGA-coated glycosaminoglycan synthesized in step (5) of Example 1 is dissolved in a phosphate buffer solution (pH = 5) with a content of 3wt%. After dissolution, the cleaned polyurethane film is immersed in the solution at 25°C for 12 hours, the immersed sample is washed with ultrapure water, and vacuum dried to obtain a coated sample.
[0083] The preparation process of the hyaluronic acid-nitric oxide catalyst-dopamine coated PU film is as follows: the hyaluronic acid-selenocystamine hydrochloride-dopamine product synthesized in step (4) of Example 1 is dissolved in a phosphate buffer solution (pH=5) with a content of 3wt%, and then NaOH is added to alkalize the solution, and then the cleaned polyurethane film is immersed in the solution at 25°C for 12h, wherein the mass ratio of NaOH to the hyaluronic acid-selenocystamine hydrochloride-dopamine product is 0.5:3; the immersed sample is washed with ultrapure water, and after vacuum drying, a sample coated with a coating is obtained.
[0084] Among the four samples tested, the surface of the sample in Example 1 had the least number of platelets, and the surface platelets were mostly spherical, indicating that the platelets were in an unactivated state. The experiment showed that the surface treated with the coating had the effect of inhibiting platelet adhesion and activation, and the inhibitory effect was better than that of the surface treated with only hyaluronic acid-nitric oxide catalyst-dopamine or the surface treated with only PLGA-coated glycosaminoglycan.
[0085] 3. Endothelial cell adhesion
[0086] Experimental conditions: Human umbilical vein endothelial cells were cultured at 20,000 cells / cm 2 The density of cells was planted on the sample surface and cultured in a constant temperature incubator for 24 hours according to the standard cell culture conditions (5% CO2, 37°C). After the culture, the cultured cells were taken out, the dead cells on the sample surface were washed with phosphate buffer solution (PBS), and the cells were fixed with 4wt% paraformaldehyde for 10-15min, and the sample was washed with PBS three times, each time for 5min. Then 0.1wt% Triton X-100 was added to the sample surface, and 5min later, it was washed with PBS three times, each time for 5min. Then, a 3wt% bovine serum albumin solution was added to the sample surface for 40-60min, and then 5wt% phalloidin-fluorescein isothiocyanate solution was used for light staining for 30-60min, and the sample was washed and soaked with PBS three times, each time for 5min. Under light-proof conditions, the cell nucleus was stained with 0.5wt% 4',6-diamidino-2-phenylindole solution for 5min, and the sample was washed and soaked with PBS 3 times, each time for 5-10min. The PBS on the surface of the sample was drained and placed face down on a glass slide. The cells on the surface of the sample were observed using an inverted fluorescence microscope and the fluorescence images of the cells were taken.
[0087] Figure 5 The endothelial cell adhesion on the PU membrane and the coating-modified surface of Example 1. Compared with the PU membrane surface, the surface of the sample in Example 1 has more endothelial cells and better cell spreading, indicating that the coating has the effect of promoting endothelial cell adhesion and proliferation, which is beneficial to the growth of endothelial cells and thus realizes surface endothelialization.
[0088] 4. Smooth muscle cell adhesion
[0089] Experimental conditions: Human umbilical vein smooth muscle cells were cultured at 20,000 cells / cm 2The density of cells was planted on the sample surface and cultured in a constant temperature incubator for 24 hours according to the standard cell culture conditions (5% CO2, 37°C). After the culture, the cultured cells were taken out, the dead cells on the sample surface were washed with phosphate buffer solution (PBS), and the cells were fixed with 4wt% paraformaldehyde for 10-15min, and the sample was washed with PBS three times, each time for 5min. Then 0.1wt% Triton X-100 was added to the sample surface, and 5min later, it was washed with PBS three times, each time for 5min. Then, a 3wt% bovine serum albumin solution was added to the sample surface for 40-60min, and then 5wt% phalloidin-fluorescein isothiocyanate solution was used for light staining for 30-60min, and the sample was washed with PBS three times, each time for 5min. Under light-proof conditions, the cell nucleus was stained with 0.5wt% 4',6-diamidino-2-phenylindole solution for 5min, and the sample was washed and soaked with PBS 3 times, each time for 5-10min. The PBS on the surface of the sample was drained and placed face down on a glass slide. The cells on the surface of the sample were observed using an inverted fluorescence microscope and the fluorescence images of the cells were taken.
[0090] Figure 6 The smooth muscle cell adhesion between the PU membrane and the coating-modified surface of Example 1. The surface of the sample of Example 1 has fewer smooth muscle cells than the surface of the PU membrane, indicating that the coating treatment has the effect of inhibiting the adhesion and proliferation of smooth muscle cells.
[0091] It should be understood that the above specific embodiments of the present invention are only used to illustrate or explain the principles of the present invention, and do not constitute a limitation of the present invention. Therefore, any modifications, equivalent substitutions, improvements, etc. made without departing from the spirit and scope of the present invention should be included in the protection scope of the present invention. In addition, the appended claims of the present invention are intended to cover all changes and modifications that fall within the scope and boundaries of the appended claims, or the equivalent forms of such scope and boundaries.
Claims
1. A method for preparing a hydrophilic and anticoagulant enhanced dual-functional coating, characterized in that: The following steps are involved: S1. synthesizing a hyaluronic acid-nitric oxide catalyst-dopamine product by an amidation reaction using the reaction between the carboxyl group of hyaluronic acid and the amino groups of dopamine hydrochloride and the nitric oxide catalyst; S2, dissolving the hyaluronic acid-nitric oxide catalyst-dopamine product in a phosphate buffer solution, and then adding NaOH to alkalize the solution; S3, continue to add PLGA-coated glycosaminoglycan to the solution obtained in step S2, and after dissolution, obtain a coating solution; S4. Soaking the substrate in the coating solution, then washing and vacuum drying to obtain a sample with a hydrophilic and anticoagulation enhanced dual-functional coating.
2. The preparation method according to claim 1, characterized in that: The specific preparation process of the hyaluronic acid-nitric oxide catalyst-dopamine product in step S1 includes the following steps: (1) dissolving sodium hyaluronate and nitric oxide catalyst in ultrapure water, and adjusting the pH of the solution to a weakly acidic pH of 5 to 5.5; (2) adding 1-ethyl-(3-dimethylaminopropyl)carbodiimide and N-hydroxysuccinimide to the solution obtained in step (1), and stirring evenly for 20-30 minutes to activate the carboxyl groups; (3) adding dopamine hydrochloride to the solution obtained in step (2), and then stirring for 10-15 hours under light-proof conditions; (4) The reaction product obtained in step (3) is transferred into a dialysis bag for dialysis, and then freeze-dried to obtain a hyaluronic acid-nitric oxide catalyst-dopamine product, which is stored for later use.
3. The preparation method according to claim 2, characterized in that: In step (1), sodium hyaluronate and a nitric oxide catalyst are dissolved in ultrapure water, wherein the mass fraction of sodium hyaluronate in the obtained solution is 0.5 to 3 wt %, and the mass fraction of the nitric oxide catalyst is 1 to 5 wt %; The mass ratio of 1-ethyl-(3-dimethylaminopropyl)carbodiimide, N-hydroxysuccinimide used in step (2), dopamine hydrochloride used in step (3) and sodium hyaluronate in step (1) is 0.3-0.6: 0.2-0.5: 0.2-2: 0.5-3.
4. The preparation method according to claim 1, characterized in that: In step S1, the nitric oxide catalyst is one or more cystamine hydrochloride compounds containing a diselenide bond, a ditellurium bond or a disulfide bond.
5. The preparation method according to claim 1, characterized in that: The preparation process of the PLGA-coated glycosaminoglycan used in step S3 is as follows: dissolving polylactic acid-glycolic acid copolymer in dichloromethane solvent, adding glycosaminoglycan to the above solution, ice bathing, ultrasonication for 20-30s, and then mixing with polyvinyl alcohol aqueous solution and ultrasonication, stirring the formed emulsion for 12-24h; then centrifugation washing, resuspending in ultrapure water and freeze-drying to obtain PLGA-coated glycosaminoglycan, which is stored for later use.
6. The preparation method according to claim 5, characterized in that: The polylactic acid-glycolic acid copolymer is dissolved in a dichloromethane solvent, wherein the mass fraction of the polylactic acid-glycolic acid copolymer in the obtained solution is 1-5wt%; the mass fraction of the polyvinyl alcohol in the polyvinyl alcohol aqueous solution is 1-5wt%; The mass ratio of polylactic acid-co-glycolic acid to glycosaminoglycan is 1-5:2-15; Among them, the glycosaminoglycan is one or more of heparan sulfate (heparin), dermatan sulfate, keratan sulfate, and chondroitin sulfate.
7. The preparation method according to claim 1, characterized in that: In step S2, the hyaluronic acid-nitric oxide catalyst-dopamine product is dissolved in a phosphate buffer solution, and the concentration of the resulting solution is 2-10 wt %; the mass ratio of NaOH to the hyaluronic acid-nitric oxide catalyst-dopamine product is 0.2-2:2-10; In step S3, the mass ratio of PLGA-coated glycosaminoglycan to hyaluronic acid-nitric oxide catalyst-dopamine product is 0.2-8:2-10.
8. The preparation method according to claim 1, characterized in that: In step S4, the substrate is made of metal or high molecular polymer. The metal substrate is stainless steel, magnesium sheet or titanium sheet. The high molecular polymer substrate is polymethacrylate, polyurethane, polydimethylsiloxane or polyvinyl chloride.
9. The preparation method according to claim 8, characterized in that: Before immersion, the substrate was ultrasonically cleaned with acetone, methanol and ethanol for 10-15 minutes respectively.
10. A hydrophilic and anticoagulant enhanced dual-functional coating, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 9.