A method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride
By using a boron-doped zinc oxide and cobalt-cerium phosphate composite catalyst, the problems of impurities and byproducts in the synthesis of 3-chloro-2-hydroxypropyltrimethylammonium chloride were solved, achieving high selectivity and high conversion rate, which is suitable for industrial production.
Patent Information
- Application Number
- CN202411336672.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-25
AI Technical Summary
The existing synthesis process of 3-chloro-2-hydroxypropyltrimethylammonium chloride contains impurities and many byproducts, especially epichlorohydrin and 1,3-dichloro-2-propanol, which are difficult to remove and affect product performance.
A composite material of boron-doped zinc oxide and cobalt cerium phosphate was used as a catalyst. The catalyst was prepared by hydrothermal reaction and calcination and used for the reaction of trimethylamine hydrochloride and epichlorohydrin to reduce by-products and improve product selectivity.
It significantly improves the selectivity and conversion rate of 3-chloro-2-hydroxypropyltrimethylammonium chloride, has good catalyst stability, is suitable for multiple industrial production processes, and reduces costs.
Smart Images

Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of chemical synthesis, and specifically relates to a preparation method of 3-chloro-2-hydroxypropyltrimethylammonium chloride. Background Art
[0002] 3-Chloro-2-hydroxypropyltrimethylammonium chloride (CHPTMAC) is a quaternary ammonium cationic etherifying agent. Because of its quaternary ammonium salt structure, it has a certain positive charge and is a multifunctional fine chemical. It is also an important reaction intermediate for organic synthesis. CHPTMAC has strong cationicity and strong bonding properties. It can react with macromolecular compounds such as starch and cellulose to obtain modified starch and modified cellulose. It is widely used in salt-free printing and dyeing, papermaking auxiliaries, cotton fiber textiles, petroleum extraction, daily chemical and other medium and light industrial fields.
[0003] 3-Chloro-2-hydroxypropyltrimethylammonium chloride is mainly synthesized by reacting raw materials such as hydrochloric acid, trimethylamine aqueous solution, and epichlorohydrin in an aqueous phase system. The preparation process route in the aqueous phase is relatively short, the cost is relatively low, and it is suitable for industrialization. However, impurities and more by-products will be accompanied by the reaction process. The main impurity is residual epichlorohydrin, and the by-products are mainly 1,3-dichloro-2-propanol, diquaternary ammonium salt, 2,3-dihydroxypropyl-trimethylammonium chloride, etc. Among them, epichlorohydrin and 1,3-dichloro-2-propanol will seriously affect the performance of the cationic etherifying agent, especially 1,3-dichloro-2-propanol is difficult to remove due to its high boiling point. Therefore, it is of great significance to study the synthesis process with less residual reactants and high selectivity of 3-chloro-2-hydroxypropyltrimethylammonium chloride. Summary of the invention
[0004] In view of the problems of impurities and more by-products in the synthesis process of 3-chloro-2-hydroxypropyltrimethylammonium chloride in the prior art, the present invention provides a method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride. The method uses a composite material of boron-doped zinc oxide and cerium cobalt phosphate as a catalyst, so as to effectively improve the conversion rate of reactants, reduce the residual epichlorohydrin content, inhibit the occurrence of side reactions, and improve the selectivity of 3-chloro-2-hydroxypropyltrimethylammonium chloride products. At the same time, the catalyst has excellent stability, can be repeatedly used in industrial production, and significantly reduces costs.
[0005] The first aspect of the present invention provides a method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride, comprising the following steps:
[0006] S1: dissolving cobalt nitrate hexahydrate in deionized water, heating and stirring to mix, then adding citric acid, and continuing heating and stirring to form a mixed solution;
[0007] S2: adding boron-doped ZnO (B-ZnO), ammonium dihydrogen phosphate, and cerium nitrate hexahydrate into the mixed solution, and then continuously stirring, drying, and calcining under inert gas conditions to obtain a catalyst;
[0008] S3: Add trimethylamine hydrochloride and a catalyst into a reaction kettle, turn on the refrigeration and cooling equipment, control the temperature at 5-20°C, then add epichlorohydrin, and keep the temperature within the range of 5-20°C for 6-12 hours to obtain 3-chloro-2-hydroxypropyltrimethylammonium chloride.
[0009] Furthermore, potassium borohydride, zinc nitrate hexahydrate and urea are dispersed in a mixed solution of ethylene glycol and deionized water in sequence, and transferred to a high-pressure hydrothermal reactor for hydrothermal reaction, and B-ZnO is obtained after filtering, washing and drying.
[0010] Furthermore, the mass ratio of potassium borohydride, zinc nitrate hexahydrate, and urea is 1:5:10~20; and the volume ratio of ethylene glycol and deionized water is 1:2.
[0011] Furthermore, the hydrothermal reaction temperature in the high-pressure hydrothermal reactor is 160~180°C, and the reaction time is 20~24h.
[0012] Furthermore, in step S1, the concentration of cobalt nitrate hexahydrate after being dissolved in deionized water is 1 mol / L, the molar ratio of cobalt nitrate hexahydrate to citric acid is 1:1-1.5, and the temperature of heating and stirring is 60-70°C.
[0013] Furthermore, in step S2, the addition ratio of B-ZnO, ammonium dihydrogen phosphate, cerium nitrate hexahydrate and the mixed solution is 1g:1g:0.5~1g:30mL.
[0014] Furthermore, in step S2, the calcination temperature is 500-550° C. and the calcination time is 3-4 hours.
[0015] Furthermore, in step S3, the mass ratio of trimethylamine hydrochloride to the catalyst is 100:3-10.
[0016] Furthermore, in step S3, the molar ratio of epichlorohydrin to trimethylamine hydrochloride is 0.95:1.
[0017] Furthermore, the obtained 3-chloro-2-hydroxypropyltrimethylammonium chloride is subjected to reduced pressure distillation, concentration and subsequent treatment.
[0018] The beneficial effects achieved by one or more technical solutions of the present invention are as follows:
[0019] The present invention uses boron-doped ZnO as a catalyst basis and composites cobalt and cerium bimetallic phosphates. The two work synergistically to exert good catalytic activity, effectively improve the conversion rate of reactants, and inhibit the occurrence of side reactions. The present invention uses boron to dope ZnO. On the one hand, it brings more active sites to the surface of ZnO, which is helpful for the loading of the composite cobalt and cerium bimetallic phosphate, improves the dispersion of active metals, and inhibits the agglomeration of active metals. On the other hand, Co-B-Ce bonds are formed between the doped boron and Co and Ce, which enriches more metals on the surface of ZnO and can also enhance the stability of the catalyst structure, so that the active metal is not easy to be stripped off and can be repeatedly used in industrial production. DETAILED DESCRIPTION
[0020] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.
[0021] Example 1
[0022] This embodiment provides a method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride, and the specific steps are:
[0023] S1: 1 g potassium borohydride, 5 g zinc nitrate hexahydrate, and 10 g urea were dispersed in a mixed solution of 20 mL ethylene glycol and 40 mL deionized water, and transferred to a high-pressure hydrothermal reactor for hydrothermal reaction at 180 ° C for 20 h, and B-ZnO was obtained after filtration, washing, and drying;
[0024] S2: dissolving cobalt nitrate hexahydrate in deionized water to form a 1 mol / L cobalt nitrate solution, heating and stirring at 70° C. to mix, then adding citric acid (the molar ratio of cobalt nitrate hexahydrate to citric acid is 1:1), and continuing heating and stirring to form a mixed solution;
[0025] S3: 4 g B-ZnO, 4 g ammonium dihydrogen phosphate, and 2 g cerium nitrate hexahydrate were added to 120 mL of the mixed solution, and then stirred continuously. After drying, the mixture was calcined at 550° C. for 3 h under inert gas conditions to obtain a catalyst;
[0026] S4: Add 50g of trimethylamine hydrochloride and 80mL of deionized water into the reactor, stir thoroughly to dissolve, add 2.5g of catalyst, turn on the refrigeration and cooling equipment, control the temperature at 5°C, then add epichlorohydrin (the molar ratio of epichlorohydrin to trimethylamine hydrochloride is 0.95:1), keep warm at 5°C for 10h, and obtain crude 3-chloro-2-hydroxypropyltrimethylammonium chloride. After further reduced pressure distillation and concentration, 3-chloro-2-hydroxypropyltrimethylammonium chloride is obtained.
[0027] Example 2
[0028] This embodiment provides a method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride, and the specific steps are:
[0029] S1: 1 g potassium borohydride, 5 g zinc nitrate hexahydrate, and 10 g urea were dispersed in a mixed solution of 20 mL ethylene glycol and 40 mL deionized water, and transferred to a high-pressure hydrothermal reactor for hydrothermal reaction at 160 ° C for 24 h, and B-ZnO was obtained after filtration, washing, and drying;
[0030] S2: dissolving cobalt nitrate hexahydrate in deionized water to form a 1 mol / L cobalt nitrate solution, heating and stirring at 70° C. to mix, then adding citric acid (the molar ratio of cobalt nitrate hexahydrate to citric acid is 1:1), and continuing heating and stirring to form a mixed solution;
[0031] S3: 4 g B-ZnO, 4 g ammonium dihydrogen phosphate, and 2 g cerium nitrate hexahydrate were added to 120 mL of the mixed solution, and then stirred continuously. After drying, the mixture was calcined at 550° C. for 3 h under inert gas conditions to obtain a catalyst;
[0032] S4: Add 50g of trimethylamine hydrochloride and 80mL of deionized water into the reactor, stir thoroughly to dissolve, add 1.5g of catalyst, turn on the refrigeration and cooling equipment, control the temperature at 10°C, then add epichlorohydrin (the molar ratio of epichlorohydrin to trimethylamine hydrochloride is 0.95:1), keep warm at a temperature range of 10°C for 12h, and obtain crude 3-chloro-2-hydroxypropyltrimethylammonium chloride. After further reduced pressure distillation and concentration, 3-chloro-2-hydroxypropyltrimethylammonium chloride is obtained.
[0033] Example 3
[0034] This embodiment provides a method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride, and the specific steps are:
[0035] S1: 1 g potassium borohydride, 5 g zinc nitrate hexahydrate, and 20 g urea were dispersed in a mixed solution of 20 mL ethylene glycol and 40 mL deionized water, and transferred to a high-pressure hydrothermal reactor for hydrothermal reaction at 180 ° C for 20 h, and B-ZnO was obtained after filtration, washing, and drying;
[0036] S2: dissolving cobalt nitrate hexahydrate in deionized water to form a 1 mol / L cobalt nitrate solution, heating and stirring at 60° C. to mix, then adding citric acid (the molar ratio of cobalt nitrate hexahydrate to citric acid is 1:1.5), and continuing heating and stirring to form a mixed solution;
[0037] S3: 4 g B-ZnO, 4 g ammonium dihydrogen phosphate, and 4 g cerium nitrate hexahydrate were added to 120 mL of the mixed solution, and then stirred continuously. After drying, the mixture was calcined at 550° C. for 3 h under inert gas conditions to obtain a catalyst;
[0038] S4: Add 50g of trimethylamine hydrochloride and 80mL of deionized water into the reactor, stir thoroughly to dissolve, add 3g of catalyst, turn on the refrigeration and cooling equipment, control the temperature at 20°C, then add epichlorohydrin (the molar ratio of epichlorohydrin to trimethylamine hydrochloride is 0.95:1), keep warm at a temperature range of 20°C for 12h to obtain crude 3-chloro-2-hydroxypropyltrimethylammonium chloride, and further distill under reduced pressure, concentrate and subsequently treat to obtain 3-chloro-2-hydroxypropyltrimethylammonium chloride.
[0039] Example 4
[0040] This embodiment provides a method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride, and the specific steps are:
[0041] S1: 1 g potassium borohydride, 5 g zinc nitrate hexahydrate, and 20 g urea were dispersed in a mixed solution of 20 mL ethylene glycol and 40 mL deionized water, and transferred to a high-pressure hydrothermal reactor for hydrothermal reaction at 180 ° C for 24 h, and B-ZnO was obtained after filtration, washing, and drying;
[0042] S2: dissolving cobalt nitrate hexahydrate in deionized water to form a 1 mol / L cobalt nitrate solution, heating and stirring at 60° C. to mix well, then adding citric acid (the molar ratio of cobalt nitrate hexahydrate to citric acid is 1:1), and continuing heating and stirring to form a mixed solution;
[0043] S3: 4 g B-ZnO, 4 g ammonium dihydrogen phosphate, and 4 g cerium nitrate hexahydrate were added to 120 mL of the mixed solution, and then stirred continuously. After drying, the mixture was calcined at 500° C. for 4 h under inert gas conditions to obtain a catalyst;
[0044] S4: Add 50g of trimethylamine hydrochloride and 80mL of deionized water into the reactor, stir thoroughly to dissolve, add 5g of catalyst, turn on the refrigeration and cooling equipment, control the temperature at 10°C, then add epichlorohydrin (the molar ratio of epichlorohydrin to trimethylamine hydrochloride is 0.95:1), keep warm at a temperature range of 10°C for 12h to obtain crude 3-chloro-2-hydroxypropyltrimethylammonium chloride, and further distill under reduced pressure, concentrate and subsequently treat to obtain 3-chloro-2-hydroxypropyltrimethylammonium chloride.
[0045] Comparative Example 1
[0046] This comparative example provides a method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride, and the specific steps are:
[0047] S1: 5 g zinc nitrate hexahydrate and 10 g urea were dispersed in a mixed solution of 20 mL ethylene glycol and 40 mL deionized water, and transferred to a high-pressure hydrothermal reactor for hydrothermal reaction at 180 ° C for 20 h, and ZnO was obtained after filtration, washing and drying;
[0048] S2: dissolving cobalt nitrate hexahydrate in deionized water to form a 1 mol / L cobalt nitrate solution, heating and stirring at 70° C. to mix, then adding citric acid (the molar ratio of cobalt nitrate hexahydrate to citric acid is 1:1), and continuing heating and stirring to form a mixed solution;
[0049] S3: 4 g ZnO, 4 g ammonium dihydrogen phosphate, and 2 g cerium nitrate hexahydrate were added to 120 mL of the mixed solution, and then stirred continuously. After drying, the mixture was calcined at 550° C. for 3 h under inert gas conditions to obtain a catalyst;
[0050] S4: Add 50g of trimethylamine hydrochloride and 80mL of deionized water into the reactor, stir thoroughly to dissolve, add 2.5g of catalyst, turn on the refrigeration and cooling equipment, control the temperature at 5°C, then add epichlorohydrin (the molar ratio of epichlorohydrin to trimethylamine hydrochloride is 0.95:1), keep warm at 5°C for 10h, and obtain crude 3-chloro-2-hydroxypropyltrimethylammonium chloride. After further reduced pressure distillation and concentration, 3-chloro-2-hydroxypropyltrimethylammonium chloride is obtained.
[0051] Comparative Example 2
[0052] This comparative example provides a method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride, and the specific steps are:
[0053] S1: 1 g potassium borohydride, 5 g zinc nitrate hexahydrate, and 10 g urea were dispersed in a mixed solution of 20 mL ethylene glycol and 40 mL deionized water, and transferred to a high-pressure hydrothermal reactor for hydrothermal reaction at 180 ° C for 20 h, and B-ZnO was obtained after filtration, washing, and drying;
[0054] S2: dissolving cobalt nitrate hexahydrate in deionized water to form a 1 mol / L cobalt nitrate solution, heating and stirring at 70° C. to mix, then adding citric acid (the molar ratio of cobalt nitrate hexahydrate to citric acid is 1:1), and continuing heating and stirring to form a mixed solution;
[0055] S3: 4 g B-ZnO and 4 g ammonium dihydrogen phosphate were added to 120 mL of the mixed solution, and then stirred continuously. After drying, the mixture was calcined at 550 °C for 3 h under inert gas conditions to obtain a catalyst;
[0056] S4: Add 50g of trimethylamine hydrochloride and 80mL of deionized water into the reactor, stir thoroughly to dissolve, add 2.5g of catalyst, turn on the refrigeration and cooling equipment, control the temperature at 5°C, then add epichlorohydrin (the molar ratio of epichlorohydrin to trimethylamine hydrochloride is 0.95:1), keep warm at 5°C for 10h, and obtain crude 3-chloro-2-hydroxypropyltrimethylammonium chloride. After further reduced pressure distillation and concentration, 3-chloro-2-hydroxypropyltrimethylammonium chloride is obtained.
[0057] Table 1 shows the content (mass percentage, %) of 3-chloro-2-hydroxypropyltrimethylammonium chloride in the materials finally obtained in Examples 1 to 4 and Comparative Examples 1 to 2.
[0058] Table 1
[0059]
[0060] As can be seen from Table 1, by using the preparation method provided by the present invention, 3-chloro-2-hydroxypropyltrimethylammonium chloride accounts for more than 98% of the total product mass, indicating excellent selectivity; the total mass of unreacted raw materials and by-products accounts for less than 2%, indicating that the conversion rate of the reactants is improved and the side reactions are effectively suppressed.
[0061] Table 2 shows the change in the content (mass percentage, %) of 3-chloro-2-hydroxypropyltrimethylammonium chloride in the product after the catalysts prepared in Examples 1 to 4 were continuously operated for a period of time.
[0062] Table 2
[0063]
[0064] It can be seen that after the catalysts in Examples 1 to 4 were continuously operated for 480 h, the selectivity of 3-chloro-2-hydroxypropyltrimethylammonium chloride did not significantly decay, proving that the catalyst prepared in the process has excellent stability and can be repeatedly used in the industrial production of 3-chloro-2-hydroxypropyltrimethylammonium chloride, thereby effectively reducing costs.
Claims
1. A method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride, characterized in that: The steps include: S1: dissolving cobalt nitrate hexahydrate in deionized water, heating and stirring to mix, then adding citric acid, and continuing heating and stirring to form a mixed solution; S2: adding B-ZnO, ammonium dihydrogen phosphate and cerium nitrate hexahydrate into the mixed solution, and then continuously stirring, drying, and calcining under inert gas conditions to obtain a catalyst; S3: adding trimethylamine hydrochloride and a catalyst to a reaction kettle, turning on a refrigeration and cooling device, controlling the temperature at 5-20° C., then adding epichlorohydrin, and keeping the temperature at 5-20° C. for 6-12 hours to obtain 3-chloro-2-hydroxypropyltrimethylammonium chloride; The B-ZnO is boron-doped ZnO; Potassium borohydride, zinc nitrate hexahydrate, and urea are dispersed in a mixed solution of ethylene glycol and deionized water in sequence, and transferred to a high-pressure hydrothermal reactor for hydrothermal reaction, and B-ZnO is obtained after filtering, washing, and drying; In step S2, the addition ratio of B-ZnO, ammonium dihydrogen phosphate, cerium nitrate hexahydrate and the mixed solution is 1g:1g:0.5~1g:30mL.
2. The method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride according to claim 1, characterized in that: The mass ratio of potassium borohydride, zinc nitrate hexahydrate, and urea is 1:5:10-20; the volume ratio of ethylene glycol and deionized water is 1:
2.
3. The method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride according to claim 1, characterized in that: The hydrothermal reaction temperature in the high-pressure hydrothermal reactor is 160~180℃, and the reaction time is 20~24h.
4. The method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride according to claim 1, characterized in that: In step S1, the concentration of cobalt nitrate hexahydrate after being dissolved in deionized water is 1 mol / L, the molar ratio of cobalt nitrate hexahydrate to citric acid is 1:1-1.5, and the temperature of heating and stirring is 60-70°C.
5. The method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride according to claim 1, characterized in that: In step S2, the calcination temperature is 500-550°C and the calcination time is 3-4 hours.
6. The method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride according to claim 1, characterized in that: In step S3, the mass ratio of trimethylamine hydrochloride to the catalyst is 100:3-10.
7. The method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride according to claim 1, characterized in that: In step S3, the molar ratio of epichlorohydrin to trimethylamine hydrochloride is 0.95:
1.
8. The method for preparing 3-chloro-2-hydroxypropyltrimethylammonium chloride according to claim 1, characterized in that: The obtained 3-chloro-2-hydroxypropyltrimethylammonium chloride is subjected to reduced pressure distillation, concentration and subsequent treatment.
Citation Information
Patent Citations
Synthesis method of 3-chloro-2-hydroxypropyl-trimethylammonium chloride through alkaline immobilization ion liquid catalysis
CN102617365A
Boron-doped defective zinc oxide as well as preparation method and application thereof
CN112076738A
Cited By
Synthesis method of chloride-free cationic etherifying agent
CN121824331A