Crushing, tailing discarding and product extracting method for low-grade surface ore

Through the method of multi-stage crushing and vibration screening combined with magnetic pulley selection, the problem of low efficiency of low-grade vanadium-titanium magnetite in the crushing and screening process has been solved, significantly improving the ore grade and recovery rate, and reducing the grinding cost. , in line with the concepts of green mining and sustainable development.

CN118847320APending Publication Date: 2024-10-29PANZHIHUA GANGCHENG GRP MIYI RUIDI MINING
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411262877.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-10
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Low-grade vanadium-titanium magnetite has low efficiency during the crushing and screening process, making it difficult to effectively separate useful components from useless components, resulting in high production costs, low economic benefits, and increased grinding energy consumption, affecting production efficiency.

Method used

The method of multi-stage crushing and vibrating screening combined with magnetic pulley roughing and selection is used to gradually refine the ore particle size, and waste rocks and impurities are removed through multiple screenings and magnetic separations to improve the ore grade.

Benefits of technology

It significantly improves the recovery rate and grade of useful components of ore, reduces grinding costs, improves mill processing capacity and efficiency, and extends mill service life.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847320A_ABST
    Figure CN118847320A_ABST
Patent Text Reader

Abstract

The invention discloses a crushing, tailing discarding and product extracting method for low-grade surface ore, and belongs to the technical field of ore processing. The method comprises the following steps that coarse separation feeding and coarse crushing are sequentially conducted on the low-grade vanadium titano-magnetite, after coarse crushing is conducted on coarse crushing materials, waste rocks are discharged from the oversize part, medium crushing is conducted on the undersize part, and medium-broken products are obtained; and repeatedly carrying out vibration screening and fine crushing on the medium-broken products, and carrying out magnetic pulley fine selection on the screened undersize part to obtain a qualified grinding material. According to the method, the ore grinding granularity can be greatly reduced, meanwhile, the grade of the ore is remarkably improved after the tailings are discarded, the handling capacity of a mill is improved, the ore grinding efficiency of the mill is improved, and meanwhile the overall ore grinding cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ore processing, and in particular relates to a method for crushing and discarding low-grade off-balance sheet ores. Background Art

[0002] With the continuous development of the global economy and the advancement of science and technology, the demand for metals such as vanadium and titanium is increasing. Although low-grade vanadium-titanium magnetite has a low grade, it still contains a large amount of valuable metal elements. Effective processing of low-grade vanadium-titanium magnetite can meet market demand and ensure the security of national strategic resources. How to maximize the use of these resources through effective processing is the top priority of the development of the relevant industrial chain.

[0003] At present, in the process of low-grade strategic reserves, there are still some technical defects in the treatment of low-grade vanadium-titanium magnetite, which not only limit the effective utilization of ore, but also increase production costs and reduce overall economic benefits. First of all, the deficiencies in crushing and screening technology are the primary problem in the treatment of low-grade vanadium-titanium magnetite. Traditional crushing equipment may not be able to effectively cope with the complex characteristics of low-grade vanadium-titanium magnetite, resulting in low crushing efficiency and uneven particle size distribution; at the same time, the accuracy and efficiency of screening equipment are also limited, and it is difficult to effectively separate the useful components from the useless components in the ore, affecting the subsequent selection and smelting process. Secondly, since the content of useful components in low-grade ores is low and is often accompanied by a large amount of gangue and impurities, how to remove these useless parts through tailings and selection technology to improve the grade of the ore is a technical difficulty that still has obstacles. In addition, due to the poor crushing and screening effect, a large amount of useless materials will enter the mill to increase grinding energy consumption and wear, reduce grinding efficiency, and thus affect the overall production efficiency.

[0004] Therefore, how to improve the processing efficiency and grade of low-grade vanadium-titanium magnetite, reduce the grinding cost, and provide a new solution for the efficient utilization of low-grade ore is one of the current technical difficulties. Summary of the invention

[0005] The purpose of the present invention is to provide a method for crushing and discarding tailings of low-grade off-balance sheet ores, which can greatly reduce the grinding particle size of the ore. At the same time, after the tailings are discarded, the grade of the ore is significantly improved, which not only improves the processing capacity of the mill and the grinding efficiency of the mill, but also reduces the overall grinding cost.

[0006] The technical solution adopted to achieve the above purpose is to provide a method for crushing and discarding low-grade off-balance sheet ores, comprising the following steps:

[0007] (1) low-grade vanadium-titanium magnetite is coarsely fed with a particle size of 200 to 250 mm, low-grade vanadium-titanium magnetite with a particle size of more than 200 to 250 mm is coarsely crushed, and the coarsely crushed low-grade vanadium-titanium magnetite is mixed with low-grade vanadium-titanium magnetite with a particle size of less than 200 to 250 mm to obtain coarsely crushed material;

[0008] (2) The coarsely crushed material is roughly selected with a particle size of 75 to 100 mm by a magnetic pulley. After the rough selection, the waste rock is discharged from the part above the screen, and the rough selection product is obtained from the part below the screen;

[0009] (3) crushing the crude product to obtain a medium crushed product;

[0010] (4) subjecting the medium-sized broken materials to vibration screening of particle sizes of 20 to 25 mm, subjecting the medium-sized broken materials with particle sizes of more than 20 to 25 mm to the first fine crushing, and subjecting them to vibration screening again after the first fine crushing;

[0011] (5) The medium and fine crushed products with a particle size of less than 20 to 25 mm obtained in step (4) are subjected to vibration screening to a particle size of 10 to 12 mm. After screening, the part above the sieve is subjected to a second fine crushing and then to vibration screening again. The part below the sieve is finely selected by a magnetic pulley to obtain qualified abrasive.

[0012] The beneficial effects of the technical scheme adopted in the present invention are as follows: through coarse crushing, medium crushing, two fine crushings and multiple vibration screenings, combined with roughing and concentrating with a magnetic pulley, magnetic minerals (such as vanadium-titanium magnetite) and non-magnetic minerals (such as waste rock) can be effectively separated. This method ensures that the ore is fully crushed to different particle size ranges, so that fine-grained useful minerals that were originally difficult to separate or recover are exposed and have the opportunity to enter the subsequent concentration process. This multi-stage treatment significantly improves the recovery rate of useful components in the ore; by setting multiple particle size screening points, it helps to subdivide the ore into a more uniform particle size distribution, providing better conditions for subsequent processing; in the process of roughing and screening, a large amount of waste rock and non-magnetic minerals are discharged in time, reducing their proportion in subsequent processing, thereby improving the grade of the ore entering the concentration process, and the qualified abrasive after being selected by the magnetic pulley has a significantly increased magnetic mineral content, a significant reduction in non-magnetic impurities, and a significantly improved ore grade.

[0013] Preferably, the method for crushing and discarding low-grade off-balance sheet ores comprises the following steps:

[0014] (1) The low-grade vanadium-titanium magnetite with a particle size of 250 mm is subjected to coarse feeding, the low-grade vanadium-titanium magnetite with a particle size of more than 250 mm is subjected to coarse crushing, and the coarse crushed low-grade vanadium-titanium magnetite is mixed with the low-grade vanadium-titanium magnetite with a particle size of less than 250 mm to obtain coarse crushed material;

[0015] (2) The coarsely crushed material is subjected to rough selection with a particle size of 100 mm by a magnetic pulley. After rough selection, the waste rock is discharged from the part above the screen, and the rough selection product is obtained from the part below the screen;

[0016] (3) crushing the crude product to obtain a medium crushed product;

[0017] (4) subjecting the medium-sized broken materials to vibration screening of a particle size of 25 mm, subjecting the medium-sized broken materials with a particle size of more than 25 mm to a first fine crushing, and subjecting them to vibration screening again after the first fine crushing;

[0018] (5) The medium and fine crushed products with a particle size of less than 25 mm obtained in step (4) are subjected to 12 mm particle size vibration screening, and the part above the sieve is subjected to a second fine crushing and then vibrated screening again, and the part below the sieve is finely selected by a magnetic pulley to obtain qualified abrasive.

[0019] Preferably, in step (1), the coarse feeding adopts HPF1560 grizzly feeder; the coarse crushing adopts PEV1100*1200 jaw crusher with a processing capacity of 246-755 t / h.

[0020] More preferably, the belt power of the HPF1560 grizzly feeder is 25-35 kW, and the feeding capacity is 350-450 t / h.

[0021] More preferably, the belt power of the HPF1560 grizzly feeder is 30 kW and the feeding capacity is 400 t / h.

[0022] Preferably, the magnetic pulleys in step (2) and step (5) are both dry-selection CTDG1212 magnetic pulleys.

[0023] Preferably, the intermediate crushing in step (3) adopts CC400-B / EC cone crusher with a processing capacity of 177 to 605 t / h.

[0024] More preferably, the medium crusher adopts belt feeding, the belt power is 10-20kW, and the feeding amount is 350-450t / h.

[0025] More preferably, the medium crusher adopts belt feeding, the belt power is 15kW, and the feeding amount is 400t / h.

[0026] Preferably, the vibration screening in step (4) and step (5) uses a 2YKR3675H double-layer circular vibrating screen.

[0027] Preferably, the first fine crushing and the second fine crushing both use CC400-F cone crusher, and the processing capacity is 180-350t / h.

[0028] More preferably, the first fine crushing and the second fine crushing are both fed by belts, the belt power is 10-20 kW, and the feeding amount is 350-450 t / h.

[0029] More preferably, the first fine crushing and the second fine crushing are both fed by belts, the belt power is 15 kW, and the feeding amount is 400 t / h.

[0030] The present invention has the following beneficial effects:

[0031] (1) The method of the present invention can gradually refine the ore particle size from an initial size of less than 1000 mm to a final size of less than 12 mm through multi-stage crushing and vibration screening. This particle size refinement is more conducive to subsequent grinding efficiency and separation effect.

[0032] (2) During the crushing and screening process, the method of the present invention effectively removes waste rock and impurities with weak magnetic properties in the ore through two stages of magnetic separation, namely roughing and cleaning, thereby significantly improving the grade of TFe in the ore.

[0033] (3) The method of the present invention can improve the processing capacity of the mill, reduce the wear and energy consumption of the mill caused by useless materials, further improve the operating efficiency of the mill, extend the service life of the mill, thereby reducing the operating difficulty and labor costs, and is in line with the current concept of green mining and sustainable development. BRIEF DESCRIPTION OF THE DRAWINGS

[0034] Figure 1 It is the process flow chart of Example 1;

[0035] Figure 2 It is the process flow chart of Comparative Example 1;

[0036] Figure 3 This is the process flow chart of Comparative Example 2. DETAILED DESCRIPTION

[0037] The features and performance of the present invention are further described in detail below in conjunction with embodiments.

[0038] Example 1

[0039] Ore source: extra-surface ore from Baima mining area, with a TFe grade of 20.45%.

[0040] A method for crushing and discarding low-grade off-balance sheet ores, comprising the following steps:

[0041] (1) The low-grade vanadium-titanium magnetite is coarsely fed with a HPF1560 bar feeder at a particle size of 250 mm, and the low-grade vanadium-titanium magnetite with a particle size of more than 250 mm is coarsely crushed with a PEV1100*1200 jaw crusher. After coarse crushing, the coarse crushed material is mixed with the low-grade vanadium-titanium magnetite with a particle size of less than 250 mm to obtain coarse crushed material;

[0042] (2) The coarsely crushed material is subjected to rough selection with a 100 mm particle size by means of a dry selection CTDG1212 magnetic pulley. After rough selection, the waste rock is discharged from the part above the screen, and the rough selection product is obtained from the part below the screen;

[0043] (3) The roughing product is crushed by a CC400-B / EC cone crusher to obtain a medium crushed product;

[0044] (4) The medium-sized broken materials are vibrated and screened with a particle size of 25 mm using a 2YKR3675H double-layer circular vibrating screen, and the medium-sized broken materials with a particle size of more than 25 mm are crushed for the first time using a CC400-F cone crusher, and then vibrated and screened again after the first crushing;

[0045] (5) The medium and fine crushed products with a particle size of less than 25 mm obtained in step (4) are vibrated and screened to a particle size of 12 mm using a 2YKR3675H double-layer circular vibrating screen. The part above the screen is crushed for the second time using a CC400-F cone crusher and then vibrated and screened again. The part below the screen is dry-selected using a CTDG1212 magnetic pulley to obtain qualified abrasives.

[0046] The process flow chart of this embodiment is as follows Figure 1 As shown, the equipment and process parameters used in this embodiment are shown in Tables 1 to 3.

[0047] Table 1 Crushing equipment and process parameters

[0048]

[0049] Table 2 Screening equipment and process parameters

[0050]

[0051]

[0052] Table 3 Feeding equipment and process parameters

[0053]

[0054] After the off-surface ore in the Baima mining area is processed by the method of this embodiment, the qualified grinding material obtained has a particle size of less than 12 mm, a TFe grade of 38.2%, and a TFe recovery rate of 79%, which meets the grade requirement of the grinding material.

[0055] Comparative Example 1

[0056] The difference between this comparative example and Example 1 is that step (5) specifically comprises: subjecting the medium-sized and fine-sized products with a particle size of less than 25 mm obtained in step (4) to a 12 mm particle size vibration screening, wherein the part above the screen is waste rock, and the part below the screen is finely selected by a magnetic pulley to obtain qualified abrasive. The process flow chart of this comparative example is as follows: Figure 2As shown, other conditions such as equipment type and process parameters are the same as those in Example 1 of the present invention.

[0057] After the off-surface ore in the Baima mining area is processed by the method of this embodiment, the qualified in-grinding material particle size obtained is less than 12 mm, the TFe grade thereof is 33.5%, and the TFe recovery rate is 72%.

[0058] Comparative Example 2

[0059] The difference between this comparative example and Example 1 is that the roughing in step (2) of Example 1 is not performed. Figure 3 As shown, other conditions such as equipment type and process parameters are the same as those in Example 1 of the present invention.

[0060] After the off-surface ore of the Baima mining area is processed by the method of this embodiment, the qualified abrasive particle size obtained is less than

[0061] 12mm with a TFe grade of 28.3% , The recovery rate of TFe was 75%.

[0062] The present invention has been described according to the above embodiments. It should be understood that the above embodiments do not limit the present invention in any form. Any technical solutions obtained by equivalent replacement or equivalent transformation shall fall within the scope of the present invention.

Claims

1. A method for crushing and discarding low-grade off-balance sheet ores, characterized in that: The following steps are involved: (1) low-grade vanadium-titanium magnetite is coarsely fed with a particle size of 200 to 250 mm, low-grade vanadium-titanium magnetite with a particle size of more than 200 to 250 mm is coarsely crushed, and the coarsely crushed low-grade vanadium-titanium magnetite is mixed with low-grade vanadium-titanium magnetite with a particle size of less than 200 to 250 mm to obtain coarsely crushed material; (2) The coarsely crushed material is roughly selected with a particle size of 75 to 100 mm by a magnetic pulley. After the rough selection, the waste rock is discharged from the part above the screen, and the rough selection product is obtained from the part below the screen; (3) crushing the crude product to obtain a medium crushed product; (4) subjecting the medium-sized broken materials to vibration screening of particle sizes of 20 to 25 mm, subjecting the medium-sized broken materials with particle sizes of more than 20 to 25 mm to the first fine crushing, and subjecting them to vibration screening again after the first fine crushing; (5) The medium and fine crushed products with a particle size of less than 20 to 25 mm obtained in step (4) are subjected to vibration screening to a particle size of 10 to 12 mm. After screening, the part above the sieve is subjected to a second fine crushing and then to vibration screening again. The part below the sieve is finely selected by a magnetic pulley to obtain qualified abrasive.

2. The method for crushing and discarding low-grade off-balance sheet ores as claimed in claim 1, characterized in that: In the step (1), the coarse feeding adopts HPF1560 rod feeder; the coarse crushing adopts PEV1100*1200 jaw crusher with a processing capacity of 246-755t / h.

3. The method for crushing and discarding low-grade off-balance sheet ores as claimed in claim 2, characterized in that: The belt power of the HPF1560 grizzly feeder is 25-35 kW, and the feeding capacity is 350-450 t / h.

4. The method for crushing and discarding low-grade off-balance sheet ores as claimed in claim 1, characterized in that: The magnetic pulleys in step (2) and step (5) are both dry-selection CTDG1212 magnetic pulleys.

5. The method for crushing and discarding low-grade off-balance sheet ores as claimed in claim 1, characterized in that: In the step (3), the intermediate crushing adopts CC400-B / EC cone crusher with a processing capacity of 177 to 605 t / h.

6. The method for crushing and discarding low-grade off-balance sheet ores as claimed in claim 5, characterized in that: The intermediate crusher adopts belt feeding, the belt power is 10-20kW, and the feeding amount is 350-450t / h.

7. The method for crushing and discarding low-grade off-balance sheet ores as claimed in claim 1, characterized in that: The vibration screening in step (4) and step (5) both uses a 2YKR3675H double-layer circular vibration screen.

8. The method for crushing and discarding low-grade off-balance sheet ores as claimed in claim 1, characterized in that: The first fine crushing and the second fine crushing both adopt CC400-F cone crusher, and the processing capacity is 180-350t / h.

9. The method for crushing and discarding low-grade off-balance sheet ores as claimed in claim 8, characterized in that: The first fine crushing and the second fine crushing both adopt belt feeding, the belt power is 10-20kW, and the feeding amount is 350-450t / h.

Citation Information

Patent Citations

  • Novel technology of low-grade magnetite two-stage pre-selecting and crushing

    CN102230071A

  • Weathered ore-containing vanadium titano-magnetite pre-dressing technology

    CN104475214A

  • Method for recycling ore by discharging rock and discarding waste from vanadium titano-magnetite

    CN115069552A