Anti-cracking process for cold bending processing of deformed steel bar

By using self-lubricating coating and water grinding treatment in the anti-cracking process of rebar, the problem of surface cracks in the cold bending process of rebar is solved, the wear resistance, anti-corrosion and lubricity of the steel are improved, and the risk of cracking during the bending process is reduced. , extending the service life and avoiding waste of resources.

CN118847477APending Publication Date: 2024-10-29GUANGDONG TAIDU STEEL IND CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410843449.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Rebar is prone to small surface cracks during the cold bending process, resulting in unstable performance and waste of resources, making it unable to meet engineering requirements.

Method used

An anti-cracking process is adopted, including converter smelting, steel casting, surface water grinding and spraying of self-lubricating coating. The coating is composed of binder, polyethylene glycol, nickel nitrate, iron nitrate, water, polytetrafluoroethylene and polypolyol , reduce the stress and corrosion risk during bending through water grinding and coating treatment, improve surface smoothness and lubricity, and reduce the probability of cracking.

Benefits of technology

It can effectively reduce the probability of cracking during the bending process of rebar, improve the wear resistance, anti-corrosion performance and lubricity of steel, extend the service life and avoid waste of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847477A_ABST
    Figure CN118847477A_ABST
Patent Text Reader

Abstract

The invention discloses an anti-cracking technology for deformed steel bar cold bending machining. The anti-cracking technology comprises the following specific steps that S1, converter smelting is conducted; s2, casting steel: transferring molten steel smelted by the converter into a model, curing for a period of time, and separating from the model to obtain the deformed steel bar; s3, surface water grinding: grinding the surface of the deformed steel bar in a water grinding manner to remove oxides, rust and other impurities on the surface of the deformed steel bar so as to keep the surface of the deformed steel bar smooth; s4, coating spraying: preparing a self-lubricating coating, and uniformly spraying the self-lubricating coating on the surface of the deformed steel bar; the step S4 of coating spraying comprises the following specific steps: S41, surface cleaning; s42, drying is carried out; s43, a coating is sprayed; according to the anti-cracking technology for cold bending machining of the deformed steel bar, optimization is conducted from the two aspects of abrasion resistance, corrosion prevention, guarantee of the surface smoothness of the deformed steel bar and optimization of the surface lubricity of the deformed steel bar, and the cracking probability of the deformed steel bar in the bending process is further reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of threaded steel processing technology, and in particular to an anti-cracking technology for threaded steel cold bending processing. Background Art

[0002] Rebar, also known as hot-rolled ribbed steel bars, is an important material widely used in various fields such as construction, infrastructure construction, manufacturing, oil and gas industry, metallurgy and mining. In the construction industry, rebar is used to make concrete reinforcement, which increases the strength and toughness of concrete by increasing friction and reducing the relative sliding between the rebar and concrete. This material not only provides reliable support and connection solutions, but is also used in projects such as ports, docks, dams, power plants, transmission towers and pipelines to meet the needs of various industries for strength and reliability.

[0003] Although traditional hot bending methods can bend steel, the strength and toughness of steel will change under high temperatures, which may cause unstable performance of the bent steel and even safety hazards during use. In addition, hot bending also consumes a lot of energy, increasing production costs.

[0004] In contrast, cold bending is a more ideal processing method. By bending steel at room temperature, it avoids the impact of high temperature on steel performance and reduces energy consumption. However, cold bending also faces some challenges. Since steel has poor plasticity in a cold state, stress concentration and uneven deformation are prone to occur during the bending process, resulting in small cracks on the surface of the steel. These cracks will seriously affect the strength and durability of the steel, making it unable to meet engineering requirements, thereby causing a waste of resources.

[0005] Therefore, we proposed an anti-cracking process for cold bending of rebar. Summary of the invention

[0006] The invention discloses an anti-cracking process for cold bending of threaded steel, aiming at solving the technical problem that fine cracks may be generated on the surface of threaded steel during the bending process of threaded steel, and the threaded steel with fine cracks cannot be used any more, thus causing waste.

[0007] In order to achieve the above object, the present invention adopts the following technical solutions:

[0008] A crack-resistant process for cold bending of threaded steel, comprising the following specific steps: S1: converter smelting; S2: steel casting: transferring the molten steel after converter smelting to a model, solidifying it for a period of time, and then separating from the model to obtain threaded steel; S3: surface water grinding: grinding the surface of the threaded steel by water grinding to remove oxides, rust and other impurities on the surface of the threaded steel, so that the surface of the threaded steel remains smooth; S4: coating spraying: preparing a self-lubricating coating and spraying it evenly on the surface of the threaded steel; the S4, coating spraying comprises the following specific steps: S41: surface cleaning: using clean water above 90°C to clean the surface of the threaded steel after water grinding; S42: drying: moving the cleaned threaded steel to a dryer, setting the dryer temperature to 150°C, and drying time to 2 minutes; S43: coating spraying: spraying a self-lubricating coating on the surface of the threaded steel, wherein the self-lubricating coating comprises a binder, polyethylene glycol, nickel nitrate, ferric nitrate, water, polytetrafluoroethylene and polyol;

[0009] S44: Curing: Place the coated rebar at room temperature for 3-10 hours;

[0010] In S43, the mass ratio of the binder, polyethylene glycol, nickel nitrate, iron nitrate, water, polytetrafluoroethylene and polyol in the coating is 1:1:2:1.5:0.8:0.8:0.5;

[0011] In the S43, the binder in the coating is sodium tetrahydroxyaluminate, and the mass concentration is 10%-15%.

[0012] By spraying a coating on the surface of the threaded steel, wherein the sprayed coating is a wear-resistant and anti-corrosion coating, wherein the binder, polyethylene glycol, nickel nitrate and ferric nitrate can provide sufficient wear resistance and corrosion resistance for the surface of the threaded steel, and the surface of the threaded steel is treated by water grinding, the stress of the threaded steel during bending can be reduced by ensuring the smoothness of the surface of the threaded steel, and the use of the spray coating can prevent the surface of the threaded steel from being corroded and damaged during storage and transportation, which affects the smoothness of the surface of the threaded steel. In addition, based on the use of polytetrafluoroethylene and polyols, wherein polytetrafluoroethylene has the effects of low friction coefficient, wear resistance and corrosion resistance, and polyols are a surfactant with good lubrication effect, and polytetrafluoroethylene and polyols are highly compatible with binders, polyethylene glycol, nickel nitrate and ferric nitrate, so that the coating is a coating that integrates lubricity and wear resistance and corrosion resistance, and is optimized from two aspects of wear resistance and corrosion resistance, ensuring the smoothness of the surface of the threaded steel, and optimizing the lubricity of the surface of the threaded steel, thereby further reducing the probability of cracking during the bending process of the threaded steel.

[0013] In a preferred embodiment, the S1, converter smelting includes the following specific steps: S11: molten iron pretreatment: before the molten iron enters the converter, harmful elements in the molten iron are removed; S12: converter: molten iron and scrap steel are loaded, wherein the molten iron temperature is 1200°C-1300°C; S13: auxiliary material addition: boron element and tungsten-molybdenum alloy are added as auxiliary materials for steelmaking; S14: molten steel smelting: high-drawing supplementary blowing process is adopted to smelt the terminal molten steel according to the carbon content required by the steel grade; S15: tapping; the S12 , the mass proportion of molten iron is 70%-85%, and the mass proportion of scrap steel is 15%-30%; in the S14, in the auxiliary material addition, the boron element is hexagonal boron nitride, and the purity of the hexagonal boron nitride is 97%; in the S14, in the auxiliary material addition, the tungsten content in the tungsten-molybdenum alloy is 30%, and the molybdenum content is 70%; in the S14, in the auxiliary material addition, the ratio of hexagonal boron nitride to tungsten-molybdenum alloy is 1:1, and the mixture of hexagonal boron nitride and tungsten-molybdenum alloy accounts for 0.25-0.45 of the total amount of molten steel.

[0014] By providing boron element and tungsten-molybdenum alloy, the boron element can improve the strength and hardness of steel in the steelmaking process without reducing its plasticity and toughness. For rebar, it can achieve stable support for rebar without reducing its plasticity and toughness in the bending process, further reducing the possibility of cracks in the bending process of rebar. In addition, although boron nitride and hexagonal boron nitride both have excellent properties such as high hardness and high thermal conductivity, hexagonal boron nitride has higher chemical stability and physical properties due to different crystal structures. Therefore, in the steelmaking process, adding hexagonal boron nitride is more conducive to improving the strength and hardness of steel while ensuring the plasticity and toughness of steel. Both tungsten and molybdenum can be used for steelmaking. The tungsten element in the tungsten-molybdenum alloy can optimize the composition design and improve its tensile strength and toughness. Molybdenum can effectively improve the tensile strength and yield strength of steel. When used with hexagonal boron nitride, it can be optimized from multiple aspects such as plasticity, toughness, strength, tensile strength and yield strength, thereby optimizing the main body of the rebar and avoiding the generation of cracks while ensuring the support strength.

[0015] As can be seen from the above, an anti-cracking process for cold bending of threaded steel includes the following specific steps: S1: converter smelting; S2: steel casting: transferring the molten steel after converter smelting to a mold, and after solidifying for a period of time, separating from the mold to obtain threaded steel; S3: surface water grinding: grinding the surface of the threaded steel by water grinding to remove oxides, rust and other impurities on the surface of the threaded steel to keep the surface of the threaded steel smooth; S4: coating spraying: preparing a self-lubricating coating and spraying it evenly on the surface of the threaded steel; the S4, coating spraying includes the following Specific steps: S41: Surface cleaning: Use clean water above 90°C to clean the surface of the threaded steel after water grinding; S42: Drying: Move the cleaned threaded steel to the dryer, set the dryer temperature to 150°C, and the drying time to 2 minutes; S43: Spraying coating: Spray self-lubricating coating on the surface of the threaded steel, wherein the self-lubricating coating includes adhesive, polyethylene glycol, nickel nitrate, iron nitrate, water, polytetrafluoroethylene and polyol; S44: Curing: Place the coated threaded steel at room temperature for curing for 3-10 hours. The anti-cracking process for cold bending of threaded steel provided by the present invention is optimized from two aspects: wear resistance and corrosion resistance, ensuring the surface smoothness of threaded steel, and optimizing the surface lubricity of threaded steel, so as to further reduce the probability of cracking during the bending process of threaded steel. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 The present invention is a schematic diagram of the overall structure of an anti-cracking process for cold bending of threaded steel bars.

[0017] Figure 2 The present invention provides a specific flow chart of the coating spraying steps for the anti-cracking process of threaded steel cold bending.

[0018] Figure 3 The present invention provides a specific flow chart of the converter smelting steps for the anti-cracking process of cold bending of threaded steel. DETAILED DESCRIPTION

[0019] The technical solutions in the embodiments of the present invention will be described clearly and completely below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments.

[0020] The invention discloses an anti-cracking process for cold bending of threaded steel bars, which is mainly used in the production of threaded steel bars.

[0021] Example 1: Reference Figure 1 and Figure 2, an anti-cracking process for cold bending of threaded steel, comprising the following specific steps: S1: converter smelting; S2: steel casting: transferring the molten steel after converter smelting into a mold, and after solidifying for a period of time, separating from the mold to obtain threaded steel; S3: surface water grinding: grinding the surface of the threaded steel by water grinding to remove oxides, rust and other impurities on the surface of the threaded steel to keep the surface of the threaded steel smooth; S4: coating spraying: preparing a self-lubricating coating and spraying it evenly on the surface of the threaded steel;

[0022] S4, coating spraying includes the following specific steps: S41: surface cleaning: use clean water above 90°C to clean the surface of the rebar after water grinding; S42: drying: move the cleaned rebar to the dryer, set the dryer temperature to 150°C, and the drying time to 2 minutes; S43: spraying coating: spray self-lubricating coating on the surface of the rebar, wherein the self-lubricating coating includes a binder, polyethylene glycol, nickel nitrate, iron nitrate, water, polytetrafluoroethylene and polyol; S44: curing: place the coated rebar at room temperature for curing for 3-10 hours, wherein the sprayed coating is a wear-resistant and anti-corrosion coating, wherein the binder, polyethylene glycol, nickel nitrate and iron nitrate can provide sufficient wear-resistant and anti-corrosion properties for the surface of the rebar, and the surface of the rebar is cured by water grinding. Treatment can reduce the stress of rebar during bending by ensuring the smoothness of the rebar surface, and the use of spray coating can prevent the surface of rebar from being corroded and damaged during storage and transportation, which affects the smoothness of the rebar surface. In addition, based on the use of polytetrafluoroethylene and polyols, polytetrafluoroethylene has the effects of low friction coefficient, wear resistance and corrosion resistance, and polyols are a surfactant with good lubrication effect, and polytetrafluoroethylene and polyols are highly compatible with binders, polyethylene glycol, nickel nitrate and ferric nitrate. Therefore, the coating is a coating that integrates lubricity and wear resistance and corrosion resistance. It is optimized from two aspects: wear resistance and corrosion resistance, ensuring the smoothness of the rebar surface, and optimizing the lubricity of the rebar surface, thereby further reducing the probability of cracking during the bending process of the rebar.

[0023] Reference Figure 2 In a preferred embodiment, S43, the mass ratio of the binder, polyethylene glycol, nickel nitrate, iron nitrate, water, polytetrafluoroethylene and polyol in the coating is 1:1:2:1.5:0.8:0.8:0.5.

[0024] Reference Figure 2 In a preferred embodiment, S43, the binder in the coating is sodium tetrahydroxyaluminate, and the mass concentration is 10%-15%.

[0025] Reference Figure 3In a preferred embodiment, S1, converter smelting includes the following specific steps: S11: molten iron pretreatment: removing harmful elements in the molten iron before entering the converter; S12: converter: loading molten iron and scrap steel, wherein the molten iron temperature is 1200℃-1300℃; S13: auxiliary material addition: adding boron element and tungsten-molybdenum alloy as auxiliary materials for steelmaking; S14: molten steel smelting: adopting high-drawing supplementary blowing process, smelting the final molten steel according to the carbon content required by the steel grade; S15: tapping.

[0026] Reference Figure 3 In a preferred embodiment, in S12, the mass proportion of molten iron is 70%-85%, and the mass proportion of scrap steel is 15%-30%.

[0027] Reference Figure 3 In a preferred embodiment, S14, in the auxiliary material addition, the boron element is hexagonal boron nitride, and the purity of hexagonal boron nitride is 97%, wherein the boron element acts on the steelmaking process, which can improve the strength and hardness of the steel without reducing its plasticity and toughness. For rebar, it can achieve the stable support of the rebar without reducing its plasticity and toughness during the bending process, further reducing the possibility of cracks in the rebar bending process. In addition, although both boron nitride and hexagonal boron nitride have excellent properties such as high hardness and high thermal conductivity, due to the different crystal structures, hexagonal boron nitride has higher chemical stability and physical properties. Therefore, in the steelmaking process, adding hexagonal boron nitride is more conducive to improving the strength and hardness of the steel while ensuring the plasticity and toughness of the steel.

[0028] Reference Figure 3 In a preferred embodiment, S14, in the auxiliary material addition, the tungsten content in the tungsten-molybdenum alloy is 30%, and the molybdenum content is 70%.

[0029] Reference Figure 3 In a preferred embodiment, S14, in the auxiliary material addition, the ratio of hexagonal boron nitride and tungsten-molybdenum alloy is 1:1, and the mixture of hexagonal boron nitride and tungsten-molybdenum alloy accounts for 0.25-0.45 of the total amount of molten steel. In the tungsten-molybdenum alloy, both tungsten and molybdenum can be used for steelmaking. The tungsten element in the tungsten-molybdenum alloy can optimize the composition design and improve its tensile strength and toughness. Molybdenum can effectively improve the tensile strength and yield strength of steel. When used with hexagonal boron nitride, it can be optimized in terms of plasticity, toughness, strength, tensile strength and yield strength, thereby realizing the optimization of the main body of the rebar, while ensuring the support strength, avoiding the generation of cracks.

[0030] Embodiment 2:

[0031] 1. Comparative Example 1: By weight, 3 parts of high modulus potassium silicate, 2.5 parts of low modulus potassium silicate, 2 parts of lithium silicate, 2.5 parts of silica sol, 1 part of alumina sol, 1 part of nano zirconium oxide sol 1.6-2.4%, 0.8 part of silicon tripolyphosphate, and 5 parts of water were mixed, and stirred at a speed of 1300 r / min for 0.5 hour to obtain a coating;

[0032] 2. Comparative Example 2: 5 parts of phosphoric acid, 1 part of aluminum hydroxide, 1.5 parts of water, 0.05 parts of chromium oxide, 1.5 parts of silica sol, 2 parts of aluminum oxide, and 0.08 parts of magnesium oxide were mixed by weight, and stirred at a speed of 1300 r / min for 0.5 hour to obtain a coating;

[0033] 3. Comparative Example 3: According to weight fraction, 1 part of binder, 1 part of polyethylene glycol, 2 parts of nickel nitrate, 1.5 parts of ferric nitrate, 0.8 parts of water, 0.8 parts of polytetrafluoroethylene and 0.5 parts of polyol were mixed, and stirred at a speed of 1300 r / min for 0.5 hours to obtain a coating;

[0034] The coatings in the comparative examples were tested, and the comparison results are as follows:

[0035]

[0036] It can be seen from this that the coating in the present invention can simultaneously achieve the simultaneous optimization of wear resistance and corrosion protection as well as the lubrication of the threaded steel surface.

[0037] Embodiment 3:

[0038] 1. Comparative Example 1: Molybdenum steel;

[0039] 2. Comparative Example 2: chromized steel;

[0040] 3. Comparative Example 3: During the steelmaking process, hexagonal boron nitride accounting for 15% of the total amount of the molten iron and tungsten-molybdenum alloy accounting for 15% of the total amount of the molten iron are added to the molten iron, wherein the tungsten content of the tungsten-molybdenum alloy is 30% and the molybdenum content is 70%;

[0041] The steel in the comparative example was tested, and the comparison results are as follows:

[0042]

[0043]

[0044] It can be seen from this that the steel material of the present invention has excellent properties and can achieve the effect of avoiding the occurrence of cracks.

[0045] Working principle: The sprayed coating is a wear-resistant and anti-corrosion coating, in which the binder, polyethylene glycol, nickel nitrate and ferric nitrate can provide sufficient wear resistance and corrosion resistance for the surface of the rebar. The surface of the rebar is treated with water grinding, which can reduce the stress of the rebar during bending by ensuring the smoothness of the surface of the rebar. The use of spray coating can prevent the surface of the rebar from being corroded and damaged during storage and transportation, which affects the smoothness of the surface of the rebar. In addition, based on the use of polytetrafluoroethylene and polyols, polytetrafluoroethylene has a low friction coefficient, wear resistance and corrosion resistance, and polyols are a surfactant with good lubrication effect. Polytetrafluoroethylene and polyols are highly compatible with binders, polyethylene glycol, nickel nitrate and ferric nitrate. Therefore, the coating is a coating that integrates lubricity and wear resistance and corrosion resistance. It is optimized from two aspects: wear resistance and corrosion resistance, ensuring the smoothness of the rebar surface, and optimizing the lubricity of the rebar surface, thereby further reducing the probability of cracking during the bending of the rebar. The boron element acts in the steelmaking process. It can improve the strength and hardness of steel without reducing its plasticity and toughness. For rebar, it can achieve stable support for rebar without reducing its plasticity and toughness during bending, further reducing the possibility of cracks in the bending process of rebar. In addition, although both boron nitride and hexagonal boron nitride have excellent properties such as high hardness and high thermal conductivity, due to the different crystal structures, hexagonal boron nitride has higher chemical stability and physical properties. Therefore, in the steelmaking process, adding hexagonal boron nitride is more conducive to improving the strength and hardness of steel while ensuring the plasticity and toughness of steel. Tungsten and molybdenum can both be used for steelmaking. Tungsten in tungsten-molybdenum alloy can optimize the composition design and improve its tensile strength and toughness. Molybdenum can effectively improve the tensile strength and yield strength of steel. When used with hexagonal boron nitride, it can be optimized from multiple aspects such as plasticity, toughness, strength, tensile strength and yield strength, thereby optimizing the main body of the rebar and avoiding the generation of cracks while ensuring the support strength.

[0046] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An anti-cracking process for cold bending of threaded steel, characterized in that: The specific steps include: S1: converter smelting; S2: Cast steel: The molten steel after smelting in the converter is transferred to the mold. After solidification for a period of time, it is separated from the mold to obtain rebar; S3: Surface water grinding: Use water grinding to grind the surface of the rebar to remove oxides, rust and other impurities on the surface of the rebar to keep the surface of the rebar smooth; S4: coating spraying: prepare self-lubricating coating and spray it evenly on the surface of threaded steel; The S4, coating spraying comprises the following specific steps: S41: Surface cleaning: Use clean water above 90°C to clean the surface of the rebar after water grinding; S42: Drying: Move the cleaned rebar to a dryer, set the dryer temperature to 150°C, and the drying time to 2 minutes; S43: Spraying coating: spraying self-lubricating coating on the surface of threaded steel, wherein the self-lubricating coating comprises a binder, polyethylene glycol, nickel nitrate, iron nitrate, water, polytetrafluoroethylene and polyol; S44: Curing: Place the coated rebar at room temperature for 3-10 hours.

2. The anti-cracking process for cold bending of threaded steel according to claim 1, characterized in that: In the S43, the mass ratio of the binder, polyethylene glycol, nickel nitrate, iron nitrate, water, polytetrafluoroethylene and polyol in the coating is 1:1:2:1.5:0.8:0.8:0.

5.

3. The anti-cracking process for cold bending of threaded steel according to claim 2, characterized in that: In the S43, the binder in the coating is sodium tetrahydroxyaluminate, and the mass concentration is 10%-15%.

4. The anti-cracking process for cold bending of threaded steel according to claim 1, characterized in that: Said S1, converter smelting comprises the following specific steps: S11: Hot metal pretreatment: Remove harmful elements from hot metal before it enters the converter; S12: Converter: Loading molten iron and scrap steel, wherein the temperature of the molten iron is 1200℃-1300℃; S13: Adding auxiliary materials: adding boron element and tungsten-molybdenum alloy as auxiliary materials for steelmaking; S14: Molten steel smelting: adopt high-drawing and supplementary blowing process to smelt the final molten steel according to the carbon content required by the steel grade; S15: Steel tapping.

5. The anti-cracking process for cold bending of threaded steel according to claim 4, characterized in that: In S12, the mass proportion of molten iron is 70%-85%, and the mass proportion of scrap steel is 15%-30%.

6. The anti-cracking process for cold bending of threaded steel according to claim 4, characterized in that: In the S14, in the auxiliary material addition, the boron element is hexagonal boron nitride, and the purity of the hexagonal boron nitride is 97%.

7. The anti-cracking process for cold bending of threaded steel according to claim 4, characterized in that: In the S14, the auxiliary materials are added, and the tungsten content in the tungsten-molybdenum alloy is 30%, and the molybdenum content is 70%.

8. The anti-cracking process for cold bending of threaded steel according to claim 4, characterized in that: In the S14, in the auxiliary material addition, the ratio of hexagonal boron nitride to tungsten-molybdenum alloy is 1:1, and the mixture of hexagonal boron nitride and tungsten-molybdenum alloy accounts for 0.25-0.45 of the total amount of molten steel.