High-permeability temperature control type magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating as well as preparation method and application of high-permeability temperature control type magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating
Magnesium-doped vanadium dioxide is prepared by hydrothermal method and combined with thermochromic microcapsules to form a double-layer phase change coating, which solves the problem of insufficient light transmittance and adjustment ability of vanadium dioxide and achieves light transmittance and Significant improvement in temperature control capabilities.
Patent Information
- Application Number
- CN202410930461.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-10-29
AI Technical Summary
Vanadium dioxide's low light transmittance and insufficient light modulation capabilities limit its performance in temperature-controlled coating applications.
Magnesium-doped vanadium dioxide is prepared using a hydrothermal method and combined with thermochromic microcapsules to improve light transmittance and light regulation capabilities through a spin-coated double-layer structure.
The light transmittance is significantly increased to 50.87% and the temperature control capability is 12.7%, which enhances the practical application performance of the coating.
Smart Images

Figure CN118847480A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of organic-inorganic composite materials, and particularly relates to a high-permeability temperature-controlled magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase-change coating, and a preparation method and application thereof. Background Art
[0002] With the rapid growth of human demand for energy and the destruction of the environment, energy-saving materials and renewable energy have gradually entered people's horizons, among which the development and utilization of solar energy is an indispensable part. Driven by solar energy, the temperature-control coating automatically reduces its light transmittance when a certain temperature is reached, thereby adjusting the indoor temperature, which is in line with the concept of energy saving and green sustainable development.
[0003] Vanadium dioxide is the main component of temperature control coatings. It is in a semiconductor state at low temperatures and has a transparent effect on infrared rays. At high temperatures, it will turn into a metallic state to absorb infrared rays. By selectively transmitting near-infrared light, temperature can be controlled. The low light transmittance and limited light modulation ability of vanadium dioxide have caused certain problems in meeting practical applications.
[0004] At present, vanadium dioxide is mainly modified by doping elements, constructing core-shell structures and multilayer film structures, but a single modification method will improve one property while damaging another. Summary of the invention
[0005] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a high-transmittance temperature-controlled magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating and its preparation method and application, so as to solve the technical defects of vanadium dioxide's low light transmittance and light regulation ability.
[0006] In order to achieve the above object, the present invention adopts the following technical solutions:
[0007] The present invention discloses a method for preparing a high-transmittance temperature-controlled magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase-change coating, comprising the following steps:
[0008] 1) preparing magnesium-doped vanadium dioxide with phase change function by hydrothermal method using a vanadium source and a magnesium source;
[0009] 2) dispersing magnesium-doped vanadium dioxide with phase change function and thermochromic microcapsules with thermal response effect in polyurethane to prepare magnesium-doped vanadium dioxide emulsion and thermochromic microcapsule emulsion respectively;
[0010] 3) spin coating the magnesium-doped vanadium dioxide emulsion on the surface of the substrate to obtain a magnesium-doped vanadium dioxide phase change coating;
[0011] 4) The thermochromic microcapsule emulsion is then spin-coated on a substrate covered with a magnesium-doped vanadium dioxide phase change coating to obtain a high-transmittance temperature-controlled magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating.
[0012] Furthermore, the vanadium source is vanadium pentoxide or ammonium metavanadate; the magnesium source is magnesium oxide or magnesium oxalate.
[0013] Preferably, in step 1), the hydrothermal method is specifically performed as follows:
[0014] Dissolve vanadium pentoxide and oxalic acid in water, add a dopant, mix thoroughly, then add a hydrothermal reaction solvent, mix well, react at 200°C for 3-12 hours, centrifuge, wash and dry the precipitate to obtain magnesium-doped vanadium dioxide, anneal it at 300-800°C for 1-4 hours in an argon atmosphere to obtain magnesium-doped vanadium dioxide with phase change function.
[0015] Further preferably, the hydrothermal reaction solvent is methanol or isopropanol, and the volume ratio of water to the hydrothermal reaction solvent is 50%; the dopant is magnesium oxalate or magnesium oxide, and the mass ratio of magnesium in the dopant to vanadium in vanadium pentoxide is (0.1-1):10.
[0016] Preferably, in step 2), the thermochromic microcapsules with thermal response effect are 25°C thermochromic microcapsules, 35°C thermochromic microcapsules or 40°C thermochromic microcapsules.
[0017] Preferably, in step 2), the mass ratio of the total mass of the magnesium-doped vanadium dioxide having a phase change function and the thermochromic microcapsules having a thermal response effect to the polyurethane is (0.1-1):20.
[0018] Preferably, in step 3), the magnesium-doped vanadium dioxide emulsion is spin-coated on the surface of the substrate, cured and dried at 50-70° C. for 10-30 min, and left at room temperature for 2 h to obtain a magnesium-doped vanadium dioxide phase change coating.
[0019] Preferably, in step 4), the thermochromic microcapsule emulsion is spin-coated on the surface of the substrate covered with the magnesium-doped vanadium dioxide phase change coating, cured and dried at 50-70°C for 10-30 minutes, and left at room temperature for 2 hours to obtain a high-transmittance temperature-controlled magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating.
[0020] Preferably, the substrate is a glass substrate; and the number of spin coating is 1 to 3 times.
[0021] The invention also discloses a high-transmittance temperature-controlled magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase-change coating prepared by the above preparation method, wherein the magnesium-doped vanadium dioxide layer in the coating has a solid spherical, egg yolk-like or hollow spherical morphology.
[0022] The invention also discloses the application of the high-transmittance temperature-controlling magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase-change coating in the preparation of a temperature-controlling coating.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] The present invention combines doping elements with the construction of a multilayer film structure to improve the light transmittance of vanadium dioxide and increase the light regulation band range and light regulation ability. Magnesium-doped vanadium dioxide for regulating infrared light and thermochromic microcapsules for regulating visible light are used to prepare a magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating. On the one hand, the light transmittance of the coating is effectively improved, increasing the practical application performance; on the other hand, the synergistic effect of magnesium-doped vanadium dioxide and thermochromic microcapsules further improves the regulation ability and spectral regulation range of sunlight, thereby improving the temperature control ability of the coating. Compared with the vanadium dioxide coating, the light transmittance of the magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating prepared by the present invention is increased by 50.87%, and the temperature control ability is increased by 12.7%. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 The working mechanism diagram of the double-layer coating;
[0026] Figure 2 The XRD spectrum of magnesium-doped vanadium dioxide prepared by the present invention;
[0027] Figure 3 The SEM and magnified images of the magnesium-doped hollow vanadium dioxide prepared by the present invention; wherein (a) is the SEM image after being magnified 8000 times; (b) is the SEM image after being magnified 30000 times;
[0028] Figure 4 This is a light transmittance diagram of the magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating prepared by the present invention;
[0029] Figure 5 This is a diagram showing the actual temperature control effect of the magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating prepared by the present invention. DETAILED DESCRIPTION
[0030] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0031] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the data used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions, for example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units that are clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices.
[0032] See also Figure 1 , is a working mechanism diagram of the double-layer coating. It can be seen that at low temperatures, the top layer of the thermochromic microcapsule coating is transparent, allowing a large amount of light to pass through. At this time, the vanadium dioxide coating allows infrared light to pass through. When the ambient temperature rises, the top layer of the thermochromic microcapsule coating develops color, thereby reducing the transmission of light. At this time, the vanadium dioxide coating has a certain degree of blocking of infrared light, and the light transmission is further reduced, thereby achieving the purpose of indoor temperature control.
[0033] The present invention is further described in detail below in conjunction with specific embodiments and experimental results of the accompanying drawings:
[0034] The green thermochromic microcapsules with a color change temperature of 25°C, the purple thermochromic microcapsules with a color change temperature of 35°C, the blue thermochromic microcapsules with a color change temperature of 40°C, the green thermochromic microcapsules with a color change temperature of 40°C and the purple thermochromic microcapsules with a color change temperature of 25°C used in the following embodiments of the present invention were purchased from Shenzhen Huancai Bianse Technology Co., Ltd.
[0035] Example 1
[0036] (1) 0.4 g of vanadium pentoxide and 0.592 g of oxalic acid were dissolved in 50 mL of deionized water, and 0.004 g of magnesium oxalate dopant was added. The mixed solution was magnetically stirred at 40 ° C for 2 h, and then reacted in a high-pressure reactor at 200 ° C for 12 h. The precipitate was collected by centrifugation, washed with water and ethanol three times, and dried to obtain blue-black B-phase magnesium-doped solid vanadium dioxide; finally, it was placed in a tubular furnace and annealed at 600 ° C for 3 h in an argon atmosphere to obtain M-phase magnesium-doped solid vanadium dioxide.
[0037] (2) 0.5 g of M-phase magnesium-doped solid vanadium dioxide and 0.5 g of green thermochromic microcapsules with a color change temperature of 25° C. were added to 10 g of polyurethane and dispersed evenly to obtain a magnesium-doped solid vanadium dioxide emulsion and a thermochromic microcapsule emulsion.
[0038] (3) 1 g of magnesium-doped solid vanadium dioxide emulsion was spin-coated on the surface of the glass substrate three times, cured and dried at 50°C for 10 min, and left at room temperature for 2 h to obtain a magnesium-doped solid vanadium dioxide phase change coating. Then 1 g of thermochromic microcapsule emulsion was spin-coated on the surface three times, cured and dried at 50°C for 10 min, and left at room temperature for 2 h to obtain a magnesium-doped solid vanadium dioxide / thermochromic microcapsule double-layer phase change coating.
[0039] Note: Phase B and phase M refer to different crystal forms of vanadium dioxide (the same meaning is used in the following examples).
[0040] Example 2
[0041] (1) 0.4 g of vanadium pentoxide and 0.592 g of oxalic acid were dissolved in 5 mL of deionized water, and the mixed solution was magnetically stirred at 40 ° C for 2 h, then mixed evenly with 45 mL of isopropanol, and reacted in a high-pressure reactor at 200 ° C for 12 h. The precipitate was collected by centrifugation, washed with water and ethanol three times, and dried to obtain blue-black B-phase hollow vanadium dioxide; finally, it was placed in a tubular furnace and annealed at 600 ° C for 3 h in an argon atmosphere to obtain M-phase hollow vanadium dioxide.
[0042] (2) 1 g of M-phase hollow vanadium dioxide and 1 g of purple thermochromic microcapsules with a color change temperature of 35° C. were added to 10 g of polyurethane respectively and dispersed evenly to obtain a hollow vanadium dioxide emulsion and a thermochromic microcapsule emulsion.
[0043] (3) Spin-coat 1 g of hollow vanadium dioxide emulsion on the surface of a glass substrate, cure and dry at 60°C for 30 min, and leave at room temperature for 2 h to obtain a magnesium-doped hollow vanadium dioxide phase change coating. Then, spin-coat 1 g of thermochromic microcapsule emulsion on the surface, cure and dry at 60°C for 30 min, and leave at room temperature for 2 h to obtain a hollow vanadium dioxide / thermochromic microcapsule double-layer phase change coating.
[0044] Example 3
[0045] (1) 0.4 g of vanadium pentoxide and 0.592 g of oxalic acid were dissolved in 25 mL of deionized water, 0.01 g of magnesium oxide dopant was added, the mixed solution was magnetically stirred at 80 ° C for 2 h, and then mixed with 25 mL of isopropanol and reacted in a high-pressure reactor at 200 ° C for 4 h. The precipitate was collected by centrifugation, washed with water and ethanol three times, and dried to obtain blue-black B-phase magnesium-doped egg yolk-like vanadium dioxide; finally, it was placed in a tubular furnace and annealed at 600 ° C for 3 h in an argon atmosphere to obtain M-phase magnesium-doped egg yolk-like vanadium dioxide.
[0046] (2) 3 g of M-phase magnesium-doped egg yolk-like vanadium dioxide and 3 g of blue thermochromic microcapsules with a color change temperature of 40°C were added to 10 g of polyurethane and dispersed evenly to obtain a magnesium-doped egg yolk-like vanadium dioxide emulsion and a thermochromic microcapsule emulsion.
[0047] (3) Spin-coat 2 g of magnesium-doped egg yolk-like vanadium dioxide emulsion once on the surface of the substrate, cure and dry at 70°C for 20 min, and leave at room temperature for 2 h to obtain a magnesium-doped egg yolk-like vanadium dioxide phase change coating. Then, spin-coat 2 g of thermochromic microcapsule emulsion once on the surface, cure and dry at 70°C for 20 min, and leave at room temperature for 2 h to obtain a magnesium-doped egg yolk-like vanadium dioxide / thermochromic microcapsule double-layer phase change coating.
[0048] Example 4
[0049] (1) 0.4 g of vanadium pentoxide and 0.592 g of oxalic acid were dissolved in 25 mL of deionized water, 0.02 g of magnesium oxide dopant was added, the mixed solution was magnetically stirred at 40 ° C for 2 h, and then mixed with 25 mL of methanol solution and reacted in a high-pressure reactor at 200 ° C for 12 h. The precipitate was collected by centrifugation, washed with water and ethanol three times, and dried to obtain blue-black B-phase magnesium-doped hollow spherical vanadium dioxide; finally, it was placed in a tubular furnace and annealed at 600 ° C for 3 h in an argon atmosphere to obtain M-phase magnesium-doped solid vanadium dioxide.
[0050] (2) 2 g of M-phase magnesium-doped hollow spherical vanadium dioxide and 2 g of green thermochromic microcapsules with a color change temperature of 40°C were added to 10 g of polyurethane and dispersed evenly to obtain a magnesium-doped hollow spherical vanadium dioxide emulsion and a thermochromic microcapsule emulsion.
[0051] (3) Spin-coat 2 g of magnesium-doped hollow spherical vanadium dioxide emulsion on the surface of the substrate once, cure and dry at 60°C for 20 min, and leave at room temperature for 2 h to obtain a magnesium-doped hollow spherical vanadium dioxide phase change coating. Then, spin-coat 2 g of thermochromic microcapsule emulsion on the surface once, cure and dry at 70°C for 20 min, and leave at room temperature for 2 h to obtain a magnesium-doped solid vanadium dioxide / thermochromic microcapsule double-layer phase change coating.
[0052] Example 5
[0053] (1) 0.4 g of vanadium pentoxide and 0.592 g of oxalic acid were dissolved in 10 mL of deionized water, and 0.01 g of magnesium oxalate dopant was added. The mixed solution was magnetically stirred at 80 ° C for 2 h, and then mixed with 40 mL of methanol and reacted in a high-pressure reactor at 200 ° C for 4 h. The precipitate was collected by centrifugation, washed with water and ethanol three times, and dried to obtain blue-black B-phase magnesium-doped hollow vanadium dioxide; finally, it was placed in a tubular furnace and annealed at 600 ° C for 3 h in an argon atmosphere to obtain M-phase magnesium-doped hollow vanadium dioxide.
[0054] (2) 1 g of M-phase magnesium-doped hollow vanadium dioxide and 1 g of purple thermochromic microcapsules with a color change temperature of 25°C were added to 10 g of polyurethane respectively and dispersed evenly to obtain a magnesium-doped vanadium dioxide emulsion and a thermochromic microcapsule emulsion.
[0055] (3) 2 g of magnesium-doped vanadium dioxide emulsion was spin-coated twice on the surface of the substrate, cured and dried at 50°C for 10 min, and left at room temperature for 1 h to obtain a magnesium-doped vanadium dioxide phase change coating. Then 2 g of thermochromic microcapsule emulsion was spin-coated twice on the surface, cured and dried at 70°C for 20 min, and left at room temperature for 2 h to obtain a magnesium-doped hollow vanadium dioxide / thermochromic microcapsule double-layer phase change coating.
[0056] The following is a corresponding test using the magnesium-doped solid vanadium dioxide / thermochromic microcapsule double-layer phase change coating prepared in Example 1 as an example. Figure 2 The XRD spectra of the prepared magnesium-doped vanadium dioxide before and after magnesium doping. It can be seen from the figure that the products before and after doping match the standard card PDF43-1051, proving that magnesium doping does not affect the structure of vanadium dioxide. Figure 3 This is the SEM and magnified image of the prepared magnesium-doped hollow vanadium dioxide. It can be seen from the image that the magnesium-doped vanadium dioxide is a hollow spherical morphology with a diameter of approximately 1 to 3 μm. Figure 4 and Figure 5 The light transmittance and actual temperature control effect of the prepared magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating were studied. Vanadium dioxide and vanadium dioxide / green thermochromic microcapsule coatings were used for comparison. It can be seen that the magnesium-doped treatment of vanadium dioxide and its synergistic effect with thermochromic microcapsules can improve the light transmittance and temperature control ability of the coating. Compared with vanadium dioxide coating, its light transmittance is increased by 50.87% and its temperature control ability is increased by 12.7%.
[0057] In summary, the preparation method of the magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating disclosed in the present invention utilizes magnesium doping to expand the bandgap width of vanadium dioxide and thus improve the light transmittance. At the same time, it is considered that the thermochromic material can change its optical properties according to the ambient temperature, that is, the color development at high temperature reduces the visible light transmittance, and the color reduction at low temperature increases the visible light transmittance, so that at high temperature (low temperature), it can present a lower (higher) surface temperature than conventional materials. Therefore, the combination of two light-regulating materials, vanadium dioxide and thermochromic microcapsules, can achieve full-band regulation of visible light and infrared light, thereby improving the light transmittance and temperature control ability of the coating.
[0058] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a high-transmittance temperature-controlled magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating, characterized in that: The following steps are involved: 1) preparing magnesium-doped vanadium dioxide with phase change function by hydrothermal method using a vanadium source and a magnesium source; 2) dispersing magnesium-doped vanadium dioxide with phase change function and thermochromic microcapsules with thermal response effect in polyurethane to prepare magnesium-doped vanadium dioxide emulsion and thermochromic microcapsule emulsion respectively; 3) spin coating the magnesium-doped vanadium dioxide emulsion on the surface of the substrate to obtain a magnesium-doped vanadium dioxide phase change coating; 4) The thermochromic microcapsule emulsion is then spin-coated on a substrate covered with a magnesium-doped vanadium dioxide phase change coating to obtain a high-transmittance temperature-controlled magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating.
2. The method for preparing the high-transmittance temperature-controlling magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating according to claim 1, characterized in that: In step 1), the vanadium source is vanadium pentoxide or ammonium metavanadate; the magnesium source is magnesium oxide or magnesium oxalate; the hydrothermal method is specifically performed as follows: The vanadium source and oxalic acid are dissolved in water, a dopant is added, the mixture is thoroughly mixed, a hydrothermal reaction solvent is added, the mixture is mixed, and the mixture is reacted at 200°C for 3 to 12 hours. The mixture is centrifuged, and the precipitate is washed and dried to obtain magnesium-doped vanadium dioxide. The precipitate is annealed at 300-800°C for 1 to 4 hours in an argon atmosphere to obtain magnesium-doped vanadium dioxide with phase change function.
3. The method for preparing the high-transmittance temperature-controlling magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase-change coating according to claim 2, characterized in that: The hydrothermal reaction solvent is methanol or isopropanol, and the volume ratio of water to the hydrothermal reaction solvent is 50%; the dopant is magnesium oxalate or magnesium oxide, and the mass ratio of magnesium in the dopant to vanadium in vanadium pentoxide is (0.1-1):
10.
4. The method for preparing the high-transmittance temperature-controlling magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating according to claim 1, characterized in that: In step 2), the thermochromic microcapsules with thermal response effect are 25°C thermochromic microcapsules, 35°C thermochromic microcapsules or 40°C thermochromic microcapsules.
5. The method for preparing the high-transmittance temperature-controllable magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase-change coating according to claim 1, characterized in that: In step 2), the mass ratio of the total mass of magnesium-doped vanadium dioxide with phase change function and thermochromic microcapsules with thermal response effect to polyurethane is (0.1-1):
20.
6. The method for preparing the high-transmittance temperature-controlling magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase-change coating according to claim 1, characterized in that: In step 3), the magnesium-doped vanadium dioxide emulsion is spin-coated on the surface of the substrate, cured and dried at 50-70° C. for 10-30 min, and left at room temperature for 2 h to obtain a magnesium-doped vanadium dioxide phase change coating.
7. The method for preparing the high-transmittance temperature-controllable magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase-change coating according to claim 1, characterized in that: In step 4), the thermochromic microcapsule emulsion is spin-coated on the surface of the substrate covered with the magnesium-doped vanadium dioxide phase change coating, cured and dried at 50-70°C for 10-30 minutes, and left at room temperature for 2 hours to obtain a high-transmittance temperature-controlled magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase change coating.
8. The method for preparing the high-transmittance temperature-controllable magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase-change coating according to claim 6 or 7, characterized in that: The substrate is a glass substrate; the number of spin coating is 1 to 3 times.
9. A high-transmittance temperature-controlled magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase-change coating prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The magnesium-doped vanadium dioxide layer in the coating has a solid spherical, egg yolk-shaped or hollow spherical morphology.
10. Use of the high-transmittance temperature-controlling magnesium-doped vanadium dioxide / thermochromic microcapsule double-layer phase-change coating according to claim 9 in the preparation of a temperature-controlling coating.