Preparation method of composite binder superhard grinding wheel
Through the preparation method of composite bond superhard grinding wheels, the problem of frequent dressing of ceramic CBN grinding wheels is solved, self-sharpening grinding is achieved, costs are reduced and efficiency is improved, and the surface stability and hardness of the workpiece are ensured.
Patent Information
- Application Number
- CN202410842921.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
AI Technical Summary
Ceramic CBN grinding wheels require frequent dressing during processing, causing the production line to stagnate. The dressing cost is high and the service life is short, which affects production efficiency and costs.
Using the preparation method of composite bond superhard grinding wheel, by mixing CBN abrasive, ceramic bond and wetting agent, ball milling, shaping, sintering, impregnating resin and drying, a composite structure with low content of ceramic bond and resin is formed to avoid Diamond dressing to achieve self-sharpening grinding.
It effectively reduces the use cost and downtime of the diamond roller, improves the service life and grinding efficiency of the grinding wheel, ensures the stability of the surface roughness and hardness of the workpiece, and reduces workpiece burns.
Smart Images

Figure CN118848837A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a CBN grinding wheel, in particular to a method for preparing a composite binder superhard grinding wheel. Background Art
[0002] CBN is a new type of artificial synthetic material, its crystal structure and physical and chemical properties are similar to those of diamond, it has excellent characteristics such as super hardness, high heat resistance, corrosion resistance, high grinding performance, etc., and is widely used in the field of mechanical processing. CBN grinding wheel is an application of its grinding performance, with CBN abrasive as raw material and metal powder, resin powder, ceramic and electroplated metal as binder.
[0003] According to different bonding methods, CBN grinding wheels can be divided into resin grinding wheels, ceramic bond grinding wheels, electroplated grinding wheels, etc., and are suitable for different working occasions according to different characteristics. For example, in the prior art, ceramic CBN grinding wheels are used for grinding the end faces of engine connecting rods. The working process is roughly as follows: the CBN grinding wheel is fixed to the grinding machine, and the connecting rod workpiece is sequentially transferred to the grinding area by a conveyor belt to realize the automatic grinding of the workpiece; after the workpiece passes through the grinding area, the excess of the workpiece surface is ground, and the workpiece processed by the ceramic CBN grinding wheel has the advantages of stable size and stable roughness.
[0004] However, the ceramic CBN grinding wheel will produce abrasive loss during the processing, and needs to be dressed with a diamond roller. One dressing takes about 35-50 minutes. The production line is stagnant during the entire dressing process and needs to wait for the dressing to be completed before restarting, which seriously affects the work rhythm. At the same time, the roller used for dressing costs about 10,000-15,000 yuan, and the service life is about 6 months. According to the normal working time of a grinder, about two rollers are lost each year, which increases the production cost.
[0005] In view of the above-mentioned prior art, it is necessary to modify the preparation process of CBN grinding wheels. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a method for preparing a composite bond superhard grinding wheel, comprising the following steps:
[0007] S1. CBN abrasive mixing: CBN abrasive, ceramic binder and wetting agent are weighed in a quantitative manner according to a ratio of 100:(3.5-4.5):(5-7) by mass, and poured into a spherical ink device in sequence, and spherical ink medium is added and repeatedly ground until a uniform mixture is obtained;
[0008] S2. Mixing and molding: The ground mixed material is loaded into a preset mold for compression molding;
[0009] S3 high temperature sintering: the formed grinding wheel piece is moved into a high temperature sintering furnace to completely solidify, and then cooled to room temperature to obtain a composite grinding wheel block;
[0010] S4 impregnation resin: the sintered composite grinding wheel abrasive block is completely immersed in the resin solution, and then removed after standing for 30-50 minutes to obtain an impregnated composite abrasive block;
[0011] S5 drying: The impregnated composite abrasive block in S4 is placed in an oven for drying for 30-50 minutes;
[0012] S6. Pasting and processing: Paste the dried grinding wheel onto the substrate according to the requirements.
[0013] Furthermore, the resin is epoxy resin or phenolic resin.
[0014] Furthermore, the particle size of the CBN abrasive is between 80 / 100 and 230 / 270.
[0015] Furthermore, in step S1, the ball milling speed is 20-30 r / min, and the ball milling ratio is (1-1.2):1.
[0016] Furthermore, the base material is 45# steel.
[0017] Furthermore, the sintering process in step S3 includes heating from room temperature to 300°C for 3.5-4h and maintaining for 1.6-2h; heating from 300°C to 600°C for 3.5-4h and maintaining for 1.6-2h; heating from 600°C to 850°C and maintaining for 0.8-1h.
[0018] Furthermore, in step S2, the mixed material is pressed under the condition of 7-9 MPa.
[0019] The present invention provides a method for preparing a composite bond superhard grinding wheel, which uses a low-content ceramic bond to maintain a certain connection strength between CBN abrasives, and then enhances the overall structural strength of the grinding wheel by impregnating it in resin. During grinding, the low-content ceramic bond will continue to sharpen itself along with the CBN abrasive, and there is no need to stop the machine for trimming with diamonds; at the same time, the CBN abrasive is provided with basic connection strength by the ceramic bond, and the grinding size of the engine connecting rod end face can be controlled to an ideal size.
[0020] The present invention adopts a composite binder system, so that the grinding wheel can replace the diamond roller dressing step through its own self-sharpening during use, effectively avoiding the problems of excessive cost and low downtime efficiency of the diamond roller, thereby achieving the purpose of reducing costs and improving efficiency. The surface roughness and hardness of the workpiece processed by the composite binder superhard grinding wheel prepared by the present invention are stable, which can effectively reduce the occurrence of workpiece burns. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 It is a microscopic connection schematic diagram of CBN abrasive, resin binder and ceramic binder in the superhard grinding wheel prepared by the present invention. DETAILED DESCRIPTION
[0022] Embodiment: A method for preparing a composite bond superhard grinding wheel, characterized in that it comprises the following steps:
[0023] S1. CBN abrasive mixing: CBN abrasive, ceramic binder and wetting agent are weighed quantitatively in a ratio of 100:(3.5-4.5):(5-7) by mass, with the particle size of the CBN abrasive ranging from 80 / 100 to 230 / 270, and poured into a ball mill in sequence, and spherical graphite medium is added and repeatedly ground for at least 3 hours until a uniform mixture is obtained; wherein, the stirring speed is 20-30r / min, and the ball-to-material ratio is (1-1.2):1.
[0024] S2. Mixing and molding: The ground mixed material is loaded into a preset mold and pressed under 7-9Mpa conditions. After demolding, a mixed blank with a certain strength is obtained.
[0025] S3. High temperature sintering: Move the mixed blank after forming into a high temperature sintering furnace, heat it from room temperature to 300°C, heat it for 3.5-4h, keep it for 1.6-2h; heat it from 300°C to 600°C, heat it for 3.5-4h, keep it for 1.6-2h; heat it from 600°C to 850°C, keep it for 0.8-1h, so that the grinding wheel is completely solidified and reaches a certain hardness and strength. Then, cool the grinding wheel to room temperature to obtain a composite grinding wheel block.
[0026] S4. Impregnation with resin: completely immerse the sintered composite grinding wheel block in the resin solution, let it stand for 30 minutes and then take it out to ensure that the resin completely penetrates into the pores of the grinding wheel to obtain an impregnated composite grinding block. The resin is evenly dispersed inside the composite grinding wheel module to provide it with overall structural strength.
[0027] S5. Drying: Place the impregnated composite abrasive block in S4 in an oven at 180° C. for drying to remove excess water or solvent in the grinding wheel until the resin is completely cured, wherein the resin is an epoxy resin or a phenolic resin.
[0028] S6. Pasting: Paste the dried grinding wheel onto the substrate according to the use requirements to obtain the superhard grinding wheel, wherein the substrate is made of 45# steel.
[0029] The superhard grinding wheel prepared by the above process can be formed into Figure 1In the microstructure diagram shown, the resin is filled between the CBN abrasives and covers the surface of the ceramic binder, providing the overall structural strength of the grinding wheel; the ceramic binder is bonded to the surface of the CBN abrasive, providing a certain strength for the CBN abrasive. When the grinding wheel contacts the workpiece, the heat generated by grinding will carbonize the resin on the surface of the grinding wheel. Due to the low content of the ceramic binder, the holding force of the binder on the CBN is low. During the continuous self-sharpening process of the CBN abrasive, the ceramic binder will also self-sharpen with the CBN abrasive. In this way, it can be ensured that the grinding wheel is always in a self-sharpening state during the grinding process, thereby completing the grinding process.
[0030] The superhard grinding wheel prepared in the embodiment is installed on a machine tool to carry out an engine connecting rod end face grinding test, and the workpiece is fixedly installed on the processing machine tool and passes through the grinding area at a speed of 0.1m / s. The roughness requirement of the workpiece is Rz2-10, the size requirement is 21±0.03, and the hardness requirement of the workpiece is HB280-320.
[0031] The obtained grinding results are as follows:
[0032]
[0033] From the data in the table above, we can see that the grinding wheel wears out relatively quickly and has a relatively large roughness in the first 10,000 pieces. This is because the abrasive surface has not formed a stable self-sharpening state in the early stage. During the processing of 10,000 to 200,000 workpieces, both the abrasive wear and the workpiece roughness are stable, and good self-sharpening and shape retention are always maintained throughout the grinding process.
[0034] Finally, the grinding wheel provided by the embodiment can meet the life of 200,000 machining volume under the conditions of workpiece hardness HB280-320, machining size 21±0.03, and roughness Rz2-10.
[0035] Comparative Example 1: A commercially available ceramic CBN grinding wheel formula was used, with a mass ratio of CBN abrasive, ceramic binder and wetting agent of 7:2:1, and a ceramic CBN grinding wheel was prepared according to the parameters in Example 1 without the impregnation in step S4 and the drying in step S5.
[0036] The engine connecting rod end surface grinding test was carried out according to the method of the embodiment, and the results are shown in the following table:
[0037]
[0038]
[0039] As can be seen from the table above, in each grinding cycle, the edge of the abrasive surface is continuously blunted, the roughness is continuously reduced, and the hardness of the workpiece is also continuously reduced, requiring diamond roller dressing. Diamond dressing causes the loss of CBN grinding wheel, and the life of the grinding wheel of comparative example 1 is only half of that of the grinding wheel of the embodiment.
[0040] Comparative Example 2: Using the same CBN abrasive, vitrified binder and wetting agent components as in Example 1, a vitrified CBN grinding wheel was prepared according to the parameters in Example 1 without the impregnation step S4 and the drying step S5. It can be foreseen that the grinding wheel prepared in Comparative Example 2 has insufficient bonding strength compared to Comparative Example 1.
[0041] The engine connecting rod end surface grinding test was carried out according to the method of the embodiment, and the results are shown in the following table:
[0042]
[0043] It can be seen from the above table that due to the poor strength of the grinding wheel, abnormal abrasive granulation will occur, the roughness changes rapidly, and the amount of dressing each time increases, which ultimately leads to a short service life of the grinding wheel.
[0044] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A method for preparing a composite bond superhard grinding wheel, characterized in that: The following steps are involved: S1. CBN abrasive mixing: CBN abrasive, ceramic binder and wetting agent are weighed in a quantitative manner according to a ratio of 100:(3.5-4.5):(5-7) by mass, and poured into a spherical ink device in sequence, and spherical ink medium is added and repeatedly ground until a uniform mixture is obtained; S2. Mixing and molding: The ground mixed material is loaded into a preset mold for compression molding; S3 high temperature sintering: the formed grinding wheel piece is moved into a high temperature sintering furnace to completely solidify, and then cooled to room temperature to obtain a composite grinding wheel abrasive block; S4 impregnation resin: the sintered composite grinding wheel abrasive block is completely immersed in the resin solution, and then removed after standing for 30-50 minutes to obtain an impregnated composite abrasive block; S5 drying: The impregnated composite abrasive block in S4 is placed in an oven for drying for 30-50 minutes; S6. Pasting and processing: Paste the dried grinding wheel onto the substrate according to the requirements.
2. The method for preparing a composite bond superhard grinding wheel according to claim 1, characterized in that: The resin is epoxy resin or phenolic resin.
3. The method for preparing a composite bond superhard grinding wheel according to claim 1, characterized in that: The particle size of the CBN abrasive is between 80 / 100 and 230 / 270.
4. The method for preparing a composite bond superhard grinding wheel according to claim 1, characterized in that: In step S1, the ball milling speed is 20-30 r / min, and the ball milling ratio is (1-1.2):
1.
5. The method for preparing a composite bond superhard grinding wheel according to claim 1, characterized in that: The base material is 45# steel.
6. The method for preparing a composite bond superhard grinding wheel according to claim 1, characterized in that: The sintering process in step S3 includes heating from room temperature to 300°C for 3.5-4h and keeping for 1.6-2h; heating from 300°C to 600°C for 3.5-4h and keeping for 1.6-2h; heating from 600°C to 850°C and keeping for 0.8-1h.
7. The method for preparing a composite bond superhard grinding wheel according to claim 1, characterized in that: In step S2, the mixed material is pressed under the condition of 7-9 MPa.
Citation Information
Patent Citations
Vitrified bond grinding wheel and process for producing the same
CN101115583A
Flexible polishing pad
CN105690240A
Hot-pressing high-strength ceramic CBN grinding wheel for grinding aerospace titanium alloy and preparation method
CN111805442A
Composite superhard stacked abrasive and preparation method thereof
CN117720879A
Cited By
Machining process of spiral grinding wheel
CN119820492A