Phase separation pore-forming method for ultra-light and ultra-thin bio-based polyurethane waterproof moisture-permeable film
Through the humidification-coagulation-suction filtration process and spiral pattern composite technology, the problem of difficulty in forming a microporous structure of highly bio-based polyurethane materials is solved, and a bio-based polyurethane waterproof and moisture-permeable membrane with efficient waterproof and moisture-permeable performance and environmentally friendly degradable properties is achieved.
Patent Information
- Application Number
- CN202410849956.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
AI Technical Summary
Existing highly bio-based waterproof and moisture-permeable polyurethane materials are difficult to form an effective microporous structure due to the hydrophilic polyol chain segment being too long, too soft, and poor elasticity, resulting in low hydrostatic pressure and poor moisture permeability, making it difficult to meet consumer demands. Aesthetic and practical requirements for clothing.
The humidification-coagulation-suction filtration process is used to form a dense layer on the membrane surface, and at the same time build an effective microporous structure, and the fabric base fabric and the waterproof and breathable membrane are compounded through a spiral pattern dispensing roller to disperse the stress. Enhance bonding strength and avoid unevenness of rubber particles, rubber blocks and fabrics.
It prevents liquid infiltration while ensuring efficient water vapor penetration, increases hydrostatic pressure, overcomes the problems of low hydrostatic pressure and poor moisture permeability in traditional methods, and provides an environmentally friendly, degradable bio-based polyurethane waterproof and moisture-permeable membrane. .
Smart Images

Figure CN118849486A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of functional textiles, in particular to a phase separation pore-forming method for an ultra-light and ultra-thin bio-based polyurethane waterproof and breathable membrane. Background Art
[0002] Bio-based materials are environmentally friendly polymer materials made from renewable biomass (such as soybeans, corn, wheat, etc.). They have the characteristics of wide range of raw materials and green environmental protection. Nowadays, most waterproof and breathable membrane materials on the market are petroleum-based materials, which will pose a threat to the environment during their production and use. Therefore, it is urgent to develop a bio-based waterproof and breathable membrane to overcome the shortcomings of traditional petroleum-based materials, such as high energy consumption in processing and difficulty in recycling.
[0003] Nowadays, with the continuous development of social living standards and economic conditions, people have put forward higher requirements for the comfort and functionality of clothing. Waterproof and breathable fabrics have the advantages of small pore size and high porosity. The pore size can effectively block the intrusion of liquid water while allowing water vapor to pass freely. It has attracted much attention because it can effectively maintain the humidity balance of the microenvironment between the human body and clothing and significantly improve the comfort of human wearing.
[0004] Waterproof and breathable membrane is a functional membrane material with excellent water permeability and moisture permeability. It is usually compounded with natural fiber fabrics or synthetic fiber fabrics to manufacture functional clothing with unique protection and comfort, such as mountaineering suits, ski suits, assault suits, field military uniforms, chemical protection suits, shoes, socks and gloves, etc. Clothing made with waterproof and breathable membrane as the core material can block rain and snow from penetrating into the interior and prevent damage from harsh external conditions, while transmitting the sweat produced by the human body in the form of moisture, thereby ensuring the safety and comfort of the human body. Therefore, it is becoming more and more important in people's production activities and daily life.
[0005] The polyurethane porous membrane has good waterproof and breathable properties, and its elasticity is excellent. It can adapt to different bonding processes during the bonding process with the fabric. At the same time, during high-intensity outdoor sports, the fabric at the joints will be stretched to varying degrees. This film material gives the clothing good elasticity and adaptability, preventing the film from tearing during intense exercise. Therefore, the polyurethane waterproof and breathable membrane is a more preferred material. The PU membrane using phase separation pores has a simple production process, an adjustable pore structure, and low cost, which is conducive to large-scale production. So far, it has been reported to be used in the field of waterproof and breathable membranes.
[0006] In addition, traditional petroleum-based waterproof and breathable membrane materials consume a lot of energy during processing, pose a threat to the human body and the environment, are prone to produce volatile organic compounds during use, and are difficult to recycle and degrade after use. Using recycled materials, converting renewable raw materials into biopolymer materials or monomers, and then developing various products to obtain environmentally friendly functional materials is a new research and development direction. Therefore, it is urgent to develop a fully bio-based polyurethane waterproof and breathable porous membrane to achieve clean and pollution-free throughout the entire process - the solvent is recyclable and the raw materials are degradable to meet the current requirements of sustainable development.
[0007] Existing high-biobased waterproof and breathable polyurethane materials (biobased content>50%) are difficult to form an effective microporous structure due to the hydrophilic polyol chain segments that are too long, too soft, and have poor elasticity. As a result, the waterproof and breathable membranes prepared by traditional methods have low hydrostatic pressure and poor moisture permeability, making it difficult to meet consumers' requirements for clothing that is both beautiful and practical. Therefore, we adopted a humidification-solidification-filtration process to form a dense layer on the membrane surface while constructing an effective microporous structure, thereby achieving the effect of preventing liquid infiltration while ensuring efficient water vapor transmission. Summary of the invention
[0008] The purpose of the present invention is to provide a fully bio-based waterproof and breathable fabric and its preparation in order to overcome the defects of the above-mentioned prior art. The humidification-solidification-filtration process is adopted to form a dense layer on the membrane surface while constructing an effective microporous structure, thereby preventing liquid infiltration while ensuring efficient water vapor transmission. At the same time, a spiral-shaped glue-dotting roller is used to compound the fabric base cloth and the waterproof and breathable membrane, which disperses the stress and enhances the bonding strength between the two, effectively overcoming the problems of rubber particles, rubber blocks, uneven fabric, hard feel, etc.
[0009] The purpose of the present invention can be achieved by the following technical solutions:
[0010] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane comprises the following steps:
[0011] The first step is to add the solvent into the reactor, and then add the bio-based polyurethane resin solution and stir to obtain a uniform and clear mixed solution; then, add a series of additives into the reactor and stir evenly;
[0012] Step 2: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free substrate;
[0013] Step 3: The substrate coated with the liquid film is sequentially subjected to humidification and drying, coagulation bath immersion, phase separation, humidification and filtration, water washing and drying to obtain a polyurethane microporous membrane, that is, a bio-based polyurethane waterproof and breathable membrane.
[0014] Furthermore, the solvent includes ethanol and acetone.
[0015] Furthermore, the bio-based polyurethane resin solution selects a polyether aliphatic polyurethane with a biomass content greater than or equal to 50%, and selects: a bio-based polyurethane containing isosorbide polyether, wherein the isosorbide polyether accounts for 10% of the total volume of the bio-based polyurethane liquid.
[0016] Furthermore, the auxiliary agent includes a bio-based penetrant, a bio-based surfactant and a bio-based porogen, the bio-based penetrant includes fatty acid methyl ester sulfonate or alkyl betaine; the bio-based surfactant includes one or more of sarcosine lipopeptide, dodecyl glucoside, polyethyleneimine lipopolysaccharide or dodecyl polyethoxylated alcohol amine; the bio-based porogen includes one or more of walnut shell particles, bamboo fiber particles, hawthorn seed particles or koizsa apricot kernel shell particles.
[0017] Furthermore, the substrate is selected from one of non-woven fabric, spunbond fabric, release paper, kraft paper, wood pulp fabric, and cotton fabric.
[0018] Furthermore, the water spraying amount during humidification and drying is 80 to 100 mL of water per square meter, the drying temperature is 80°C-100°C, and during the coagulation bath immersion, the composition of the coagulation bath liquid is a volume ratio of non-solvent to solvent of 8:2, and the coagulation bath immersion time is 2 min to 5 min.
[0019] Furthermore, during the humidification and filtration, the amount of water sprayed is 20-30 ml of water per square meter, and the vacuum degree is controlled to be -0.01-0.05 Mpa during filtration.
[0020] Furthermore, the water washing is carried out at a water temperature of 25-40°C, and the washing time is 20min to 40min.
[0021] Furthermore, after washing, the drying temperature is 80 to 120° C., and the drying time is 10 to 20 minutes.
[0022] A bio-based polyurethane waterproof and breathable membrane phase separation pore-forming device is applied to the bio-based polyurethane waterproof and breathable membrane phase separation pore-forming method, and is sequentially arranged along the material conveying direction: a substrate unwinding component, a bio-based polyurethane resin solution coating component, a moisture spraying and drying component, a coagulation bath impregnation component, a phase separation traction roller, a water washing and filtration unit, and a winding device.
[0023] Compared with the prior art, the present invention has the following advantages and beneficial effects:
[0024] (1) The bio-based polyurethane resin solution independently synthesized by the present invention can replace traditional petroleum-based raw materials and effectively reduce carbon emissions. The solvents used are all environmentally friendly bio-based solvents extracted from natural ingredients such as plants and animals. The surfactants, penetrants and porogens used are all bio-based materials, which have the characteristics of wide sources, renewable and degradable, and are environmentally friendly membrane materials.
[0025] (3) The present invention sets a water spraying and drying device in the humidification zone, so that a dense layer with a thickness of 0.1 to 5 μm is formed on the membrane surface, thereby increasing the hydrostatic pressure and overcoming the shortcoming of low hydrostatic pressure in the traditional wet process.
[0026] (4) The present invention provides a heating rod in the coagulation tank, which can achieve precise temperature control and can also be set to a temperature gradient, thereby effectively controlling the coagulation speed, accelerating phase separation, and making it easier to obtain a thin, soft, waterproof and breathable material.
[0027] (6) The present invention provides a DMF concentration detector at the tail of the coagulation device and the water washing device, and uses a single-chip microcomputer to accurately control the electric control valve on the clean water pipe. The detection device can control the DMF concentration of the aqueous solution within the range of 15±0.5% to 20±0.5%. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a SEM image of the bio-based polyurethane waterproof and breathable membrane prepared in Example 1;
[0029] Figure 2 This is a SEM image of the bio-based polyurethane waterproof and breathable membrane prepared in Comparative Example 1;
[0030] Figure 3 This is a SEM image of the bio-based polyurethane waterproof and breathable membrane prepared in Comparative Example 2;
[0031] Figure 4 This is a SEM image of the bio-based polyurethane waterproof and breathable membrane prepared in Comparative Example 3;
[0032] Figure 5 It is a phase separation pore-forming device for a bio-based polyurethane waterproof and breathable membrane;
[0033] Reference numerals in the figures:
[0034] Substrate unwinding component B1, bio-based polyurethane resin solution coating component B2, moisture spray drying component B3, coagulation bath immersion component B4, coagulation bath heating rod B41, coagulation bath immersion tank B42, phase separation traction roller B5, water washing and filtration unit B6, humidification and suction component B61, water washing box B62, pressing roller B63, and winding device B71. DETAILED DESCRIPTION
[0035] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0036] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane comprises the following steps:
[0037] The first step is to add the solvent into the reactor, and then add the bio-based polyurethane resin solution and stir to obtain a uniform and clear mixed solution; then, add a series of additives into the reactor and stir evenly;
[0038] Step 2: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free substrate;
[0039] Step 3: The substrate coated with the liquid film is sequentially subjected to humidification and drying, coagulation bath immersion, phase separation, humidification and filtration, water washing and drying to obtain a polyurethane microporous membrane, that is, a bio-based polyurethane waterproof and breathable membrane.
[0040] In some specific embodiments, the solvent includes ethanol and acetone.
[0041] In some specific embodiments, the bio-based polyurethane resin solution selects a polyether aliphatic polyurethane with a biomass content greater than or equal to 50%, and selects: a bio-based polyurethane containing isosorbide polyether, wherein the isosorbide polyether accounts for 10% of the total volume of the bio-based polyurethane liquid, and the bio-based polyurethane resin solution accounts for 35% to 55% of the volume of the bio-based solvent.
[0042] In some specific embodiments, the auxiliary agent includes a bio-based penetrant, a bio-based surfactant and a bio-based porogen. The bio-based penetrant includes fatty acid methyl ester sulfonate or alkyl betaine, and the added content is 0.5% to 3%; the bio-based surfactant includes one or more of sarcosine lipopeptide, dodecyl glucoside, polyethyleneimine lipopolysaccharide or dodecyl polyethoxylated alcohol amine, and the added content is 3% to 12%; the bio-based porogen includes one or more of walnut shell particles, bamboo fiber particles, hawthorn seed particles or koizsa apricot shell particles.
[0043] In some specific embodiments, the substrate is selected from one of non-woven fabric, spunbond fabric, release paper, kraft paper, wood pulp fabric, and cotton fabric.
[0044] In some specific embodiments, the water spraying amount during humidification and drying is 80 to 100 mL of water per square meter, the drying temperature is 80°C-100°C, and during the coagulation bath immersion, the composition of the coagulation bath liquid is a non-solvent to solvent volume ratio of 8:2, and the coagulation bath immersion time is 2 min to 5 min.
[0045] In some specific embodiments, during the humidification and filtration, the amount of water sprayed is 20-30 ml of water per square meter, and the vacuum degree is controlled to be -0.01-0.05 MPa during filtration.
[0046] In some specific embodiments, the water washing is carried out at a water temperature of 25-40° C., and the washing time is 20 min to 40 min.
[0047] In some specific embodiments, after washing, the drying temperature is 80-120° C., and the drying time is 10 min-20 min.
[0048] A bio-based polyurethane waterproof and breathable membrane phase separation pore-forming device is applied to a bio-based polyurethane waterproof and breathable membrane phase separation pore-forming method. The device comprises: a substrate unwinding component, a bio-based polyurethane resin solution coating component, a moisture spraying and drying component, a coagulation bath impregnation component, a phase separation traction roller, and a water washing, filtration and drying unit, which are arranged in sequence along the material conveying direction.
[0049] In some specific embodiments, the bio-based polyurethane resin solution coating component B2 includes a substrate introduction bin B22 and a scraper B21 for coating arranged at the outlet of the substrate introduction bin B22. The scraper B21 is preferably a rotating circular scraper with a gap of 0.03 to 1.0 mm, which can achieve precise control of the coating thickness and take away excess resin during the coating process, thereby avoiding the problem of unstable coating caused by the accumulation of liquid flowing to both sides due to the continuous movement of the base cloth, thereby ensuring the uniformity and flatness of the bio-based polyurethane film and significantly improving the quality of the film.
[0050] In some specific embodiments, the moisture spray drying assembly B3 includes a spray head, an impact force controller and a heating device. The spray head uses an atomizing nozzle to spray moisture, and the spraying amount is 80-100 mL of water per square meter. A plurality of spray holes are provided on the spray head, and the spray holes are evenly arranged along the length direction of the spray pipe, which can realize the pre-solidification of the bio-based polyurethane resin solution, accelerate the evaporation of the bio-based polyurethane resin solution, and is conducive to the formation of a dense layer on the surface of the bio-based polyurethane film, thereby effectively increasing the hydrostatic pressure;
[0051] The drying temperature is 80℃~100℃.
[0052] In some specific embodiments, the coagulation bath immersion assembly B4 includes a coagulation bath immersion tank B42 and a coagulation bath heating rod B41 disposed at the bottom of the coagulation bath immersion tank B42. The coagulation bath immersion tank has four layers, the first layer is 15 to 20 m long, the second and third layers are 10 to 15 m long, and the last layer is 15 to 20 m long.
[0053] Among them, the coagulation bath heating rod B41 can realize the precise temperature control of the solution in the coagulation bath immersion tank, and can also set a series of temperature gradients to make the base fabric heated evenly, while accelerating the coagulation speed of the film, which is conducive to obtaining a uniformly thick and thin bio-based polyurethane film with good elasticity and breathability.
[0054] In some specific embodiments, the phase separation traction roller B5 is a pair of tension control rollers, which prevent the film from shrinking while giving the film traction, thereby ensuring the flatness and uniformity of the film surface, thereby greatly improving product quality.
[0055] In some specific embodiments, the water washing, filtration and drying unit B6 includes a humidification and suction component B61: by means of spraying and humidification in the filtration, the shortcomings of the traditional water washing method that is difficult to clean are solved, the concentration of residual DMF in the membrane is greatly reduced, and the problem of DMF residue is effectively solved to obtain a bio-based polyurethane film with stable structure and good quality;
[0056] The water washing box B62 and the pressing roller B63 arranged at the outlet of the water washing box B62: the pressing roller B63 is conducive to removing excess water from the bio-based polyurethane film, so that the final film has a very low water content, thereby improving the efficiency of subsequent drying;
[0057] Drying box B64: The drying temperature is set at 80-120°C and the drying time is set at 10-20 minutes.
[0058] In some specific embodiments, a DMF precision monitoring device B10 is provided in the coagulation bath immersion tank B42 and the water washing box B62, and the detector transmits the concentration signal to the single chip microcomputer, and the single chip microcomputer controls the electric control valve on the clean water pipe. It can realize the precise monitoring of the DMF concentration in the tank and provide a response plan in real time to ensure the stability of product quality, ensure that there is no DMF residue on the final bio-based polyurethane film after water washing, and will not affect the microscopic pore morphology in the film after drying, so as to obtain a bio-based polyurethane film with good air permeability.
[0059] In some specific embodiments, 2 to 3 tanks may be provided in the water washing box B62.
[0060] In some specific embodiments, a substrate recovery component B71 for recovering the peeled substrate is further provided on one side of the peeling roller B7.
[0061] The mechanism of the present invention is described as follows:
[0062] (1) Phase separation mechanism of polyurethane microporous membrane
[0063] Polyurethane wet film formation is a porous material with a dense surface and a porous structure inside. The method of using non-solvent induced phase formation belongs to one of the phase separation pore formation methods. Bio-based polyurethane is dissolved with solvents such as bio-based ethanol, and other additives are added to form a casting solution, which is coated on the substrate and immersed in a non-solvent solidification tank that is affinity with the solvent but not affinity with the polyurethane to solidify into a film. The solvent diffuses into the non-solvent phase through the semi-permeable membrane, and the non-solvent also diffuses and penetrates into the coating phase. As the solvent in the casting solution is extracted by the non-solvent, the polyurethane gradually solidifies, thereby forming a polyurethane microporous membrane. This method requires that the polyurethane and the solvent contained in the casting solution, and the solvent and the non-solvent are completely miscible, and the polyurethane is insoluble in the non-solvent. If the pore size distribution of these micropores is controlled within 0.1 to 1 μm (the water droplet diameter is below 3 μm, and the water molecule diameter is 0.4 nm), a film that is both breathable and waterproof and moisture permeable can be made.
[0064] (2) Regulation mechanism of surfactants during polyurethane coagulation
[0065] The purpose of adding surfactants to the casting solution of polyurethane membranes is to adjust the pore structure. The molecular structure of surfactants has a common feature. Its molecules are composed of two parts, one is solvent-philic (polar part) and the other is solvent-phobic (non-polar part). The surface activity of surfactants comes from the amphiphilic structure of surfactant molecules.
[0066] When the surfactant is dissolved in the polyurethane solution, according to the rule of "like attracts like", the polar groups make the molecules tend to enter the solvent, that is, the strongly polar solvent is friendly to the polar groups in the surfactant, while the non-polar long hydrocarbon chains try their best to prevent them from dissolving in the solvent and migrate from the inside of the solvent, tending to escape from the solvent.
[0067] When the non-solvent enters, the polarity of the non-solvent molecule is weak, which is not enough to make the polar group of the surfactant break away from the action of the solvent and combine with the non-solvent. Therefore, one end of the polar group in the surfactant extends to the solvent with stronger polarity, while the non-polar group extends to the non-solvent with weaker polarity. It is precisely because of this state of existence of the surfactant that the surfactant can change the two-way diffusion rate of the solvent and the non-solvent when the polyurethane solidifies. Different surfactants have different effects.
[0068] 1) When the dipole moment of the surfactant molecule is large, that is, the force of the polar group is stronger than that of the non-polar group, when the non-solvent enters the polyurethane solution, in addition to the force between the solvent and the non-solvent, the polar group of the surfactant also promotes the entry of the non-solvent, thereby accelerating the replacement between the non-solvent and the solvent.
[0069] 2) When the force of the non-polar groups of the surfactant is dominant, the presence of the non-polar groups hinders the entry of the non-solvent and slows down the replacement of the non-solvent and the solvent.
[0070] The following embodiments are implemented based on the above technical solution of the present invention, and provide detailed implementation methods and specific operation processes, but the protection scope of the present invention is not limited to the following embodiments.
[0071] The following are more detailed implementation cases, which further illustrate the technical solutions of the present invention and the technical effects that can be obtained.
[0072] Example 1
[0073] A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane, the specific steps are as follows:
[0074] Step 1: Add bio-based ethanol and bio-based acetone to the reactor in a ratio of 1:1, add the self-synthesized polyether-type aliphatic polyurethane resin and stir to obtain a uniform and clear mixed solution. Then, add a series of additives to the reactor, including 1% fatty acid methyl ester sulfonate, 2% sarcosine lipopeptide, and 5% walnut shell particles, and stir evenly. The proportion of each part is 60 parts of solvent, 35 parts of polyurethane resin, and 5 parts of additives.
[0075] Step 2: Use a circular scraper to scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free release paper, and control the thickness of the liquid layer between 100 μm and 200 μm, and the flatness within ±0.5%;
[0076] Step 3: passing the substrate coated with the solution layer through a humidification zone, which includes a water spraying device and a heating device, using an atomizing nozzle, with a water spraying amount of 80 mL of water per square meter and a drying temperature of 80°C;
[0077] Step 4: The substrate is placed in a coagulation bath apparatus, the temperature in the coagulation bath is maintained at 40°C, and the coagulation time is 5 minutes;
[0078] Step 5: The polyurethane microporous membrane formed by the above phase separation is passed through a spraying and suction device, with a water output of 20 mL of water per square meter, and the vacuum degree of the suction device is controlled at -0.05 MPa to remove the residual DMF solution;
[0079] Step 6: Wash the microporous membrane with water at room temperature for 20 minutes to remove residual solvent;
[0080] Step 7: Dry the washed polyurethane microporous membrane at a temperature of 100° C. for 5 minutes to remove moisture, and finally peel off and roll up the dried polyurethane microporous membrane.
[0081] Example 2
[0082] Step 1: Add bio-based ethanol and bio-based acetone to the reactor in a ratio of 1:1.5, add the self-synthesized polyether-type aliphatic polyurethane resin and stir to obtain a uniform and clear mixed solution. Then, add a series of additives to the reactor, including 0.5% fatty acid methyl ester sulfonate, 3% sarcosine lipopeptide, and 10% walnut shell particles, and stir evenly. The proportion of each part is 50 parts of solvent, 40 parts of polyurethane resin, and 10 parts of additives.
[0083] Step 2: Use a circular scraper to scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free non-woven fabric, with a liquid layer thickness of 150 μm and a flatness controlled within ±0.5%;
[0084] Step 3: passing the substrate coated with the solution layer through a humidification zone, which includes a water spraying device and a heating device, using an atomizing nozzle, with a water spraying amount of 90 mL of water per square meter and a drying temperature of 90°C;
[0085] Step 4: The substrate is placed in a coagulation bath apparatus, the temperature in the coagulation bath is maintained at 40°C, and the coagulation time is 2 minutes;
[0086] Step 5: The polyurethane microporous membrane formed by the above phase separation is passed through a spraying and suction device, with a water output of 50 mL of water per square meter, and the vacuum degree of the suction device is controlled at -0.02 MPa to remove the residual DMF solution;
[0087] Step 6: Wash the microporous membrane with water at room temperature for 30 minutes to remove residual solvent;
[0088] Step 7: Dry the washed polyurethane microporous membrane at 120°C for 2 minutes to remove moisture, and finally peel off and roll up the dried polyurethane microporous membrane.
[0089] Example 3
[0090] Step 1: Add bio-based ethanol and bio-based acetone into the reactor in a ratio of 1:3, add the self-synthesized polyether-type aliphatic polyurethane resin and stir to obtain a uniform and clear mixed solution. Then, add a series of additives into the reactor, including 2% fatty acid methyl ester sulfonate, 2% sarcosine lipopeptide, and 10% walnut shell particles, and stir evenly. The proportion of each part is 45 parts of solvent, 35 parts of polyurethane resin, and 20 parts of additives.
[0091] Step 2: Use a circular scraper to scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free wood pulp cloth, with a liquid layer thickness of 120 μm and a flatness controlled within ±0.5%;
[0092] Step 3: passing the substrate coated with the solution layer through a humidification zone, which includes a water spraying device and a heating device, using an atomizing nozzle, with a water spraying amount of 50 mL of water per square meter and a drying temperature of 80°C;
[0093] Step 4: The substrate is placed in a coagulation bath apparatus, the temperature in the coagulation bath is maintained at 50°C, and the coagulation time is 3 minutes;
[0094] Step 5: The polyurethane microporous membrane formed by the above phase separation is passed through a spraying and suction device, with a water output of 20 mL of water per square meter, and the vacuum degree of the suction device is controlled at -0.05 MPa to remove the residual DMF solution;
[0095] Step 6: Wash the microporous membrane with water at 30°C for 20 minutes to remove residual solvent;
[0096] Step 7: Dry the washed polyurethane microporous membrane at a temperature of 125° C. for 2 minutes to remove moisture, and finally peel off and roll up the dried polyurethane microporous membrane.
[0097] Example 4
[0098] Step 1: Add bio-based ethanol and bio-based acetone to the reactor in a ratio of 1:2, add the self-synthesized polyether-type aliphatic polyurethane resin and stir to obtain a uniform and clear mixed solution. Then, add a series of additives to the reactor, including 3% fatty acid methyl ester sulfonate, 3% sarcosine lipopeptide, and 5% walnut shell particles, and stir evenly. The proportion of each part is 50 parts of solvent, 45 parts of polyurethane resin, and 5 parts of additives.
[0099] Step 2: Use a round scraper to scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free kraft paper, with a liquid layer thickness of 200 μm and a flatness controlled within ±0.5%;
[0100] Step 3: passing the substrate coated with the solution layer through a humidification zone, which includes a water spraying device and a heating device, using an atomizing nozzle, with a water spraying amount of 100 mL of water per square meter and a drying temperature of 100°C;
[0101] Step 4: The substrate is placed in a coagulation bath apparatus, the temperature in the coagulation bath is maintained at 50°C, and the coagulation time is 4 minutes;
[0102] Step 5: The polyurethane microporous membrane formed by the above phase separation is passed through a spraying and suction device, with a water output of 50 mL of water per square meter, and the vacuum degree of the suction device is controlled at -0.04 MPa to remove the residual DMF solution;
[0103] Step 6: Wash the microporous membrane with water at room temperature for 30 minutes to remove residual solvent;
[0104] Step 7: Dry the washed polyurethane microporous membrane at 80°C for 5 minutes to remove moisture, and finally peel off and roll up the dried polyurethane microporous membrane.
[0105] Example 5
[0106] Step 1: Add bio-based ethanol and bio-based acetone into a reactor at a ratio of 1.2:1, add self-synthesized polyether-type aliphatic polyurethane resin and stir to obtain a uniform and clear mixed solution. Then, add a series of additives into the reactor, including 0.5% fatty acid methyl ester sulfonate, 2% sarcosine lipopeptide, and 8% walnut shell particles, and stir evenly. The proportion of each part is 55 parts of solvent, 40 parts of polyurethane resin, and 5 parts of additives.
[0107] Step 2: Use a round scraper to scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free nylon cloth, with a liquid layer thickness of 150 μm and a flatness controlled within ±0.5%;
[0108] Step 3: passing the substrate coated with the solution layer through a humidification zone, which includes a water spraying device and a heating device, using an atomizing nozzle, with a water spraying amount of 80 mL of water per square meter and a drying temperature of 90°C;
[0109] Step 4: The substrate is placed in a coagulation bath apparatus, the temperature in the coagulation bath is maintained at 60°C, and the coagulation time is 3 minutes;
[0110] Step 5: The polyurethane microporous membrane formed by the above phase separation is passed through a spraying and suction device, with a water output of 40 mL of water per square meter, and the vacuum degree of the suction device is controlled at -0.05 MPa to remove the residual DMF solution;
[0111] Step 6: Wash the microporous membrane with water at 30°C for 20 minutes to remove residual solvent;
[0112] Step 7: Dry the washed polyurethane microporous membrane at a temperature of 100° C. for 3 minutes to remove moisture, and finally peel off and roll up the dried polyurethane microporous membrane.
[0113] Example 6
[0114] Step 1: Add bio-based ethanol and bio-based acetone into a reactor at a ratio of 2:1, add the self-synthesized polyether-type aliphatic polyurethane resin and stir to obtain a uniform and clear mixed solution. Then, add a series of additives into the reactor, including 2% fatty acid methyl ester sulfonate, 2% sarcosine lipopeptide, and 12% walnut shell particles, and stir evenly. The proportion of each part is 50 parts of solvent, 40 parts of polyurethane resin, and 10 parts of additives.
[0115] Step 2: Use a round scraper to scrape the mixed solution in the above reaction kettle onto a flat, clean, water-free cotton cloth, and control the thickness of the liquid layer to be between 200 μm and the flatness to be within ±0.5%;
[0116] Step 3: passing the substrate coated with the solution layer through a humidification zone, which includes a water spraying device and a heating device, using an atomizing nozzle, with a water spraying amount of 90 mL of water per square meter and a drying temperature of 80°C;
[0117] Step 4: The substrate is placed in a coagulation bath apparatus, the temperature in the coagulation bath is maintained at 40°C, and the coagulation time is 5 minutes;
[0118] Step 5: The polyurethane microporous membrane formed by the above phase separation is passed through a spraying and suction device, with a water output of 40 mL of water per square meter, and the vacuum degree of the suction device is controlled at -0.02 MPa to remove the residual DMF solution;
[0119] Step 6: Wash the microporous membrane with water at 40° C. for 10 minutes to remove residual solvent;
[0120] Step 7: Dry the washed polyurethane microporous membrane at a temperature of 100° C. for 5 minutes to remove moisture, and finally peel off and roll up the dried polyurethane microporous membrane.
[0121] Example 7
[0122] A bio-based polyurethane waterproof and breathable membrane phase separation pore forming device is applied to the bio-based polyurethane waterproof and breathable membrane phase separation pore forming method of the above-mentioned embodiments 1-6, such as Figure 5 As shown, including:
[0123] Substrate unwinding component B1, bio-based polyurethane resin solution coating component B2, moisture spray drying component B3, coagulation bath immersion component B4, phase separation traction roller B5, water washing and filtration unit B6, winding device B71.
[0124] In this embodiment, the speed of the substrate unwinding assembly B1 is controlled at 15 m / min.
[0125] In this embodiment, the bio-based polyurethane resin solution coating assembly B2 includes a substrate introduction bin B22 and a coating scraper B21 provided at the outlet of the substrate introduction bin B22. The scraper B21 is a rotating circular scraper with a gap of 0.06 mm.
[0126] In this embodiment, the moisture spraying and drying component B3 uses an atomizing nozzle to spray moisture, spraying 100 mL / min of water on the membrane surface, and the drying temperature is set to 80°C to 100°C.
[0127] In this embodiment, the coagulation bath immersion assembly B4 includes a coagulation bath immersion tank B42 and a coagulation bath heating rod B41 disposed at the bottom of the coagulation bath immersion tank B42. The coagulation bath immersion tank has four layers, the first layer is 20m long, the second and third layers are 15m long, and the last layer is 20m long.
[0128] The coagulation bath heating rod B41 is set at an interval of 0.3m, and the temperature adjustable range is set to 40℃.
[0129] The composition of the coagulation bath in the coagulation bath immersion tank is a volume ratio of non-solvent water to solvent DMF of 8:2.
[0130] In this embodiment, the phase separation traction roller B5 is a pair of tension control rollers, which transport the bio-based polyurethane film to the water washing, filtration and drying unit B6.
[0131] In this embodiment, the water washing and filtration unit B6 sprays 20-30 ml of water per square meter during humidification and filtration, and the vacuum degree is controlled to be -0.01-0.05 MPa during filtration to remove the DMF solution remaining on the membrane surface. The temperature during water washing is room temperature or not more than 40°C, and the washing time is set to 20min~40min. The excess water is removed by the pressing roller B63 at the outlet of the washing box B62 and then dried. After drying, it is rolled up by the winding device B71 (the thickness is 0.1 to 5μm).
[0132] Comparative Example 1
[0133] Step 1: Add bio-based ethanol and bio-based acetone into a reactor in a ratio of 3:2, add self-synthesized polyether-type aliphatic polyurethane resin and stir to obtain a uniform and clear mixed solution. Then, add a series of additives into the reactor, including 3% fatty acid methyl ester sulfonate, 3% sarcosine lipopeptide, and 10% walnut shell particles, and stir evenly. The proportion of each part is 45 parts of solvent, 35 parts of polyurethane resin, and 20 parts of additives.
[0134] Step 2: Use a round scraper to scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free nylon cloth, with a liquid layer thickness of 150 μm and a flatness controlled within ±0.5%;
[0135] Step 3: The substrate is placed in a coagulation bath apparatus, the temperature in the coagulation bath is maintained at 40°C, and the coagulation time is 5 minutes;
[0136] Step 4: The polyurethane microporous membrane formed by the above phase separation is passed through a spraying and suction device, with a water output of 20 mL of water per square meter, and the vacuum degree of the suction device is controlled at -0.03 MPa- to remove the residual DMF solution;
[0137] Step 5: Wash the microporous membrane with water at 40° C. for 15 minutes to remove residual solvent;
[0138] Step 6: Dry the washed polyurethane microporous membrane at 80°C for 5 minutes to remove moisture, and finally peel off and roll up the dried polyurethane microporous membrane.
[0139] Comparative Example 2
[0140] Step 1: Add bio-based ethanol and bio-based acetone into the reactor in a ratio of 3:1, add the self-synthesized polyether-type aliphatic polyurethane resin and stir to obtain a uniform and clear mixed solution. Then, add a series of additives into the reactor, including 0.5% fatty acid methyl ester sulfonate, 1% sarcosine lipopeptide, and 12% walnut shell particles, and stir evenly. The proportion of each part is 40 parts of solvent, 40 parts of polyurethane resin, and 20 parts of additives.
[0141] Step 2: Use a circular scraper to scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free spunbond fabric, with a liquid layer thickness of 200 μm and a flatness controlled within ±0.5%;
[0142] Step 3: passing the substrate coated with the solution layer through a humidification zone, which includes a water spraying device and a heating device, using an atomizing nozzle, with a water spraying amount of 100 mL of water per square meter and a drying temperature of 100°C;
[0143] Step 4: The substrate is placed in a coagulation bath device, the temperature in the coagulation bath is maintained at room temperature, and the coagulation time is 5 minutes;
[0144] Step 5: The polyurethane microporous membrane formed by the above phase separation is passed through a spraying and suction device, with a water output of 50 mL of water per square meter, and the vacuum degree of the suction device is controlled at -0.03 MPa to remove the residual DMF solution;
[0145] Step 6: Wash the microporous membrane with water at room temperature for 30 minutes to remove residual solvent;
[0146] Step 7: Dry the washed polyurethane microporous membrane at 80°C for 5 minutes to remove moisture, and finally peel off and roll up the dried polyurethane microporous membrane.
[0147] Comparative Example 3
[0148] Step 1: Add bio-based ethanol and bio-based acetone to the reactor in a ratio of 1:1, add the self-synthesized polyether-type aliphatic polyurethane resin and stir to obtain a uniform and clear mixed solution. Then, add a series of additives to the reactor, including 0.5% fatty acid methyl ester sulfonate, 1% sarcosine lipopeptide, and 5% walnut shell particles, and stir evenly. The proportion of each part is 60 parts of solvent, 35 parts of polyurethane resin, and 5 parts of additives.
[0149] Step 2: Use a round scraper to scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free release paper, with a liquid layer thickness of 100 μm and a flatness controlled within ±5%;
[0150] Step 3: The substrate is placed in a coagulation bath apparatus, the temperature in the coagulation bath is maintained at 40°C, and the coagulation time is 5 minutes;
[0151] Step 4: passing the polyurethane microporous membrane formed by the above phase separation through a spraying device, spraying water at a rate of 20 mL of water per square meter;
[0152] Step 5: Wash the microporous membrane with water at room temperature for 20 minutes to remove residual solvent;
[0153] Step 6: Dry the washed polyurethane microporous membrane at a temperature of 150° C. for 2 minutes to remove moisture, and finally peel off and roll up the dried polyurethane microporous membrane.
[0154] The following table is a performance characterization table of Examples 1-6 and Comparative Examples 1-3
[0155]
[0156]
[0157] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A phase separation pore forming method for a bio-based polyurethane waterproof and breathable membrane, characterized in that: The following steps are involved: The first step is to add the solvent into the reactor, and then add the bio-based polyurethane resin solution and stir to obtain a uniform and clear mixed solution; then, add a series of additives into the reactor and stir evenly; Step 2: Scrape the mixed solution in the above reaction kettle onto a flat, clean and water-free substrate; Step 3: The substrate coated with the liquid film is sequentially subjected to humidification and drying, coagulation bath immersion, phase separation, humidification and filtration, water washing and drying to obtain a polyurethane microporous membrane, that is, a bio-based polyurethane waterproof and breathable membrane.
2. The phase separation pore forming method of the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: The solvents include ethanol and acetone.
3. The phase separation pore forming method of the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: The bio-based polyurethane resin solution is a polyether-type aliphatic polyurethane having a biomass content greater than or equal to 50%, and is selected as: a bio-based polyurethane containing isosorbide polyether, wherein the isosorbide polyether accounts for 10% of the total volume of the bio-based polyurethane liquid.
4. The phase separation pore forming method of the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: The auxiliary agent includes a bio-based penetrant, a bio-based surfactant and a bio-based porogen. The bio-based penetrant includes fatty acid methyl ester sulfonate or alkyl betaine; the bio-based surfactant includes one or more of sarcosine lipopeptide, dodecyl glucoside, polyethyleneimine lipopolysaccharide or dodecyl polyethoxy alcoholamine; the bio-based porogen includes one or more of walnut shell particles, bamboo fiber particles, hawthorn seed particles or koizsa apricot kernel shell particles.
5. The phase separation pore forming method of the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: The substrate is selected from one of non-woven fabric, spunbond fabric, release paper, kraft paper, wood pulp fabric, and cotton fabric.
6. The phase separation pore forming method of the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: The water spraying amount during humidification and drying is 80-100 mL of water per square meter, the drying temperature is 80°C-100°C, and during the coagulation bath immersion, the composition of the coagulation bath liquid is a volume ratio of non-solvent to solvent of 8:2, and the coagulation bath immersion time is 2min-5min.
7. The phase separation pore forming method of the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: During the humidification and filtration, the amount of water sprayed is 20-30 ml per square meter, and the vacuum degree is controlled to be -0.01-0.05 Mpa during filtration.
8. The phase separation pore forming method of the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: The water washing is carried out at a water temperature of 25-40°C and the washing time is 20min to 40min.
9. The phase separation pore forming method of the bio-based polyurethane waterproof and breathable membrane according to claim 1, characterized in that: After washing, the drying temperature is between 80 and 120°C, and the drying time is between 10 and 20 minutes.
10. A phase separation pore-forming device for a bio-based polyurethane waterproof and breathable membrane, characterized in that: The method for phase separation and pore formation of a bio-based polyurethane waterproof and breathable membrane as described in any one of claims 1 to 9 is characterized in that the following are arranged in sequence along the material conveying direction: a substrate unwinding component (B1), a bio-based polyurethane resin solution coating component (B2), a moisture spraying and drying component (B3), a coagulation bath immersion component (B4), a phase separation traction roller (B5), a water washing and filtration unit (B6), and a winding device (B71).