Iron phosphate composite material as well as preparation method and application thereof
By introducing titanium elements and nitrogen-carbon quantum dots into lithium iron phosphate battery materials, a three-dimensional spherical structure is prepared, which solves the problems of low lithium ion diffusion rate and poor conductivity, and significantly improves the specific capacity and electrochemistry of lithium iron phosphate cathode materials. performance, improving the overall performance of lithium batteries.
Patent Information
- Application Number
- CN202410860386.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-28
AI Technical Summary
Existing lithium iron phosphate battery materials have low lithium ion diffusion rate and poor conductivity, resulting in short cycle life and poor electrical performance, and conventional preparation methods lead to problems such as limited lithium ion diffusion and reduced specific capacity.
A titanium-doped iron phosphate composite material is used, combined with nitrogen-carbon quantum dots, to prepare a three-dimensional flower ball-shaped iron phosphate material through hydrothermal reaction and co-precipitation method to improve lithium ion diffusion and conductivity.
The specific capacity and electrochemical performance of the lithium iron phosphate cathode material are significantly improved. The charge and discharge capacity of the lithium battery reaches 156.6mAh/g and 149.7mAh/g at 0.1C and 0.5C, and the first charge and discharge efficiency can reach up to 97.45%. Improved the overall performance of lithium batteries.
Smart Images

Figure CN118851118A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery materials, and in particular relates to an iron phosphate composite material and a preparation method and application thereof. Background Art
[0002] As a new type of high-energy battery, lithium power batteries have been widely used in the field of electric vehicles. The main types include ternary lithium batteries and lithium iron phosphate batteries. Compared with ternary lithium batteries, lithium iron phosphate batteries with olivine crystal configuration have high safety, long cycle life, low price and environmental protection characteristics, and have become the most promising lithium battery positive electrode materials; however, due to its structural characteristics, lithium ions can only diffuse in one-dimensional channels, which leads to low lithium ion diffusion rate and poor conductivity of lithium iron phosphate materials (LiFePO4), and limits the further commercial application of this positive electrode material. Iron phosphate (FePO4) is an important precursor for the preparation of lithium iron phosphate, and the changes in its microstructure and chemical composition directly affect the performance of LiFePO4 materials. In the process of improving the defects of iron phosphate positive electrode materials, although carbon coating can improve the conductivity of the material to a certain extent, it is difficult to fundamentally solve the problem of poor conductivity, and it will also lead to a decrease in the specific capacity of the battery. Iron phosphate particles produced by conventional preparation methods such as co-precipitation and high-temperature solid-phase method mostly have problems of severe agglomeration, large particle size and small specific surface area, which limits the diffusion and transfer of lithium ions and affects the electrical properties of lithium batteries.
[0003] Therefore, how to improve the conductivity of lithium iron phosphate while reducing the impact on its specific capacity has become a technical problem that needs to be solved urgently; and developing a simple and reliable modification method to produce iron phosphate with stable physical and chemical properties is of great significance for obtaining lithium iron phosphate positive electrode materials with excellent performance. Summary of the invention
[0004] In view of the problems existing in the prior art, the object of the present invention is to provide an iron phosphate composite material and a preparation method and application thereof, aiming to increase the specific capacity of lithium iron phosphate positive electrode materials and enhance the overall electrochemical performance of lithium batteries.
[0005] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides an iron phosphate composite material, the iron phosphate composite material comprising titanium-doped iron phosphate and nitrogen-carbon quantum dots;
[0007] The iron phosphate composite material has a three-dimensional flower ball morphology.
[0008] In an optional embodiment, the specific surface area of the iron phosphate composite material is 7m 2 / g-10m 2 / g;
[0009] In an optional embodiment, the content of titanium in the iron phosphate composite material is 5.0%-8.5%. ;
[0010] In an optional embodiment, the average particle size of the nitrogen-carbon quantum dots is 5.5 nm-9.0 nm.
[0011] In the iron phosphate composite material prepared by the present invention, the construction of a three-dimensional flower ball-like structure, the doping of nitrogen-carbon quantum dots and a small amount of titanium element are beneficial to synergistically promote the rapid diffusion of lithium ions and electrolytes, increase the specific capacity of lithium iron phosphate positive electrode materials and enhance the overall electrochemical performance of lithium batteries.
[0012] In a second aspect, the present invention provides a method for preparing an iron phosphate composite material, the preparation method comprising the following steps:
[0013] (1) mixing trivalent iron salt, two-dimensional titanium carbide multilayer nanosheets and nitrogen-carbon quantum dots in water to obtain a suspension, and performing a hydrothermal reaction to obtain a flower ball-shaped framework precursor material;
[0014] (2) dispersing the three-dimensional flower ball-shaped framework precursor material into water and mixing it with a phosphorus source to perform a coprecipitation reaction to obtain a flower ball-shaped hydrated iron phosphate material;
[0015] (3) sintering the hydrated iron phosphate material to obtain a titanium-doped anhydrous iron phosphate material;
[0016] (4) The titanium-doped anhydrous iron phosphate material is immersed in an acid solution to obtain an iron phosphate composite material.
[0017] The present invention first uses titanium aluminum carbide (Ti3AlC2) as a precursor and obtains two-dimensional titanium carbide (Ti3C2T x ) multilayer nanosheets, dissolving trivalent iron salt in water and mixing with the above nanosheets, the trivalent iron ions intercalate the negatively charged titanium carbide nanosheets under electrostatic force, thereby expanding the interlayer spacing to realize the exfoliation of the nanosheets to form a few-layer titanium carbide nanosheets, and at the same time, the trivalent iron ions adhere to the surface of the few-layer titanium carbide nanosheets; adding nitrogen-carbon quantum dots (NCQD) to the above mixed solution, stirring evenly, and self-assembling at high temperature and high pressure to generate a framework precursor material with a three-dimensional flower ball structure by a hydrothermal method; then, mixing the above framework precursor material with a phosphate solution, adjusting the pH of the solution, and using a coprecipitation method to make iron phosphate particles grow in situ on the surface of the titanium carbide sheet that constitutes the flower ball shape to obtain an iron phosphate material, and after the reaction is completed, the flower ball-shaped hydrated iron phosphate material is first placed in a muffle furnace for high-temperature calcination, and then the calcined crude product is placed in an acid solution for immersion to dissolve excess titanium elements, to obtain a titanium-doped iron phosphate / nitrogen-carbon quantum dot material, that is, an iron phosphate composite material.
[0018] Titanium carbide (Ti3C2T x ) The multilayer nanosheets serve as a doped titanium source on the one hand, and on the other hand, they self-assemble into a three-dimensional flower-ball-like structure with iron ions in the presence of nitrogen-carbon quantum dots (NCQDs), and serve as a template for the generation of iron phosphate particles. After subsequent high-temperature sintering, both iron phosphate and lithium iron phosphate can inherit the three-dimensional flower-ball-like morphology of the precursor material. The large specific surface area of this structure is conducive to the migration and transmission of lithium ions.
[0019] In an optional embodiment, the mass ratio of the trivalent iron salt to the two-dimensional titanium carbide multilayer nanosheets in step (1) is 1:(1-1.5), for example, it can be 1:1, 1:1.1, 1:1.2, 1:1.3, 1:1.4 or 1:1.5, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0020] In an optional embodiment, the nitrogen-carbon quantum dots (NCQD) in step (1) is a nitrogen-carbon quantum dot dispersion with a mass concentration of 2 mg / mL, and the solid-liquid ratio of the trivalent iron salt to the nitrogen-carbon quantum dot dispersion is 1 g:(5-12) mL, for example, it can be 1g:5 mL, 1g:6 mL, 1g:7 mL, 1g:8 mL, 1g:9 mL, 1g:10 mL, 1g:11 mL or 1g:12 mL, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0021] In an optional embodiment, the temperature of the hydrothermal reaction in step (1) is 150-180°C, for example, 150°C, 155°C, 160°C, 165°C, 170°C, 175°C or 180°C, and the reaction time is 5-8h, for example, 5h, 6h, 7h or 8h, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0022] The present invention introduces nitrogen-carbon quantum dots (NCQDs) in the process of preparing the iron phosphate composite material, which can not only improve the conductivity of the positive electrode material, but also serve as an effective skeleton to support the precursor material, which is beneficial to strengthen the structure of the flower ball-shaped template agent and alleviate the structural degradation and volume change of the positive electrode material during the charge and discharge process; in addition, the nitrogen-carbon quantum dots can also serve as a partial carbon source for the subsequent high-temperature calcination to prepare the lithium iron phosphate material.
[0023] In an optional embodiment, after the mixing in step (2), the pH value of the mixed solution is adjusted to 1.5-2.2 by adding ammonia water or sodium hydroxide solution. For example, it can be 1.5, 1.6, 1.7, 1.8, 1.9, 2.0, 2.1 or 2.2, but is not limited to the listed values. Other values not listed within the above numerical range are also applicable.
[0024] In an optional embodiment, the temperature of the heating coprecipitation reaction in step (2) is 80-90°C, for example, 80°C, 82°C, 85°C, 87°C or 90°C, and the coprecipitation reaction time is 6-8h, for example, 6h, 6.5h, 7h, 7.5h or 8h, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0025] In an optional embodiment, after the coprecipitation reaction in step (2) is completed, an aging treatment is further performed, and the aging time is 3-5 hours, for example, it can be 3 hours, 3.5 hours, 4 hours, 4.5 hours or 5 hours, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0026] In an optional embodiment, the sintering temperature in step (3) is 550-750°C, for example, 550°C, 600°C, 650°C, 700°C or 750°C, and the sintering time is 4-6h, for example, 4h, 4.5h, 5h, 5.5h or 6h, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0027] In an optional embodiment, the atmosphere for the sintering treatment in step (3) includes an oxygen-containing nitrogen atmosphere, in which the volume proportion of nitrogen is 95%, and the volume proportion of oxygen is 4% to 5%, for example, it can be 4%, 4.2%, 4.4%, 4.6%, 4.8% or 5%, but is not limited to the listed values, and other unlisted values within the above numerical range are also applicable.
[0028] In an optional embodiment, the acid solution in step (4) includes hydrofluoric acid, and the molar concentration of the hydrofluoric acid solution is 0.1-0.2 mol / L, for example, it can be 0.1 mol / L, 0.12 mol / L, 0.15 mol / L, 0.18 mol / L or 0.2 mol / L, and the immersion time is 2-3 h, for example, it can be 2 h, 2.2 h, 2.5 h, 2.7 h or 3 h, but is not limited to the listed values, and other values not listed within the above numerical range are also applicable.
[0029] In an optional embodiment, the ferric iron salt includes any one of ferric chloride, ferric sulfate or ferric nitrate, or a combination of at least two of them.
[0030] In an optional embodiment, the phosphorus source includes any one of phosphoric acid, ammonium dihydrogen phosphate or diammonium hydrogen phosphate, or a combination of at least two of them.
[0031] In an optional embodiment, the molar ratio of the iron element in the ferric iron salt to the phosphorus element in the phosphorus source is 1:1.
[0032] The iron phosphate particles prepared by the present invention grow in situ on the surface of two-dimensional titanium carbide nanosheets constituting the flower ball-shaped precursor material, and the titanium dioxide formed by calcining the titanium carbide is removed by soaking in hydrofluoric acid, while part of the residual titanium element is doped into the lattice of the iron phosphate, so that the material produces internal lattice defects and inhibits its lattice distortion, which can not only reduce the de- / insertion resistance of lithium ions, but also the formed fine grains can improve the electronic / ionic conductivity of the material.
[0033] In a third aspect, the present invention provides a lithium iron phosphate positive electrode material, which is obtained by mixing and sintering the iron phosphate composite material described in the second aspect with a lithium source and a carbon source.
[0034] In a fourth aspect, the present invention provides a lithium-ion battery, wherein the lithium-ion battery comprises the lithium iron phosphate positive electrode material as described in the third aspect.
[0035] Compared with the prior art, the present invention has the following beneficial effects:
[0036] (1) The iron phosphate composite material prepared by the present invention has a three-dimensional flower-shaped structure. Compared with ordinary spherical particles, the structure has a highly open framework, which is conducive to the full exposure of active sites and the full contact between the positive electrode material and the battery electrolyte; at the same time, the material of this structure has a large specific surface area, which effectively shortens the transmission path of lithium ions and promotes its lithiation / delithiation process, thereby improving the rate performance of lithium iron phosphate batteries.
[0037] (2) The composite iron phosphate material prepared by the present invention has good performance indicators. The lithium iron phosphate positive electrode material prepared therefrom also exhibits excellent electrochemical performance after being assembled into a lithium battery. Its charge and discharge capacity at 0.1C and 0.5C can reach up to 156.6mAh / g and 149.7mAh / g respectively; the first charge and discharge efficiency can reach up to 97.45%.
[0038] Other aspects will be apparent upon reading and understanding the drawings and detailed description. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] The accompanying drawings are used to provide further understanding of the technical solution of this article and constitute a part of the specification. Together with the embodiments of the present application, they are used to explain the technical solution of this article and do not constitute a limitation on the technical solution of this article.
[0040] Figure 1 The XRD spectrum of the iron phosphate composite material prepared in Example 1 of the present invention;
[0041] Figure 2 This is the XPS spectrum of the iron phosphate composite material prepared in Example 1 of the present invention;
[0042] Figure 3This is a SEM image of the iron phosphate composite material prepared in Example 1 of the present invention;
[0043] Figure 4 This is a SEM image of the lithium iron phosphate material prepared in Example 1 of the present invention;
[0044] Figure 5 This is a TEM image of the iron phosphate composite material prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0045] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present disclosure and should not be regarded as specific limitations of the present invention.
[0046] It should be noted that, if the specific conditions are not specified in the examples, the experiments were carried out according to conventional conditions or the conditions recommended by the manufacturer. The reagents or instruments used, if the manufacturers are not specified, are all conventional products that can be purchased commercially.
[0047] The two-dimensional titanium carbide (Ti3C2T x ) The multilayer nanosheets and the nitrogen-carbon quantum dot (NCQD) dispersion are prepared by known prior art, and the preparation method comprises the following steps:
[0048] (1) 1.26 g of NaF was dissolved in a hydrochloric acid solution (100 mL, 0.3 mol / L), and 3.92 g of titanium aluminum carbide powder (Ti3AlC2) was added to the mixture after stirring evenly. The mixture was stirred at 40 °C for 24 h, and the product was washed with distilled water until the pH value of the supernatant was close to neutral. Subsequently, the product was washed with anhydrous ethanol and vacuum dried to obtain multilayer blocky titanium carbide (Ti3C2T x )(T x Refers to surface groups -F, -OH, -O). The above multilayer block Ti3C2T x The precipitate was dispersed in a dimethyl sulfoxide (DMSO) solution, stirred at room temperature for 12 h, and centrifuged to collect the precipitate; then, the precipitate was dispersed in 100 ml of deionized water, ultrasonically treated for 3 h, and centrifuged for 1 h to obtain a black supernatant, which was collected by filtration and vacuum dried to obtain two-dimensional titanium carbide (Ti3C2T x )Multilayer nanosheet powder.
[0049] (2) Dissolve 0.50 g of citric acid and 0.25 g of acrylamide in 30 mL of deionized water, mix evenly by ultrasonication, pour the solution into a 50 mL polytetrafluoroethylene-lined reactor, and heat it in an oven at 180 °C for 5 h. After the reaction is completed, filter the reaction solution with a 0.22 μm filter membrane, and then dialyze it in deionized water for 48 h with a dialysis bag (molecular weight cutoff 1000). Freeze-dry it for 24 h to obtain a light yellow carbon dot powder, namely NCQD. Finally, adjust the volume to 2 mg / mL of nitrogen-carbon quantum dot dispersion and store it in a refrigerator at 4 °C for later use.
[0050] The specific surface area of the iron phosphate composite material prepared by the method of the present invention is measured by a specific surface analyzer; the titanium content is measured by an inductively coupled plasma mass spectrometer; and the particle size of the nitrogen-carbon quantum dots is measured by a transmission electron microscope.
[0051] Example 1
[0052] This embodiment provides an iron phosphate composite material, including titanium-doped iron phosphate and nitrogen-carbon quantum dots. The specific surface area of the iron phosphate composite material is 9.3 m 2 / g; the content of titanium in the iron phosphate composite material is 7.65%; and the average particle size of the nitrogen-carbon quantum dots is 7.0nm.
[0053] This embodiment provides a method for preparing an iron phosphate composite material, the method comprising the following steps:
[0054] (1) Dissolve 0.562 g (0.001 mol) of ferric sulfate nonahydrate in 70 mL of deionized water, and then take 0.731 g of Ti3C2T x The multilayer nanosheets were added to the above solution, and after ultrasonic mixing, 4.50 mL of NCQD (2 mg / mL) dispersion was added to the above mixture. After stirring for 0.5 h, the mixture was placed in a 100 mL polytetrafluoroethylene-lined reactor and placed in an oven at 170 ° C for hydrothermal reaction for 6 h. The product was then collected by centrifugation and washed several times with deionized water and anhydrous ethanol to obtain a framework precursor material with a three-dimensional flower ball structure. Among them, the trivalent iron salt and Ti3C2T x The mass ratio of the trivalent iron salt to the NCQD dispersion is 1g:8mL.
[0055] (2) The three-dimensional flower ball-shaped framework precursor material was dispersed in 50 mL of deionized water, and then 0.132 g (0.001 mol) of diammonium hydrogen phosphate was added. After stirring evenly, ammonia water was continuously added to adjust the pH value of the mixture to 1.8, and then a coprecipitation reaction was carried out: the reaction temperature of the system was raised to 85°C and maintained in a water bath for 6 hours. After the reaction was completed, it was aged for 4 hours, and the product was collected and washed by centrifugation. After vacuum drying, a hydrated iron phosphate material with a three-dimensional flower ball-shaped structure was obtained.
[0056] (3) The hydrated iron phosphate material is placed in a muffle furnace and heated to 650° C. at a rate of 10° C. / min and sintered in an oxygen-nitrogen atmosphere for 4 h to obtain a titanium-doped anhydrous iron phosphate material.
[0057] (4) The titanium-doped anhydrous iron phosphate material is immersed in a hydrofluoric acid solution (0.15 mol / L) for 2 h to dissolve the excess titanium element, and then the product is collected and washed by centrifugation, and then vacuum-dried to obtain an iron phosphate composite material.
[0058] The XRD pattern of the iron phosphate composite material prepared in this embodiment is as follows: Figure 1 As shown in the XPS spectrum Figure 2 As shown. Figure 1 It can be seen that the titanium-doped iron phosphate composite material of Example 1 has the same characteristic peaks as the FePO4 standard card, and has no other impurity diffraction peaks, indicating that the residual titanium element is doped into the interior of the iron phosphate crystal structure and forms a continuous solid solution, and does not affect its phase structure; Figure 2 It can be seen that peaks corresponding to Fe, Li, P, and Ti elements appear in the XPS spectrum of the titanium-doped iron phosphate composite material of Example 1, further indicating that the titanium element is successfully doped into the structure of the iron phosphate.
[0059] The SEM images of the iron phosphate composite material and the lithium iron phosphate material prepared in this embodiment are as follows: Figure 3 and 4 It can be seen that both of them have three-dimensional flower ball structures.
[0060] The TEM image of the iron phosphate composite material prepared in this embodiment is as follows: Figure 5 As shown, it can be seen that the nitrogen-carbon quantum dots are evenly distributed on the iron phosphate composite material, and the average particle size is 7.0 nm.
[0061] Example 2
[0062] This embodiment provides an iron phosphate composite material, including titanium-doped iron phosphate and nitrogen-carbon quantum dots. The specific surface area of the iron phosphate composite material is 8.5 m 2 / g; the content of titanium in the iron phosphate composite material is 5.35%; and the average particle size of the nitrogen-carbon quantum dots is 6.6nm.
[0063] This embodiment provides a method for preparing an iron phosphate composite material, the method comprising the following steps:
[0064] (1) Dissolve 0.270 g (0.001 mol) of ferric chloride hexahydrate in 70 mL of deionized water, and then take 0.297 g of Ti3C2T xThe multilayer nanosheets were added to the above solution and stirred evenly. Then, 2.16 mL of NCQD (2 mg / mL) dispersion was added to the above mixture. After stirring for 0.5 h, the mixture was placed in a 100 mL polytetrafluoroethylene-lined reactor and placed in an oven at 175 ° C for hydrothermal reaction for 7 h. The product was then collected by centrifugation and washed several times with deionized water and anhydrous ethanol to obtain a framework precursor material with a three-dimensional flower ball structure. Among them, the trivalent iron salt and Ti3C2T x The mass ratio of the trivalent iron salt to the NCQD dispersion is 1g:8mL.
[0065] (2) The three-dimensional flower ball-shaped framework precursor material was dispersed in 50 mL of deionized water, and then 0.115 g (0.001 mol) of ammonium dihydrogen phosphate was added. After stirring evenly, ammonia water was continuously added to adjust the pH value of the mixture to 1.5, and then a coprecipitation reaction was carried out: the reaction temperature of the system was raised to 85°C and maintained in a water bath for 7 hours. After the reaction was completed, it was aged for 3 hours, and the product was collected and washed by centrifugation. After vacuum drying, a hydrated iron phosphate material with a three-dimensional flower ball-shaped structure was obtained.
[0066] (3) The hydrated iron phosphate material is placed in a muffle furnace and heated to 550° C. at a rate of 10° C. / min and sintered in an oxygen-nitrogen atmosphere for 6 h to obtain a titanium-doped anhydrous iron phosphate material.
[0067] (4) The titanium-doped anhydrous iron phosphate material is immersed in a hydrofluoric acid solution (0.1 mol / L) for 2 h to dissolve the excess titanium element, and then the product is collected and washed by centrifugation, and then vacuum-dried to obtain an iron phosphate composite material.
[0068] Example 3
[0069] This embodiment provides an iron phosphate composite material, including titanium-doped iron phosphate and nitrogen-carbon quantum dots. The specific surface area of the iron phosphate composite material is 9.0 m 2 / g; the content of titanium in the iron phosphate composite material is 8.28%; and the average particle size of the nitrogen-carbon quantum dots is 8.3nm.
[0070] This embodiment provides a method for preparing an iron phosphate composite material, the method comprising the following steps:
[0071] (1) 0.404 g (0.001 mol) of ferric nitrate nonahydrate was dissolved in 70 mL of deionized water, and then 0.566 g of Ti3C2T xThe multilayer nanosheets were added to the above solution, and after ultrasonic mixing, 4.04 mL of NCQD (2 mg / mL) dispersion was added to the above mixture. After stirring for 0.5 h, the mixture was placed in a 100 mL polytetrafluoroethylene-lined reactor and placed in an oven at 165 ° C for hydrothermal reaction for 8 h. The product was then collected by centrifugation and washed several times with deionized water and anhydrous ethanol to obtain a framework precursor material with a three-dimensional flower ball structure. Among them, the trivalent iron salt and Ti3C2T x The mass ratio of the trivalent iron salt to the NCQD dispersion is 1g:10mL.
[0072] (2) The three-dimensional flower ball-shaped framework precursor material was dispersed in 50 mL of deionized water, and then 0.132 g (0.001 mol) of diammonium hydrogen phosphate was added. After stirring evenly, ammonia water was continuously added to adjust the pH value of the mixture to 2.2, and then a coprecipitation reaction was performed: the reaction temperature of the system was raised to 85°C and maintained in a water bath for 8 h. After the reaction was completed, it was aged for 5 h, and the product was collected and washed by centrifugation. After vacuum drying, a hydrated iron phosphate material with a three-dimensional flower ball structure was obtained;
[0073] (3) placing the hydrated iron phosphate material in a muffle furnace and heating it to 750° C. at a rate of 10° C. / min in an oxygen-nitrogen atmosphere and sintering it for 5 h to obtain a titanium-doped anhydrous iron phosphate material;
[0074] (4) The titanium-doped anhydrous iron phosphate material is immersed in a hydrofluoric acid solution (0.2 mol / L) for 2 h to dissolve the excess titanium element, and then the product is collected and washed by centrifugation, and then vacuum-dried to obtain an iron phosphate composite material.
[0075] Example 4
[0076] This embodiment provides an iron phosphate composite material, including titanium-doped iron phosphate and nitrogen-carbon quantum dots. The specific surface area of the iron phosphate composite material is 8.4 m 2 / g; the content of titanium in the iron phosphate composite material is 5.0%; and the average particle size of the nitrogen-carbon quantum dots is 7.3nm.
[0077] This embodiment provides a method for preparing an iron phosphate composite material. The difference between the preparation method and the embodiment 1 is that the Ti3C2T x The mass of the nanosheets was 0.562 g, and the other conditions and steps were exactly the same as those in Example 1. x The mass ratio of is 1:1)
[0078] Example 5
[0079] This embodiment provides an iron phosphate composite material, including titanium-doped iron phosphate and nitrogen-carbon quantum dots. The specific surface area of the iron phosphate composite material is 8.7 m 2 / g; the content of titanium in the iron phosphate composite material is 8.50%; and the average particle size of the nitrogen-carbon quantum dots is 6.8nm.
[0080] This embodiment provides a method for preparing an iron phosphate composite material. The difference between the preparation method and the embodiment 1 is that the Ti3C2T x The mass of the nanosheets was 0.843 g, and the other conditions and steps were exactly the same as those in Example 1. x The mass ratio of is 1:1.5)
[0081] Example 6
[0082] This embodiment provides an iron phosphate composite material, including titanium-doped iron phosphate and nitrogen-carbon quantum dots. The specific surface area of the iron phosphate composite material is 7.8 m 2 / g; the content of titanium in the iron phosphate composite material is 7.61%; and the average particle size of the nitrogen-carbon quantum dots is 5.8nm.
[0083] This embodiment provides a method for preparing an iron phosphate composite material. The difference between the preparation method and Example 1 is that the volume of the NCQD dispersion is changed to 2.81 mL, and the other conditions and steps are exactly the same as those of Example 1. (The solid-liquid ratio of the trivalent iron salt to the NCQD dispersion is 1 g: 5 mL)
[0084] Example 7
[0085] This embodiment provides an iron phosphate composite material, including titanium-doped iron phosphate and nitrogen-carbon quantum dots. The specific surface area of the iron phosphate composite material is 7.6 m 2 / g; the content of titanium in the iron phosphate composite material is 7.68%; and the average particle size of the nitrogen-carbon quantum dots is 9.0nm.
[0086] This embodiment provides a method for preparing an iron phosphate composite material. The difference between the preparation method and Example 1 is that the volume of the NCQD dispersion is changed to 6.75 mL, and the other conditions and steps are exactly the same as those of Example 1. (The solid-liquid ratio of the trivalent iron salt to the NCQD dispersion is 1 g: 12 mL)
[0087] Example 8
[0088] This embodiment provides an iron phosphate composite material, including titanium-doped iron phosphate and nitrogen-carbon quantum dots. The specific surface area of the iron phosphate composite material is 8.0 m 2 / g; the content of titanium in the iron phosphate composite material is 7.64%; and the average particle size of the nitrogen-carbon quantum dots is 7.5nm.
[0089] This embodiment provides a method for preparing an iron phosphate composite material. The preparation method is different from that of Example 1 only in that the temperature of the hydrothermal reaction is changed to 150° C. and the reaction time is changed to 6 h. Other conditions and steps are exactly the same as those of Example 1.
[0090] Example 9
[0091] This embodiment provides an iron phosphate composite material, including titanium-doped iron phosphate and nitrogen-carbon quantum dots. The specific surface area of the iron phosphate composite material is 8.3 m 2 / g; the content of titanium in the iron phosphate composite material is 7.70%; and the average particle size of the nitrogen-carbon quantum dots is 7.3nm.
[0092] This embodiment provides a method for preparing an iron phosphate composite material. The preparation method is different from that of Example 1 only in that the temperature of the hydrothermal reaction is changed to 180° C. and the reaction time is changed to 6 h. Other conditions and steps are exactly the same as those of Example 1.
[0093] Comparative Example 1
[0094] Compared with Example 1, the titanium-free iron phosphate material doped with nitrogen and carbon quantum dots is directly prepared by the co-precipitation method.
[0095] This comparative example provides an iron phosphate composite material, including iron phosphate and nitrogen-carbon quantum dots. The iron phosphate composite material has a morphology of irregular particles and a specific surface area of 2.8 m 2 / g, and the average particle size of nitrogen-carbon quantum dots is 7.3nm.
[0096] This comparative example provides a method for preparing an iron phosphate composite material, the method comprising the following steps:
[0097] 0.562 g (0.001 mol) of ferric sulfate nonahydrate and 0.132 g (0.001 mol) of diammonium hydrogen phosphate were dissolved in 50 mL of deionized water, and 4.50 mL of nitrogen-carbon quantum dot (NCQD) dispersion was added to the mixed solution after stirring. Ammonia water was continuously added to adjust the pH value of the mixed solution to 1.5. Then the temperature of the reaction system was raised to 85°C and maintained for 6 hours under water bath conditions. After the reaction was completed, it was allowed to stand and age for 4 hours. The products were collected and washed with deionized water and anhydrous ethanol in turn, and vacuum dried to obtain a hydrated iron phosphate crude product. The above materials were placed in a muffle furnace and heated to 650°C at a rate of 10°C / min and sintered in an oxygen-nitrogen atmosphere for 4 hours to obtain an iron phosphate composite material.
[0098] Comparative Example 2
[0099] This comparative example provides an iron phosphate composite material, including titanium-doped iron phosphate. The iron phosphate composite material has a morphology of irregular particles and a specific surface area of 3.2 m 2 / g, and the content of titanium in the iron phosphate composite material is 7.60%.
[0100] This comparative example provides a method for preparing an iron phosphate composite material. Compared with Example 1, the method does not add nitrogen-carbon quantum dot (NCQD) dispersion to the mixed solution, and other conditions and steps are exactly the same as those in Example 1.
[0101] Comparative Example 3
[0102] Compared with Example 1, Fe 3+ For Ti3C2T x Multilayer nanosheets were intercalated to prepare NCQD-Ti3C2T x Flower-like structure material is used as a template to prepare iron phosphate material.
[0103] This comparative example provides an iron phosphate composite material, including titanium-doped iron phosphate and nitrogen-carbon quantum dots. The specific surface area of the iron phosphate composite material is 4.0 m 2 / g; the content of titanium in the iron phosphate composite material is 7.67%; and the average particle size of the nitrogen-carbon quantum dots is 7.4nm.
[0104] This comparative example provides a method for preparing an iron phosphate composite material, the method comprising the following steps:
[0105] Take 0.675g Ti3C2T xThe multilayer nanosheets and 4.50 mL of nitrogen-carbon quantum dot (NCQD) dispersion were added to 70 mL of deionized water, and after stirring, the mixture was placed in a 100 mL polytetrafluoroethylene-lined reactor and placed in an oven at 170 ° C. and heated at a constant temperature for 6 h, and then the product was collected by centrifugation and washed to obtain a framework precursor material with a three-dimensional flower ball structure; the washed material was dispersed in 50 mL of deionized water, and 0.562 g (0.001 mol) of ferric sulfate nonahydrate and 0.132 g (0.001 mol) of diammonium hydrogen phosphate were added successively, and after stirring, ammonia was continuously added dropwise to adjust the p of the mixture. The H value is 1.5, and then the temperature of the reaction system is raised to 85°C and maintained in a water bath for 6 hours. After the reaction is completed, it is allowed to stand for 4 hours, and the product is collected by centrifugation and washed, and then vacuum-dried to obtain a hydrated iron phosphate material with a three-dimensional flower ball structure; the above material is placed in a muffle furnace and the temperature is raised to 650°C at a rate of 10°C / min and sintered in an oxygen-nitrogen atmosphere for 4 hours to obtain a titanium-doped anhydrous iron phosphate material; then, the above material is placed in a hydrofluoric acid solution (0.1 mol / L) and immersed for 2 hours to dissolve excess titanium elements, and then the product is collected by centrifugation and washed, and then vacuum-dried to obtain an iron phosphate composite material.
[0106] The iron phosphate composite materials prepared in Examples 1 to 9 and Comparative Examples 1 to 3 are made into lithium iron phosphate positive electrode materials, and then the lithium iron phosphate positive electrode materials are assembled into button batteries and their electrochemical performance is evaluated, which specifically includes the following steps:
[0107] (1) Preparation of lithium iron phosphate positive electrode material
[0108] Lithium carbonate, iron phosphate composite material and glucose were dispersed in anhydrous ethanol according to the molar ratio of lithium source, iron source and carbon source of 1:1:0.05, ball milled for 3 hours until mixed evenly, with a rotation speed of 3000rpm, and then spray dried to obtain precursor powder. Subsequently, the precursor powder was heated to 400℃ at a heating rate of 8℃ / min in a high-purity argon atmosphere for 3 hours, and then heated to 700℃ for high-temperature calcination for 8 hours to obtain lithium iron phosphate positive electrode material.
[0109] (2) Preparation of button cells
[0110] The lithium iron phosphate positive electrode material, the conductive agent acetylene black and the adhesive polyvinylidene fluoride are uniformly mixed in N-methylpyrrolidone at a mass ratio of 92:4:4 to make a slurry, which is then coated on an aluminum foil and placed in a vacuum drying oven for drying. It is then pressed into a positive electrode sheet using a tablet press. The negative electrode sheet is a metal lithium sheet, the electrolyte is 1 mol / L lithium hexafluorophosphate-ethylene carbonate: dimethyl carbonate (LiPF6-EC:DMC, volume ratio of 1:1), and a polypropylene porous membrane is used as a separator. The battery is assembled in an argon glove box.
[0111] (3) Electrochemical performance test
[0112] The assembled button cell was tested for electrochemical performance in the charge and discharge voltage range of 2.5-4.5V. First, it was charged to 4.5V at a constant current, then discharged to 2.5V at a rate current. The released capacity is the discharge capacity at the rate. After the discharge, it was discharged to 2.5V at a constant current again; then the next rate test was performed. The test results are shown in Table 1.
[0113] Table 1
[0114]
[0115] As can be seen from Table 1, from Examples 1-9, the lithium iron phosphate positive electrode material prepared by the composite iron phosphate prepared by the method of the present invention is configured into a button battery, and the discharge specific capacity at 0.1C can reach more than 156.6 mAh / g, the discharge specific capacity at 0.5C can reach more than 149.7 mAh / g, and the first charge and discharge efficiency can reach more than 97.45%.
[0116] By comparing Example 1 with Examples 4-5, it can be seen that in the preparation process of the iron phosphate composite material of the present invention, the trivalent iron salt and Ti3C2T x The mass ratio of Al to Ti will affect its performance. If the mass ratio of the two is too low, the doping amount of titanium element is low, which is not conducive to the improvement of the electrical conductivity and rate performance of the positive electrode material; if the mass ratio of the two is too high, the doping amount of titanium element will increase, which will make the structure of the positive electrode material unstable and reduce the transmission efficiency of electrons and ions, thereby affecting the electrical properties of the lithium battery.
[0117] By comparing Example 1 with Example 6-7, it can be seen that in the preparation process of the iron phosphate composite material of the present invention, the solid-liquid ratio of the trivalent iron salt to the NCQD dispersion will affect its performance. If the solid-liquid ratio of the two is too low, the amount of carbon material nitrogen-carbon quantum dots (NCQD) added is too little, which makes the flower ball structure skeleton of the precursor material difficult to support, thereby affecting the subsequent generation of iron phosphate materials and is not conducive to improving the conductivity of the positive electrode material; if the solid-liquid ratio of the two is too high, the amount of NCQD added is too much, which will not only block the pore structure of the precursor material, but also occupy the active sites on the surface of the material, affecting the Fe 3+ With PO4 3+ and the formation of iron phosphate materials.
[0118] By comparing Example 1 with Examples 8-9, it can be seen that in the preparation process of the iron phosphate composite material of the present invention, the temperature of the hydrothermal reaction during the synthesis of the precursor material will affect its performance, and the construction of the three-dimensional flower-ball-like structure of the precursor material requires the high temperature and high pressure generated in the hydrothermal process as a driving force. A lower reaction temperature will affect the construction of its three-dimensional flower-ball-like structure, thereby affecting the electrical properties of the subsequently prepared lithium battery positive electrode material; and a higher reaction temperature will cause particle agglomeration to a certain extent, resulting in an increase in particle size, thereby affecting the migration and transmission of lithium ions in the positive electrode material.
[0119] By comparing Example 1 and Comparative Examples 1-2, it can be seen that the iron phosphate composite material prepared by the present invention has a three-dimensional flower-ball structure and is added with titanium and nitrogen-carbon quantum dots, while the iron phosphate materials of Comparative Examples 1-2 are all solid irregular structures. The iron phosphate of Comparative Example 1 is directly synthesized by co-precipitation method without adding titanium, and nitrogen-carbon quantum dots are not added during the synthesis of the iron phosphate of Comparative Example 2, so there is no effective skeleton to support the flower-ball structure of the precursor material, which leads to a lower specific surface area, poor conductivity and slow lithium ion diffusion rate of the two, so the electrical properties of the lithium battery positive electrode material prepared therefrom are also poor.
[0120] From the comparison between Example 1 and Comparative Example 3, it can be seen that the lithium positive electrode material prepared by the iron phosphate composite material prepared by the present invention has excellent electrical properties, while Comparative Example 3 does not use Fe in advance. 3+ For Ti3C2T x Nanosheets are intercalated to expand the interlayer spacing, so Ti3C2T x Nanosheets may stack and Fe 3+ It also cannot be evenly distributed on its surface, which affects the structure of the product to a certain extent, and thus affects the electrical properties of the lithium battery.
[0121] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.
Claims
1. An iron phosphate composite material, characterized in that: The iron phosphate composite material includes titanium-doped iron phosphate and nitrogen-carbon quantum dots; The iron phosphate composite material has a three-dimensional flower ball morphology.
2. The iron phosphate composite material according to claim 1, characterized in that: The iron phosphate composite material meets one or more of the following characteristics 1 to 3: Feature 1: The specific surface area of the iron phosphate composite material is 7m 2 / g-10m 2 / g; Feature 2: The content of titanium in the iron phosphate composite material is 5.0%-8.5%; Feature 3: The average particle size of the nitrogen-carbon quantum dots is 5.5nm-9.0nm.
3. A method for preparing the iron phosphate composite material according to any one of claims 1 to 2, characterized in that: The following steps are involved: (1) mixing trivalent iron salt, two-dimensional titanium carbide multilayer nanosheets and nitrogen-carbon quantum dots in water to obtain a suspension, and performing a hydrothermal reaction to obtain a flower ball-shaped framework precursor material; (2) dispersing the flower ball-shaped framework precursor material into water and mixing it with a phosphorus source to obtain a mixed solution, and performing a coprecipitation reaction to obtain a flower ball-shaped hydrated iron phosphate material; (3) sintering the hydrated iron phosphate material to obtain a titanium-doped anhydrous iron phosphate material; (4) The titanium-doped anhydrous iron phosphate material is immersed in an acid solution to obtain an iron phosphate composite material.
4. The preparation method according to claim 3, characterized in that: The step (1) first disperses trivalent iron salt and two-dimensional titanium carbide multilayer nanosheets in water to form a dispersion, then disperses nitrogen-carbon quantum dots in water to obtain a nitrogen-carbon quantum dot dispersion, and then mixes the two dispersions to obtain a suspension; Preferably, the mass ratio of the trivalent iron salt to the two-dimensional titanium carbide multilayer nanosheet is 1:(1-1.5); Preferably, the mass concentration of the nitrogen-carbon quantum dot dispersion is 2 mg / mL, and the solid-liquid ratio of the trivalent iron salt to the nitrogen-carbon quantum dot dispersion is 1 g: (5-12) mL; Preferably, the temperature of the hydrothermal reaction is 150-180° C., and the time of the hydrothermal reaction is 5-8 h.
5. The preparation method according to claim 3, characterized in that: In step (2), one or more of the following characteristics 1 to 3 are met: Feature 1: After the mixing, the pH value of the mixed solution is adjusted to 1.5-2.2 by adding ammonia water or sodium hydroxide solution; Feature 2: The coprecipitation reaction temperature is 80-90°C, and the coprecipitation reaction time is 6-8h; Feature 3: After the coprecipitation reaction is completed, an aging treatment is further performed, and the aging treatment time is 3-5 hours.
6. The preparation method according to claim 3, characterized in that: The sintering temperature in step (3) is 550-750°C and the sintering time is 4-6h; The atmosphere for the high temperature sintering treatment includes oxygen-containing nitrogen, in which nitrogen accounts for 95% by volume and oxygen accounts for 4% to 5% by volume.
7. The preparation method according to claim 3, characterized in that: The acid solution in step (4) includes hydrofluoric acid, the molar concentration of the hydrofluoric acid is 0.1-0.2 mol / L, and the immersion time is 2-3 hours.
8. The preparation method according to claim 3, characterized in that: The ferric iron salt includes any one of ferric chloride, ferric sulfate or ferric nitrate, or a combination of at least two thereof; The phosphorus source includes any one of phosphoric acid, ammonium dihydrogen phosphate or diammonium hydrogen phosphate, or a combination of at least two thereof; The molar ratio of the iron element in the ferric iron salt to the phosphorus element in the phosphorus source is 1:
1.
9. A lithium iron phosphate positive electrode material, characterized in that: The lithium iron phosphate positive electrode material is prepared by mixing and sintering the iron phosphate composite material according to any one of claims 1 to 2 with a lithium source and a carbon source.
10. A lithium ion battery, characterized in that: The lithium-ion battery comprises the lithium iron phosphate positive electrode material as claimed in claim 9.
Citation Information
Patent Citations
Iron phosphate and preparation method thereof
CN113912034A
Manganese sodium fluorophosphate / titanium carbide lamella-carbon quantum dot composite material as well as preparation method and application thereof
CN113991109A
Preparation method of titanium-doped graphene-coated lithium iron phosphate positive electrode material
CN115676814A
Composite lithium iron phosphate positive electrode material and preparation method and application thereof
CN116143097A
Sodium-ion battery positive electrode material and preparation method thereof, and sodium-ion battery
CN117790717A
Cited By
Titanium carbide modified high-nickel ternary material, preparation method and battery
CN121044642A