Sodium-ion battery hard carbon negative electrode material, preparation method thereof and sodium-ion battery
Through the impurity removal and acid oxidation treatment of hard carbon negative electrode materials for sodium-ion batteries, the problems of high cost and serious pollution in the existing technology have been solved, and the preparation of high-capacity and high-efficiency hard carbon negative electrode materials for sodium-ion batteries has been achieved.
Patent Information
- Application Number
- CN202410778845.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-17
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-17
AI Technical Summary
The preparation process of existing hard carbon anode materials for sodium-ion batteries suffers from high cost, serious pollution and uneven production. In particular, the long-term pyrolysis of soft carbon precursors leads to increased costs and toxic gas emissions.
After impurity removal treatment on the soft carbon precursor material, a two-stage carbonization treatment is performed in an inert atmosphere, a mixed acid solution is introduced for acid oxidation treatment, and then a heating carbonization treatment is performed to form a high-capacity hard carbon anode material.
It effectively increases the sodium storage capacity, reduces polluting gas emissions and energy consumption, reduces production costs, and improves the first Coulomb efficiency and capacity retention rate of the material.
Smart Images

Figure CN118851139A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of sodium ion batteries, and in particular to a sodium ion battery hard carbon negative electrode material and a preparation method thereof, and a sodium ion battery. Background Art
[0002] Sodium-ion batteries have become one of the emerging technologies with large-scale development potential in the field of energy storage due to the high abundance and wide distribution of sodium resources, and the cost of key elements of their electrode materials is significantly lower than that of lithium-ion batteries. Hard carbon materials as negative electrodes for sodium-ion batteries have advantages such as high specific capacity, low sodium storage potential, and wide temperature operating range, and their industrialization process is faster than that of soft carbon and layered graphene negative electrode materials. However, the precursors of hard carbon negative electrode materials for sodium-ion batteries are usually biomass and phenolic resins, which have problems such as high cost, low residual carbon rate, and poor product consistency. For this reason, a preparation method for regulating the microstructure of the carbon layer and hindering the graphitization process is proposed to produce hard carbon materials for sodium-ion batteries using soft carbon precursors.
[0003] The structural regulation of soft carbon precursors for sodium ion batteries mainly uses the oxidation method; usually, the asphalt precursor is placed in an air or oxygen atmosphere for a long time to pyrolyze, introducing more oxygen defects while twisting and basically shaping the graphitized sheet structure at a lower temperature. In the subsequent inert atmosphere carbonization process, this twisted cross-linked structure can be retained, thereby hindering the graphitization process and using the soft carbon precursor to prepare sodium ion battery hard carbon materials. However, long-term pyrolysis will increase costs, and the gases volatilized by asphalt pyrolysis are highly toxic and harmful, and the feasibility is low in actual production applications.
[0004] Therefore, the prior art still needs to be improved and developed. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a sodium ion battery hard carbon negative electrode material and a preparation method thereof, and a sodium ion battery, aiming to solve the problems of high cost and serious pollution in the existing preparation of sodium ion battery hard carbon materials using soft carbon precursors.
[0006] The technical solution of the present invention is as follows:
[0007] A method for preparing a hard carbon negative electrode material for a sodium ion battery comprises the following steps:
[0008] Performing impurity removal treatment on the soft carbon precursor material to obtain a first intermediate product;
[0009] The first intermediate product is crushed and sieved, and then placed in an inert atmosphere for two-stage carbonization treatment to obtain a second intermediate product;
[0010] mixing the second intermediate product with a mixed acid solution to obtain a third intermediate product;
[0011] The third intermediate product is placed in an inert atmosphere for heating and carbonization treatment to obtain a hard carbon negative electrode material for a sodium ion battery.
[0012] The method for preparing the hard carbon negative electrode material for a sodium ion battery, wherein the soft carbon precursor material is composed of hydrocarbons of different molecular weights and their non-metallic derivatives.
[0013] The method for preparing the hard carbon negative electrode material for a sodium ion battery, wherein the temperature of the two-stage carbonization treatment is 200°C-1000°C, the time of the two-stage carbonization treatment is 2h-8h per stage, and the heating rate of the two-stage carbonization treatment is 1°C / min-5°C / min.
[0014] The method for preparing a sodium ion battery hard carbon negative electrode material, wherein the two-stage carbonization treatment includes a first stage carbonization treatment and a second stage carbonization treatment; the temperature of the first stage carbonization treatment is 200°C-500°C; the temperature of the second stage carbonization treatment is 700°C-1000°C.
[0015] The method for preparing the hard carbon negative electrode material for a sodium ion battery, wherein the temperature of the heating carbonization treatment is 800°C-1500°C, the time of the heating carbonization treatment is 2h-6h, and the heating rate of the heating carbonization treatment is 1°C / min-2°C / min.
[0016] The method for preparing the hard carbon negative electrode material for a sodium ion battery, wherein the step of removing impurities from the soft carbon precursor material to obtain the first intermediate product comprises:
[0017] The soft carbon precursor material is alternately washed with a mixed acid solution, a mixed alkali solution and water, and the first intermediate product is obtained after vacuum drying.
[0018] The preparation method of the hard carbon negative electrode material for a sodium ion battery, wherein the mixed acid solution is a mixture of at least one of dilute sulfuric acid, dilute hydrochloric acid, nitric acid, phosphoric acid, and boric acid; the concentrations of the dilute sulfuric acid, the dilute hydrochloric acid, the nitric acid, the phosphoric acid, and the boric acid are independently 0.05 mol / L-1 mol / L.
[0019] The method for preparing the hard carbon negative electrode material for a sodium ion battery, wherein the mixed alkaline solution is one or both of sodium hydroxide and potassium hydroxide; the concentrations of the sodium hydroxide and the potassium hydroxide are independently 0.1 mol / L-0.5 mol / L.
[0020] A sodium ion battery hard carbon negative electrode material is prepared by using the preparation method of the sodium ion battery hard carbon negative electrode material.
[0021] A sodium ion battery comprises a sodium ion battery negative electrode plate, wherein the sodium ion battery negative electrode plate is composed of a negative electrode collector and an active layer arranged on one side of the negative electrode collector; the active layer is prepared by mixing the sodium ion battery hard carbon negative electrode material, a conductive agent, a binder and deionized water.
[0022] Beneficial effects: The present invention provides a sodium ion battery hard carbon negative electrode material and a preparation method thereof, and a sodium ion battery. The preparation method of the sodium ion battery hard carbon negative electrode material comprises the following steps: removing impurities from a soft carbon precursor material to obtain a first intermediate product; crushing and screening the first intermediate product, placing it in an inert atmosphere for two-stage carbonization treatment to obtain a second intermediate product; mixing the second intermediate product with a mixed acid solution to obtain a third intermediate product; placing the third intermediate product in an inert atmosphere for heating and carbonization treatment to obtain a sodium ion battery hard carbon negative electrode material. The present invention utilizes a soft carbon precursor material to be subjected to two-stage carbonization treatment, and then introduces a mixed acid solution to modify the soft carbon precursor material through acid oxidation, etc., and then heats and carbonizes the soft carbon precursor material to obtain a sodium ion battery hard carbon negative electrode material. Among them, the soft carbon precursor material that has undergone two-stage carbonization treatment has basically formed a multi-layer ordered carbon layer structure. The introduction of an oxidizing acid can disrupt its ordered carbon layer structure, introduce more oxygen functional groups and defects, effectively improve the sodium storage capacity, and form a large number of open pores at the same time. The present invention introduces oxidizing acid to replace the traditional long-term pre-oxidation process, which can reduce the emission of polluting gases in the production process, reduce energy consumption and save time costs. In the subsequent heating carbonization process, the carbon layer structure cannot be arranged in order due to the large amount of carbon-oxygen bonds formed, thereby obtaining a high-capacity hard carbon negative electrode material in the soft carbon precursor. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 A schematic diagram of a process flow of a method for preparing a hard carbon negative electrode material for a sodium ion battery according to the present invention;
[0024] Figure 2 This is a charge and discharge curve diagram of the first week of use of the hard carbon negative electrode material prepared in Example 1;
[0025] Figure 3 This is a charge and discharge curve diagram of the first week of use of the soft carbon negative electrode material prepared in Comparative Example 1;
[0026] Figure 4 It is the rate performance diagram of Example 1 and Comparative Example 1;
[0027] Figure 5 The X-ray diffraction patterns of Example 1 and Comparative Example 1;
[0028] Figure 6 The transmission electron microscope images of Example 1 and Comparative Example 1 are shown. DETAILED DESCRIPTION
[0029] The present invention provides a sodium ion battery hard carbon negative electrode material and a preparation method thereof, and a sodium ion battery. In order to make the purpose, technical solution and effect of the present invention clearer and more specific, the present invention is further described in detail below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0030] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as generally understood by those skilled in the art in the art to which the present invention belongs. It should also be understood that terms such as those defined in general dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless specifically defined as herein.
[0031] At present, the preparation of hard carbon negative electrode materials for sodium ion batteries from soft carbon precursors through structural adjustment mainly uses long-term air pyrolysis or high-purity oxygen oxidation. However, the above methods have problems such as long pyrolysis time, high energy consumption, strong toxicity and harmfulness, and low and uneven oxidation efficiency, which cannot meet the actual requirements of large-scale industrial production.
[0032] Based on this, Figure 1 The present invention provides a method for preparing a hard carbon negative electrode material for a sodium ion battery, comprising the steps of:
[0033] Step S10: performing impurity removal treatment on the soft carbon precursor material to obtain a first intermediate product;
[0034] Step S20: crushing and screening the first intermediate product, and then placing it in an inert atmosphere for two-stage carbonization treatment to obtain a second intermediate product;
[0035] Step S30: mixing the second intermediate product with a mixed acid solution to obtain a third intermediate product;
[0036] Step S40: placing the third intermediate product in an inert atmosphere for heating and carbonization treatment to obtain a hard carbon negative electrode material for a sodium ion battery.
[0037] In this embodiment, impurities in the soft carbon precursor material are first removed by impurity removal treatment to obtain a first intermediate product, and then the first intermediate product is crushed and sieved, and then subjected to a two-stage carbonization treatment in an inert atmosphere, which is conducive to the uniform growth of the carbon layer structure; the second intermediate product is then treated with a mixed acid solution to oxidize the soft carbon and insert oxygen defects, causing the carbon layer to twist and bend, breaking up the carbon layer structure, so that the carbon layer structure can be fixed into a hard carbon structure after the final heating carbonization treatment, thereby obtaining a hard carbon negative electrode material for a sodium ion battery.
[0038] Specifically, the present invention utilizes a soft carbon precursor material, after undergoing two-stage carbonization treatment, to introduce a mixed acid solution treatment, to achieve modification of the soft carbon precursor material through acid oxidation, etc., and then to obtain a sodium ion battery hard carbon negative electrode material through heating carbonization treatment. Among them, the soft carbon precursor material that has undergone two-stage carbonization treatment has basically formed a multi-layer ordered carbon layer structure. The introduction of oxidizing acid can disrupt its ordered carbon layer structure, introduce more oxygen functional groups and defects, effectively improve the sodium storage capacity, and form a large number of open pores. The present invention can reduce the emission of polluting gases in the production process, reduce energy consumption, and save time costs by introducing oxidizing acid to replace the traditional long-term pre-oxidation process. In the subsequent heating carbonization process, the carbon layer structure cannot be arranged in order due to the large number of carbon-oxygen bonds formed, thereby obtaining a high-capacity hard carbon negative electrode material in the soft carbon precursor.
[0039] In some embodiments, the soft carbon precursor material is composed of hydrocarbons of different molecular weights and non-metallic derivatives thereof, and is a dark brown complex mixture, and belongs to a solid soft carbon substrate.
[0040] In some embodiments, the soft carbon precursor material is selected from but not limited to one or more of Sinopec Donghai 70A, Sinopec Donghai 90A, Kunlun asphalt, CNOOC 36-1 heavy cross-linked asphalt, and asphalt extracted from crude oil imported from Argentina or Mexico.
[0041] It should be noted that soft carbon has no platform area but only a slope area during the charge and discharge process; hard carbon is carbon with a sodium storage platform area.
[0042] In some embodiments, the temperature of the two-stage carbonization treatment is 200°C-1000°C, the time of the two-stage carbonization treatment is 2h-8h per stage, and the heating rate of the two-stage carbonization treatment is 1°C / min-5°C / min. The first intermediate product after impurity removal is crushed and sieved and then subjected to two-stage carbonization treatment, which helps to uniformly grow the carbon layer structure.
[0043] In some embodiments, the two-stage carbonization treatment includes a first stage carbonization treatment and a second stage carbonization treatment; the temperature of the first stage carbonization treatment is 200°C-500°C; the temperature of the second stage carbonization treatment is 700°C-1000°C. The softening point of the soft carbon precursor material is between 200°C and 400°C, and it can soften when the temperature reaches 300°C, so that the carbon layer structure of the soft carbon precursor material tends to be stable, neat and uniform; 800°C is pre-carbonization, so that the structure of the soft carbon precursor material is basically finalized, and at the same time, some volatilizable or sublimable colloids are removed, so that the carbon structure is purer, which is conducive to subsequent processing.
[0044] In a preferred embodiment, the temperature of the first carbonization treatment is 400°C; the temperature of the second carbonization treatment is 900°C, the time of the two carbonization treatments is 6 hours each, and the heating rate of the two carbonization treatments is 5°C / min. Under these conditions, the first carbonization treatment can obtain a carbon layer with a stable structure, a neat and uniform structure, and then the second carbonization treatment is carried out to obtain a second intermediate product with a basically fixed structure and purity.
[0045] In some embodiments, the temperature of the heating carbonization treatment is 800°C-1500°C, the time of the heating carbonization treatment is 2h-6h, and the heating rate of the heating carbonization treatment is 1°C / min-2°C / min. The carbon layer structure of the third intermediate product obtained after the second intermediate product is treated with acid will be disassembled, and after heating carbonization treatment under this condition, the loose carbon layer can be fixed / shaped again to obtain hard carbon with a sodium storage platform, which meets the requirements of energy storage and can maintain cyclic stability.
[0046] In a preferred embodiment, the temperature of the heating carbonization treatment is 1400° C., the time of the heating carbonization treatment is 6 hours, and the heating rate of the heating carbonization treatment is 2° C. / min.
[0047] In some embodiments, the step of removing impurities from the soft carbon precursor material to obtain the first intermediate product includes: washing the soft carbon precursor material alternately with a mixed acid solution, a mixed alkali solution and water, and obtaining the first intermediate product after vacuum drying. Some substances in the soft carbon precursor material are dissolved in acid and some are dissolved in alkali, and water is interspersed to dissolve water-soluble substances. Alternating washing the soft carbon precursor material with a mixed acid solution, a mixed alkali solution and water can effectively remove impurities in the soft carbon precursor material.
[0048] In some embodiments, the mixed acid solution is a mixture of at least one of dilute sulfuric acid, dilute hydrochloric acid, nitric acid, phosphoric acid, and boric acid, but not limited thereto; the concentrations of the dilute sulfuric acid, the dilute hydrochloric acid, the nitric acid, the phosphoric acid, and the boric acid are independently 0.05 mol / L-1 mol / L. The mixed acid solution can be used to remove acid-soluble impurities in the soft carbon precursor material, and the mixed acid solution can be soluble in water. Finally, water washing can be used to remove the mixed acid solution.
[0049] In some embodiments, the mixed alkali solution is but not limited to one or both of sodium hydroxide and potassium hydroxide; the concentrations of the sodium hydroxide and potassium hydroxide are independently 0.1 mol / L-0.5 mol / L. The mixed alkali solution can be used to remove alkali-soluble impurities in the soft carbon precursor material, and the mixed alkali solution can be soluble in water. Finally, water washing can be used to remove the mixed alkali solution.
[0050] In some embodiments, when performing the impurity removal treatment, the treatment time of the mixed acid solution, the mixed alkali solution and water is 4-6 minutes each time, and the treatment is performed alternately and repeated 5-10 times.
[0051] In some embodiments, the vacuum drying temperature is 60-110° C., and the vacuum drying time is 4-24 h.
[0052] In some embodiments, in step S30, the second intermediate product is mixed with the mixed acid solution at a stirring speed of 500-1500 rpm, and the mixed solution is dried; preferably, the drying temperature is 60°C-110°C, and the drying time is 4h-24h.
[0053] In some embodiments, the inert atmosphere is selected from, but not limited to, one or more of nitrogen, argon, and helium.
[0054] In addition, the present invention also provides a sodium ion battery hard carbon negative electrode material, which is prepared using the preparation method of the sodium ion battery hard carbon negative electrode material.
[0055] In this embodiment, the hard carbon negative electrode material obtained by the preparation method introduces a mixed acid to fully oxidize the soft carbon precursor material, prevent the carbon layer from being arranged in an orderly manner during the carbonization process, and realize the conversion of the soft carbon precursor to the hard carbon negative electrode material. In addition, the hard carbon negative electrode material obtained by the preparation method has a higher first coulomb efficiency, a larger first cycle charge specific capacity, and a better capacity retention rate.
[0056] In addition, the present invention also provides a sodium ion battery, comprising a sodium ion battery negative electrode plate, the sodium ion battery negative electrode plate comprising a negative electrode current collector and an active layer disposed on one side of the negative electrode current collector; the active layer is prepared by mixing a sodium ion battery hard carbon negative electrode material, a conductive agent, a binder and deionized water.
[0057] In some embodiments, the sodium ion battery hard carbon negative electrode material is applied in a sodium ion battery, so that the sodium ion battery has a higher first coulombic efficiency, a larger first cycle charge specific capacity, and a better capacity retention rate.
[0058] In some embodiments, the hard carbon negative electrode material is used to prepare a negative electrode sheet for a sodium ion battery, comprising the steps of: taking the prepared hard carbon negative electrode material for a sodium ion battery, crushing and sieving it to a particle size of 1 to 20 μm, adding a conductive agent, a binder and deionized water, mixing and coating it on the surface of the negative electrode collector of the sodium ion battery, drying and cutting the sheet to obtain a negative electrode sheet for a sodium ion battery, wherein the negative electrode sheet for a sodium ion battery can be applied to a sodium ion half-cell.
[0059] In some embodiments, the mass ratio of the sodium ion battery hard carbon negative electrode material, the conductive agent, the binder and the deionized water is (80-90):(5-10):(2.5-5):(200-600).
[0060] In some embodiments, the negative electrode current collector of the sodium ion battery is selected from but not limited to copper foil and carbon-coated aluminum foil.
[0061] In some embodiments, the drying temperature of the sodium ion battery negative electrode plate is 90-110° C., and the drying time is 8-16 hours.
[0062] In some embodiments, the conductive agent is CLOUD super P, and the binder is CMC / SBR=1:1.
[0063] The following examples are further given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention.
[0064] Comparative Example 1
[0065] This comparative example provides a bitumen-based sodium ion battery soft carbon negative electrode material, comprising the following preparation steps:
[0066] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use mixed acid (0.5 mol / L dilute hydrochloric acid and dilute sulfuric acid), mixed alkali (0.5 mol / L sodium hydroxide and potassium hydroxide) and deionized water to wash and remove impurities 5 times alternately, and vacuum dry at 100°C for 12 hours to obtain intermediate product A.
[0067] 2) Take the intermediate product A, crush and sieve it, place it in an inert atmosphere and heat it in two stages to 400°C and 900°C, with a heating rate of about 5°C / min and a holding time of 6 hours each, to obtain the intermediate product B;
[0068] 3) The intermediate product B was taken and heated to 1400°C in an inert atmosphere at a heating rate of about 2°C / min and a holding time of 6 hours to obtain a asphalt-based sodium ion battery soft carbon negative electrode material.
[0069] Example 1
[0070] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery, and the specific steps are as follows:
[0071] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use mixed acid (0.5 mol / L dilute hydrochloric acid and dilute sulfuric acid), mixed alkali (0.5 mol / L sodium hydroxide and potassium hydroxide) and deionized water to wash and remove impurities 5 times alternately, and vacuum dry at 100°C for 12 hours to obtain intermediate product A.
[0072] 2) Take the intermediate product A, crush and sieve it, place it in an inert atmosphere and heat it in two stages to 400°C and 900°C, with a heating rate of about 5°C / min and a holding time of 6 hours each, to obtain the intermediate product B;
[0073] 3) adding 0.5 mol / L of a mixed acid of dilute hydrochloric acid and dilute sulfuric acid (50% / 50%) to the intermediate product B, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product C;
[0074] 4) Take the intermediate product C, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0075] The electrochemical performance of the obtained materials was tested according to the following method:
[0076] The sodium ion battery hard carbon negative electrode material prepared in Example 1 and the sodium ion battery soft carbon negative electrode material prepared in Comparative Example 1 were mixed with Super P and CMC SBR in a mass ratio of 80:10:5:5, and 450 μL of deionized water were added to mix into a slurry. The electrode slurry was evenly coated on the carbon-coated aluminum foil using a 100 μm four-sided preparation device, and then vacuum dried in an oven at 100 ° C for 12 hours. The electrode sheet was cut into a disc with a diameter of 12 mm using a punching machine, with metallic sodium as the counter electrode and 1 mol / L NaClO 4 DEGDME was used as electrolyte and glass fiber as separator, and a CR2016 button cell was assembled in a glove box. The button cell was subjected to constant current charge and discharge test with a current density of 20 mA g -1 , the voltage range is 3-0.005 V. The electrode materials prepared in Comparative Example 1 and Example 1 were assembled into CR 2016 button cells for electrochemical performance testing. The results are shown in Table 1.
[0077] Table 1 Electrochemical performance of Comparative Example 1 and Example 1
[0078]
[0079] By comparison in Table 1, it can be seen that the soft carbon precursor-derived sodium ion battery hard carbon negative electrode material prepared in Example 1 has a higher first coulombic efficiency, a larger first-week charging specific capacity, and a better capacity retention rate than the sodium ion battery soft carbon negative electrode of Comparative Example 1, which means that the rapid acid treatment specified in the present invention replaces the long-term pre-oxidation of the soft carbon precursor material to obtain a sodium ion battery hard carbon negative electrode material with a high specific capacity.
[0080] like Figures 2 to 6 As shown, they are charge and discharge curves, rate performance diagrams, X-ray diffraction patterns and transmission electron microscope images of the hard carbon negative electrode material prepared in Example 1 and the soft carbon negative electrode material prepared in Comparative Example 1 when used.
[0081] Figure 1 and Figure 2 The horizontal axis is the specific capacity (unit: mAh g -1 ), the ordinate is voltage (unit: V); during discharge, the voltage starts to decrease from a high potential (about 3V) and ends when it reaches 0.005V. The charging process is the opposite, starting from 0.005V and ending at 3V.
[0082] Figure 3 In the figure, the horizontal axis is the cycle number, and 10 cycles are performed at each increasing current density. The vertical axis on the left is the specific capacity (unit: mAh g -1 ), the right axis ordinate is the coulomb efficiency (unit: %). From left to right, every 10 cycles is a section, and the current density is: 10mAg -1 , 20mA g -1 , 50mAg -1 , 100mAg -1 and 20mAg -1 After the current density fluctuation and high current rapid charge and discharge, the battery is charged and discharged with a relatively small current to test the rate performance. Before and after the high current charge and discharge, the battery is charged and discharged with a 20mA g -1 When charged and discharged at a current density of , the specific capacity and coulombic efficiency of Example 1 fluctuate very little, indicating that the prepared soft carbon precursor-derived sodium ion battery hard carbon negative electrode material has good electrochemical charge and discharge rate performance.
[0083] Figure 4 In the figure, the horizontal axis is the diffraction angle (2 times the X-ray incident angle, unit: °), and the vertical axis is the intensity of the diffraction peak (unit: au). The characteristic peaks of the soft carbon precursor-derived sodium ion battery hard carbon negative electrode material prepared in Example 1 appear at 25.2° and 44°, respectively, showing broad diffraction peaks in an amorphous state, corresponding to the 002 crystal plane and 100 crystal plane of the hard carbon material, indicating that the carbonization is sufficient and the prepared hard carbon material has the characteristics of amorphous carbon.
[0084] Figure 5 The interlayer spacing (d 002 , unit: nm) is calculated by Fourier transform on the transmission electron microscope image, which is about 0.382nm. Compared with the interlayer spacing of artificial graphite of 0.335nm, the prepared hard carbon material shows a larger interlayer spacing, which can allow sodium ions to pass through and is the basis for high-capacity sodium storage. At the same time, the transmission electron microscope image also shows that the prepared hard carbon material has a high degree of disorder and a distorted lamellar structure, indicating that the introduction of oxidizing acid treatment such as dilute sulfuric acid helps to regulate the formation of a hard carbon structure from a soft carbon precursor.
[0085] Example 2
[0086] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0087] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use mixed acid (0.3 mol / L dilute hydrochloric acid and dilute sulfuric acid), mixed alkali (0.3 mol / L sodium hydroxide and potassium hydroxide) and deionized water to wash and remove impurities 5 times alternately, and vacuum dry at 100°C for 12 hours to obtain intermediate product A.
[0088] 2) Take the intermediate product A, crush and sieve it, place it in an inert atmosphere and heat it in two stages to 400°C and 900°C, with a heating rate of about 5°C / min and a holding time of 6 hours each, to obtain the intermediate product B;
[0089] 3) adding 0.3 mol / L of a mixed acid of dilute hydrochloric acid and dilute sulfuric acid (50% / 50%) to the intermediate product B, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product C;
[0090] 4) Take the intermediate product C, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0091] Example 3
[0092] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0093] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use mixed acid (0.8 mol / L dilute hydrochloric acid and dilute sulfuric acid), mixed alkali (0.8 mol / L sodium hydroxide and potassium hydroxide) and deionized water to wash and remove impurities 5 times alternately, and vacuum dry at 100°C for 12 hours to obtain intermediate product A.
[0094] 2) Take the intermediate product A, crush and sieve it, place it in an inert atmosphere and heat it in two stages to 400°C and 900°C, with a heating rate of about 5°C / min and a holding time of 6 hours each, to obtain the intermediate product B;
[0095] 3) adding 0.8 mol / L of a mixed acid of dilute hydrochloric acid and dilute sulfuric acid (50% / 50%) to the intermediate product B, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product C;
[0096] 4) Take the intermediate product C, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0097] Example 4
[0098] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0099] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use mixed acid (1 mol / L dilute hydrochloric acid and dilute sulfuric acid), mixed alkali (1 mol / L sodium hydroxide and potassium hydroxide) and deionized water to wash and remove impurities 5 times alternately, and vacuum dry at 100°C for 12h to obtain intermediate product A.
[0100] 2) Take the intermediate product A, crush and sieve it, place it in an inert atmosphere and heat it in two stages to 400°C and 900°C, with a heating rate of about 5°C / min and a holding time of 6 hours each, to obtain the intermediate product B;
[0101] 3) adding 1 mol / L of a mixed acid of dilute hydrochloric acid and dilute sulfuric acid (50% / 50%) to the intermediate product B, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product C;
[0102] 4) Take the intermediate product C, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0103] Example 5
[0104] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0105] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use mixed acid (0.5 mol / L dilute hydrochloric acid and dilute sulfuric acid), mixed alkali (0.5 mol / L sodium hydroxide and potassium hydroxide) and deionized water to wash and remove impurities 5 times alternately, and vacuum dry at 100°C for 12 hours to obtain intermediate product A.
[0106] 2) Take the intermediate product A, crush and sieve it, place it in an inert atmosphere and heat it in two stages to 400°C and 900°C, with a heating rate of about 5°C / min and a holding time of 6 hours each, to obtain the intermediate product B;
[0107] 3) adding 0.5 mol / L of a mixed acid of dilute hydrochloric acid and dilute sulfuric acid (25% / 75%) to the intermediate product B, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product C;
[0108] 4) Take the intermediate product C, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0109] Example 6
[0110] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0111] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use mixed acid (0.5 mol / L dilute hydrochloric acid and dilute sulfuric acid), mixed alkali (0.5 mol / L sodium hydroxide and potassium hydroxide) and deionized water to wash and remove impurities 5 times alternately, and vacuum dry at 100°C for 12 hours to obtain intermediate product A.
[0112] 2) Take the intermediate product A, crush and sieve it, place it in an inert atmosphere and heat it in two stages to 400°C and 900°C, with a heating rate of about 5°C / min and a holding time of 6 hours each, to obtain the intermediate product B;
[0113] 3) adding 0.5 mol / L dilute sulfuric acid to the intermediate product B, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product C;
[0114] 4) Take the intermediate product C, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0115] Example 7
[0116] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0117] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use mixed acid (0.5 mol / L dilute hydrochloric acid and dilute sulfuric acid), mixed alkali (0.5 mol / L sodium hydroxide and potassium hydroxide) and deionized water to wash and remove impurities 5 times alternately, and vacuum dry at 100°C for 12 hours to obtain intermediate product A.
[0118] 2) Take the intermediate product A, crush and sieve it, place it in an inert atmosphere and heat it in two stages to 400°C and 900°C, with a heating rate of about 5°C / min and a holding time of 6 hours each, to obtain the intermediate product B;
[0119] 3) adding 0.5 mol / L of a mixed acid of dilute hydrochloric acid and dilute sulfuric acid (75% / 25%) to the intermediate product B, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product C;
[0120] 4) Take the intermediate product C, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0121] Example 8
[0122] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0123] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use mixed acid (0.5 mol / L dilute hydrochloric acid and dilute sulfuric acid), mixed alkali (0.5 mol / L sodium hydroxide and potassium hydroxide) and deionized water to wash and remove impurities 5 times alternately, and vacuum dry at 100°C for 12 hours to obtain intermediate product A.
[0124] 2) Take the intermediate product A, crush and sieve it, place it in an inert atmosphere and heat it in two stages to 400°C and 900°C, with a heating rate of about 5°C / min and a holding time of 6 hours each, to obtain the intermediate product B;
[0125] 3) Add 0.5 mol / L dilute hydrochloric acid to the intermediate product B, stir for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinse with deionized water, and vacuum dry at 100° C. for 12 hours to obtain an intermediate product C;
[0126] 4) Take the intermediate product C, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0127] In Examples 2 to 8, the intermediate product C was treated with different acid concentrations to achieve a comparison of the acid concentration difference; the negative electrode materials prepared in Comparative Example 1 and Examples 2 to 8 were assembled into CR2016 button batteries in the manner of Example 1 for electrochemical performance testing, and the results are shown in Table 2:
[0128] Table 2 Electrochemical performance of Comparative Example 1 and Examples 2 to 8
[0129]
[0130]
[0131] Compared with Comparative Example 1, the increase in the mixed acid concentration in Examples 2 to 8 has different degrees of improvement on the first coulombic efficiency, first-cycle charge specific capacity and capacity retention rate of the hard carbon material, but the biggest impact is the improvement in specific capacity. When the ratio of the mixed acid is adjusted, the specific capacity and capacity retention rate are also greatly improved, and it is feasible to use a single acid to replace the mixed acid.
[0132] Example 9
[0133] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0134] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use deionized water to wash and remove impurities alternately 5 times, and vacuum dry at 100° C. for 12 h to obtain intermediate product A.
[0135] 2) Take the intermediate product A, crush and sieve it, place it in an inert atmosphere and heat it in two stages to 300°C and 800°C, with a heating rate of about 5°C / min and a holding time of 6 hours each, to obtain the intermediate product B;
[0136] 3) Add 0.5 mol / L dilute hydrochloric acid to the intermediate product B, stir for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinse with deionized water, and vacuum dry at 100° C. for 12 hours to obtain an intermediate product C;
[0137] 4) Take the intermediate product C, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0138] Example 10
[0139] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0140] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use deionized water to wash and remove impurities alternately 5 times, and vacuum dry at 100° C. for 12 h to obtain intermediate product A.
[0141] 2) Take the intermediate product A, crush and sieve it, place it in an inert atmosphere and heat it in two stages to 300°C and 800°C, with a heating rate of about 5°C / min and a holding time of 6 hours each, to obtain the intermediate product B;
[0142] 3) adding 0.5 mol / L dilute sulfuric acid to the intermediate product B, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product C;
[0143] 4) Take the intermediate product C, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0144] Embodiment 11
[0145] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0146] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use deionized water to wash and remove impurities alternately 5 times, and vacuum dry at 100° C. for 12 h to obtain intermediate product A.
[0147] 2) Take the intermediate product A, crush and sieve it, place it in an air atmosphere and heat it to 300°C for pre-oxidation, the heating rate is about 5°C / min, and the holding time is 6 hours to obtain the intermediate product B;
[0148] 3) taking intermediate product B, heating it to 800°C in an inert atmosphere at a heating rate of about 5°C / min and keeping it at this temperature for 6 hours to obtain intermediate product C;
[0149] 4) adding 0.5 mol / L dilute hydrochloric acid to the intermediate product C, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product D;
[0150] (5) The intermediate product D was taken and heated to 1400°C in an inert atmosphere at a heating rate of about 2°C / min for 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0151] Example 12
[0152] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0153] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use deionized water to wash and remove impurities alternately 5 times, and vacuum dry at 100° C. for 12 h to obtain intermediate product A.
[0154] 2) Take the intermediate product A, crush and sieve it, place it in an air atmosphere and heat it to 300°C for pre-oxidation, the heating rate is about 5°C / min, and the holding time is 6 hours to obtain the intermediate product B;
[0155] 3) taking intermediate product B, heating it to 800°C in an inert atmosphere at a heating rate of about 5°C / min and keeping it at this temperature for 6 hours to obtain intermediate product C;
[0156] 4) adding 0.5 mol / L dilute sulfuric acid to the intermediate product C, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product D;
[0157] 5) Take the intermediate product D, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0158] Embodiment 13
[0159] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0160] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use mixed acid (0.5 mol / L dilute hydrochloric acid and dilute sulfuric acid), mixed alkali (0.5 mol / L sodium hydroxide and potassium hydroxide) and deionized water to wash and remove impurities 5 times alternately, and vacuum dry at 100°C for 12h to obtain intermediate product A.
[0161] 2) Take the intermediate product A, crush and sieve it, place it in an air atmosphere and heat it to 300°C for pre-oxidation, the heating rate is about 5°C / min, and the holding time is 6 hours to obtain the intermediate product B;
[0162] 3) taking intermediate product B, heating it to 800°C in an inert atmosphere at a heating rate of about 5°C / min and keeping it at this temperature for 6 hours to obtain intermediate product C;
[0163] 4) adding 0.5 mol / L dilute sulfuric acid to the intermediate product C, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product D;
[0164] 5) Take the intermediate product D, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0165] Embodiment 14
[0166] This embodiment provides a method for preparing a hard carbon negative electrode material for a sodium ion battery derived from a pitch-based soft carbon, and the specific steps are as follows:
[0167] 1) Take petroleum asphalt precursor material (Sinopec Donghai brand 90A), crush and sieve, use mixed acid (0.5 mol / L dilute hydrochloric acid and dilute sulfuric acid), mixed alkali (0.5 mol / L sodium hydroxide and potassium hydroxide) and deionized water to wash and remove impurities 5 times alternately, and vacuum dry at 100°C for 12h to obtain intermediate product A.
[0168] 2) Take the intermediate product A, crush and sieve it, place it in an air atmosphere and heat it to 300°C for pre-oxidation, the heating rate is about 5°C / min, and the holding time is 6 hours to obtain the intermediate product B;
[0169] 3) taking intermediate product B, heating it to 800°C in an inert atmosphere at a heating rate of about 5°C / min and keeping it at this temperature for 6 hours to obtain intermediate product C;
[0170] 4) adding 0.5 mol / L dilute hydrochloric acid to the intermediate product C, stirring for 30-120 minutes at a stirring speed of 500-1500 rpm, then rinsing with deionized water, and vacuum drying at 100° C. for 12 hours to obtain an intermediate product D;
[0171] 5) Take the intermediate product D, place it in an inert atmosphere and heat it to 1400°C, with a heating rate of about 2°C / min and a holding time of 6 hours to obtain a pitch-based soft carbon-derived sodium ion battery hard carbon negative electrode material.
[0172] Examples 9 to 14 are comparisons of different impurity removal and carbonization processes; the negative electrode materials prepared in Comparative Example 1 and Examples 9 to 14 were assembled into CR 2016 button batteries according to the method of Example 1 for electrochemical performance testing, and the results are shown in Table 3.
[0173] Table 3 Electrochemical performance of Comparative Example 1 and Examples 9 to 14
[0174]
[0175]
[0176] Compared with Comparative Example 1, the increase in the mixed acid concentration in Examples 9 to 14 has different degrees of improvement on the first coulombic efficiency, first cycle charge specific capacity and capacity retention rate of the hard carbon material. Compared with Examples 2 to 8, reducing the impurity removal process will partially reduce the first coulombic efficiency, and introducing the pre-oxidation process will also compensate for the reduction in capacity and the attenuation of capacity retention rate on the basis of reducing impurity removal.
[0177] In summary, the present invention provides a sodium ion battery hard carbon negative electrode material and a preparation method thereof, a sodium ion battery, and a preparation method of the sodium ion battery hard carbon negative electrode material, which includes the steps of: removing impurities from a soft carbon precursor material to obtain a first intermediate product; crushing and screening the first intermediate product, placing it in an inert atmosphere for two-stage carbonization treatment to obtain a second intermediate product; mixing the second intermediate product with a mixed acid solution to obtain a third intermediate product; placing the third intermediate product in an inert atmosphere for heating and carbonization treatment to obtain a sodium ion battery hard carbon negative electrode material. The present invention utilizes a soft carbon precursor material to introduce a mixed acid solution after two-stage carbonization treatment, and achieves a modification treatment of the soft carbon precursor material through acid oxidation, etc., and then heats and carbonizes the soft carbon precursor material to obtain a sodium ion battery hard carbon negative electrode material. Among them, the soft carbon precursor material that has undergone two-stage carbonization treatment has basically formed a multi-layer ordered carbon layer structure. The introduction of an oxidizing acid can disrupt its ordered carbon layer structure, introduce more oxygen functional groups and defects, effectively improve the sodium storage capacity, and form a large number of open pores. The present invention introduces oxidizing acid to replace the traditional long-term pre-oxidation process, which can reduce the emission of polluting gases in the production process, reduce energy consumption and save time costs. In the subsequent heating carbonization process, the carbon layer structure cannot be arranged in order due to the large amount of carbon-oxygen bonds formed, thereby obtaining a high-capacity hard carbon negative electrode material in the soft carbon precursor.
[0178] It should be understood that the application of the present invention is not limited to the above examples. For ordinary technicians in this field, improvements or changes can be made based on the above description. All these improvements and changes should fall within the scope of protection of the claims attached to the present invention.
Claims
1. A method for preparing a hard carbon negative electrode material for a sodium ion battery, characterized in that: Includes steps: Performing impurity removal treatment on the soft carbon precursor material to obtain a first intermediate product; The first intermediate product is crushed and sieved, and then placed in an inert atmosphere for two-stage carbonization treatment to obtain a second intermediate product; mixing the second intermediate product with a mixed acid solution to obtain a third intermediate product; The third intermediate product is placed in an inert atmosphere for heating and carbonization treatment to obtain a hard carbon negative electrode material for a sodium ion battery.
2. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: The soft carbon precursor material consists of hydrocarbons with different molecular weights and non-metal derivatives thereof.
3. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: The temperature of the two-stage carbonization treatment is 200°C-1000°C, the time of the two-stage carbonization treatment is 2h-8h for each stage, and the heating rate of the two-stage carbonization treatment is 1°C / min-5°C / min.
4. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 3, characterized in that: The two-stage carbonization treatment includes a first stage carbonization treatment and a second stage carbonization treatment; the temperature of the first stage carbonization treatment is 200°C-500°C; the temperature of the second stage carbonization treatment is 700°C-1000°C.
5. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: The temperature of the heating carbonization treatment is 800° C.-1500° C., the time of the heating carbonization treatment is 2 h-6 h, and the heating rate of the heating carbonization treatment is 1° C. / min-2° C. / min.
6. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1, characterized in that: The step of removing impurities from the soft carbon precursor material to obtain a first intermediate product comprises: The soft carbon precursor material is alternately washed with a mixed acid solution, a mixed alkali solution and water, and the first intermediate product is obtained after vacuum drying.
7. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 1 or 6, characterized in that: The mixed acid solution is a mixture of at least one of dilute sulfuric acid, dilute hydrochloric acid, nitric acid, phosphoric acid, and boric acid; the concentrations of the dilute sulfuric acid, the dilute hydrochloric acid, the nitric acid, the phosphoric acid, and the boric acid are independently 0.05 mol / L-1 mol / L.
8. The method for preparing a hard carbon negative electrode material for a sodium ion battery according to claim 6, characterized in that: The mixed alkaline solution is one or both of sodium hydroxide and potassium hydroxide; the concentrations of the sodium hydroxide and potassium hydroxide are independently 0.1 mol / L-0.5 mol / L.
9. A hard carbon negative electrode material for a sodium ion battery, characterized in that: The material is prepared by the method for preparing a hard carbon negative electrode material for a sodium ion battery according to any one of claims 1 to 8.
10. A sodium ion battery, comprising a sodium ion battery negative electrode plate, characterized in that: The negative electrode plate of the sodium ion battery is composed of a negative electrode collector and an active layer arranged on one side of the negative electrode collector; the active layer is prepared by mixing the sodium ion battery hard carbon negative electrode material according to claim 9, a conductive agent, a binder and deionized water.
Citation Information
Patent Citations
Biomass-based sodium ion battery hard carbon negative electrode material and preparation method thereof
CN115092906A
Novel hard carbon material as well as preparation method and application thereof
CN115360348A
Sodium-ion battery hard carbon negative electrode material and preparation method thereof
CN116022769A
Mechanical surface modified biomass hard carbon material as well as preparation method and application thereof
CN116534837A
Preparation method and application of sodium ion battery hard carbon negative electrode material