Preparation method and application of flexible current collector material

By performing temperature-raising pretreatment and carbonization treatment on chitin gel, the problems of complex preparation process and poor flexibility of three-dimensional porous carbon current collectors in the existing technology are solved, and a flexible current collector material with good mechanical strength and flexibility is prepared. Meet the application needs of flexible electrodes.

CN118851141AActive Publication Date: 2024-10-29SHENZHEN POLYTECHNIC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410835862.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-29
Estimated Expiration
2044-06-26

AI Technical Summary

Technical Problem

The preparation process of existing high-performance three-dimensional porous carbon current collectors is complex, high cost, and low yield. Moreover, the final product prepared from biomass raw materials has poor mechanical strength and flexibility, which cannot meet the application needs of flexible electrodes.

Method used

Chitin gel is used for heating pretreatment and carbonization. By controlling the temperature and heating rate, the internal stress of the molecules is reduced, a loose and orderly carbon skeleton is formed, and the mechanical strength and flexibility of the flexible current collector material are improved.

Benefits of technology

The preparation of flexible current collector materials is achieved, which has good mechanical strength and flexibility, improves the repeatability and operability of the preparation process, and meets the application requirements of flexible electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851141A_ABST
    Figure CN118851141A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a flexible current collector material, and relates to the technical field of current collector preparation, the preparation method of the flexible current collector material comprises the following steps: chitin gel is heated to a first temperature T1 for pretreatment, and the first temperature T1 is lower than the carbonization temperature of the chitin gel; and carrying out carbonization treatment on the pretreated chitin gel to obtain the flexible current collector material. Wherein local damage of molecular internal stress to a basic carbon skeleton of chitin is reduced through heating pretreatment, and the structure of the basic carbon skeleton of chitin gel can be maintained; the temperature rising temperature lower than the carbonization temperature of the chitin gel also reduces excessive dehydration and excessive hardening of the chitin gel, meanwhile, molecular chains of the chitin gel are rearranged and adjusted at a low speed, the structure of the formed flexible current collector material is looser and more ordered, the material keeps certain mechanical strength, and meanwhile, the flexibility of the flexible current collector material is improved. Good flexibility is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of current collector preparation, and in particular to a preparation method and application of a flexible current collector material. Background Art

[0002] Three-dimensional porous carbon has unique three-dimensional network structure, high conductivity, large specific surface area and other characteristics, which are conducive to mass transfer and electron diffusion, and has great application prospects in the field of current collectors for advanced energy storage batteries such as lithium-ion batteries and sodium-ion batteries. In addition, considering the diverse application scenarios such as wearables, flexible batteries are now the focus of development, and the corresponding flexible current collectors also have important demands.

[0003] However, the preparation of existing high-performance three-dimensional porous carbon current collectors often requires complex and cumbersome preparation processes with high costs and low yields. Derivatives based on biomass raw materials such as cellulose and chitin are new environmentally friendly and low-carbon methods for preparing three-dimensional porous carbon that have been developed in recent years. However, the final product obtained after conventional high-temperature carbonization treatment is difficult to ensure good mechanical strength, has poor effects, low pass rates, and poor repeatability of experimental operations. In addition, existing carbonization products are basically not flexible and cannot meet the actual application requirements of flexible electrodes. Summary of the invention

[0004] The main purpose of the present invention is to propose a preparation method and application of a flexible current collector material, aiming to solve the problems of poor mechanical strength, low pass rate, poor flexibility and poor repeatability of flexible current collector materials prepared using biomass raw materials in the prior art.

[0005] To achieve the above object, the present invention provides a method for preparing a flexible current collector material, comprising the following steps:

[0006] The chitosan gel is heated to a first temperature T1 for pretreatment, wherein the first temperature T1 is lower than the carbonization temperature of the chitosan gel;

[0007] The chitosan gel that has undergone the pretreatment is carbonized to obtain the flexible current collector material.

[0008] In one embodiment, the pretreatment of heating the chitosan gel to a first temperature T1 comprises:

[0009] The chitosan gel is heated to T0 for a first pretreatment, and then heated to a first temperature T1 for a second pretreatment, wherein T0<the first temperature T1<the carbonization temperature of the chitosan gel.

[0010] In one embodiment, the chitosan gel is heated to T0 for a first pretreatment, and then heated to a first temperature T1 for a second pretreatment:

[0011] The value range of T0 is 280-320° C.; and / or,

[0012] The heating rate to T0 is less than or equal to 1°C / min, and / or,

[0013] The first pretreatment includes heat preservation at T0, and the heat preservation time is 0.3 to 0.7 hours; and / or,

[0014] The first temperature T1 has a value range of 380-420° C.; and / or,

[0015] The heating rate to the first temperature T1 is less than or equal to 1°C / min;

[0016] The second pretreatment includes keeping warm at a first temperature T1, and the keeping warm time is 0.3 to 0.7 hours.

[0017] In one embodiment, the carbonizing the pretreated chitosan gel to obtain the flexible current collector material comprises:

[0018] The chitosan gel that has completed the pretreatment is heated to a second temperature T2 for a first carbonization treatment, and then heated to a third temperature T3 for a second carbonization treatment to obtain the flexible current collector material.

[0019] In one embodiment, the chitosan gel that has completed the pretreatment is heated to a second temperature T2 for a first carbonization treatment, and then heated to a third temperature T3 for a second carbonization treatment to obtain the flexible current collector material:

[0020] The second temperature T2 has a value range of 580-620° C.; and / or,

[0021] The heating rate of heating to the second temperature T2 is less than or equal to 2°C / min; and / or,

[0022] The first carbonization treatment includes heat preservation at a second temperature T2, the heat preservation time is 1.8 to 2.2 hours; and / or,

[0023] The third temperature T3 has a value range of 780-820° C.; and / or,

[0024] The heating rate of heating to the third temperature T3 is less than or equal to 1°C / min; and / or,

[0025] The second carbonization treatment includes heat preservation at a second temperature T2, and the heat preservation time is 0.8 to 1.2 hours.

[0026] In one embodiment, the chitosan gel is prepared by the following steps:

[0027] S11, obtaining a chitosan solution;

[0028] S12, mixing the chitosan solution and the cross-linking agent for chemical cross-linking, so that at least part of the chitosan is chemically cross-linked to obtain a first chitosan gel;

[0029] S13, mixing the first chitosan gel and a solution containing monovalent hydrogen ions for physical crosslinking, so that at least part of the chitosan is physically crosslinked to obtain a second chitosan gel;

[0030] S14, washing the second chitosan gel with an alcohol reagent and water in sequence, cooling, and drying to obtain a chitosan gel.

[0031] In one embodiment, step S11 includes:

[0032] S111. Mix chitosan, alkali, urea, thiourea and water, and prepare a chitosan solution by adopting a freeze-thaw cycle technique.

[0033] In one embodiment, in step S111, the mass ratio of chitosan, alkali, urea, thiourea and water is (0.5-3): (9-11): (3-5): (0.5-1.5): (80-90); and / or,

[0034] The freezing temperature in the freeze-thaw cycle technology is -40 to -60°C; and / or,

[0035] The freezing time in the cyclic freeze-thaw technology is 4 to 12 hours; and / or,

[0036] The thawing temperature in the freeze-thaw cycle technique is 20-25°C; and / or,

[0037] The thawing time in the cyclic freeze-thaw technology is 2.5 to 3.5 hours; and / or,

[0038] The number of cycles in the cyclic freeze-thaw technique is 3 to 5 times.

[0039] In one embodiment, in step S12, the volume ratio of the chitosan solution to the cross-linking agent is (18-22):1; and / or,

[0040] In step S12, the chemical cross-linking time is 0.5 to 1 hour; and / or,

[0041] In step S12, the cross-linking agent includes any one of epichlorohydrin and epichlorohydrin, and / or,

[0042] In step S13, the physical cross-linking time is 15 to 25 seconds; and / or,

[0043] In step S13, the solution containing monovalent hydrogen ions includes any one of hydrochloric acid and acetic acid; and / or,

[0044] In step S14, the cooling method includes freezing with liquid nitrogen; and / or,

[0045] In step S14, the drying method includes freeze drying.

[0046] The present invention also proposes an application, in which the flexible current collector material prepared by the method for preparing the flexible current collector material is applied to a wearable device, and the method for preparing the flexible current collector material comprises the following steps:

[0047] The chitosan gel is heated to a first temperature T1 for pretreatment, wherein the first temperature T1 is lower than the carbonization temperature of the chitosan gel;

[0048] The chitosan gel that has completed the pretreatment is carbonized to obtain the flexible current collector material.

[0049] The present invention proposes a preparation method and application of a flexible current collector material, wherein, on the one hand, the temperature pretreatment removes the free water, part of the bound water and volatile gas in the chitosan gel in advance, so that it is slowly dehydrated and degassed, reducing the generation of molecular internal stress, reducing the local damage of the molecular internal stress to the basic carbon skeleton of chitosan, and helping to maintain the structure of the basic carbon skeleton of chitosan gel; on the other hand, the temperature rise below the carbonization temperature of chitosan gel also reduces the excessive dehydration and excessive hardening of chitosan gel, and at the same time, the molecular chain of chitosan gel is rearranged and adjusted at a slower speed, so that the structure of the flexible current collector material formed is looser and more orderly, so that the material has better flexibility while maintaining a certain mechanical strength. Through this pretreatment procedure, the stable structure and mechanical properties of the flexible current collector material can be more accurately controlled, and the repeatability and operability of the experimental process are enhanced. BRIEF DESCRIPTION OF THE DRAWINGS

[0050] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.

[0051] Figure 1 This is a scanning electron microscope image of the flexible current collector material in Example 1 provided by the present invention;

[0052] Figure 2 This is a test diagram of the flexibility performance of the flexible current collector material in Example 1 provided by the present invention.

[0053] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION

[0054] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.

[0055] Three-dimensional porous carbon has unique three-dimensional network structure, high conductivity, large specific surface area and other characteristics, which are conducive to mass transfer and electron diffusion, and has great application prospects in the field of current collectors for advanced energy storage batteries such as lithium-ion batteries and sodium-ion batteries. In addition, considering the diverse application scenarios such as wearables, flexible batteries are now the focus of development, and the corresponding flexible current collectors also have important demands.

[0056] However, the preparation of existing high-performance three-dimensional porous carbon current collectors often requires complex and cumbersome preparation processes with high costs and low yields. Derivatives based on biomass raw materials such as cellulose and chitin are new environmentally friendly and low-carbon methods for preparing three-dimensional porous carbon that have been developed in recent years. However, it is difficult to ensure good mechanical strength of the final product obtained after conventional high-temperature carbonization treatment, and the effect is poor and the qualified rate is low; and conventional high-temperature carbonization treatment is usually an extensive heat treatment process, and the repeatability of experimental operations is poor. In addition, the existing carbonization products are basically not flexible and cannot meet the actual application requirements of flexible electrodes.

[0057] In view of this, the present invention provides a method for preparing a flexible current collector material, comprising the following steps:

[0058] The chitosan gel is heated to a first temperature T1 for pretreatment, wherein the first temperature T1 is lower than the carbonization temperature of the chitosan gel; and the chitosan gel that has undergone the pretreatment is carbonized to obtain the flexible current collector material.

[0059] In the technical scheme of the present invention, the chitosan gel is pretreated by heating below the carbonization temperature of the chitosan gel before being carbonized, wherein the heating pretreatment removes the free water, part of the bound water and volatile gas in the chitosan gel in advance, so that it is slowly dehydrated and degassed, reducing the generation of molecular internal stress, reducing the local damage of the molecular internal stress to the basic carbon skeleton of chitosan, and helping to maintain the structure of the basic carbon skeleton of the chitosan gel; on the other hand, the heating temperature below the carbonization temperature of the chitosan gel also reduces the excessive dehydration and excessive hardening of the chitosan gel, and at the same time, the molecular chain of the chitosan gel is rearranged and adjusted at a slower speed, and the structure of the flexible current collector material formed is looser and more orderly, so that the material has better flexibility while maintaining a certain mechanical strength. Through this pretreatment procedure, the stable structure and mechanical properties of the flexible current collector material can be more accurately controlled, and the repeatability and operability of the experimental process are enhanced.

[0060] It should be noted that the temperature pretreatment process of the present invention can be set to be completed in a single temperature increase mode or in a gradient temperature increase mode. As long as the temperature of the temperature pretreatment is higher than the room temperature and lower than the carbonization temperature of the chitosan gel, the effect of the present invention is finally achieved. There is no strict restriction on the length of the pretreatment time and the number of temperature increases.

[0061] It should be noted that the carbonization treatment of the present invention can be completed in a single heating mode or in a gradient heating mode. As long as the temperature of the carbonization treatment is higher than the carbonization temperature of the chitosan gel and the effect of the present invention is finally achieved, there is no strict restriction on the length of the pretreatment time and the number of heating times.

[0062] In some embodiments of the present invention, the pretreatment of the chitosan gel by heating it to a first temperature T1 includes: heating the chitosan gel to T0 for a first pretreatment, and then heating it to the first temperature T1 for a second pretreatment, wherein T0 < the first temperature T1 < the carbonization temperature of the chitosan gel. The pretreatment is divided into two steps of heating, so that the chitosan molecular chains are rearranged under milder conditions, which helps to control the process of physical and chemical changes inside the chitosan molecules, is conducive to obtaining a more structurally perfect carbon basic skeleton, and is also conducive to improving the flexibility of the final flexible current collector material.

[0063] In some embodiments of the present invention, the chitosan gel is heated to T0 for the first pretreatment, and then heated to the first temperature T1 for the second pretreatment: the value range of T0 is 280-320°C. T0 can be 280°C, 300°C, 310°C or 320°C. Within this range, T0 can ensure that the chemical bonds inside the chitosan gel molecules are broken at a lower temperature to obtain a relatively complete and stable basic carbon skeleton, which is beneficial to improve the flexibility of the final flexible current collector material.

[0064] In some embodiments of the present invention, the chitosan gel is heated to T0 for a first pretreatment, and then heated to a first temperature T1 for a second pretreatment: the heating rate to T0 is less than or equal to 1°C / min. The heating rate to T0 can be 0.2°C / min, 0.6°C / min, 0.8°C / min or 1°C / min. The heating rate to T0 within a suitable range can ensure that the chemical bonds inside the chitosan gel molecules are broken at a slower speed, maintaining the basic carbon skeleton structure from being destroyed, which is beneficial to improving the flexibility of the final flexible current collector material.

[0065] In some embodiments of the present invention, the chitosan gel is heated to T0 for a first pretreatment, and then heated to a first temperature T1 for a second pretreatment: the first pretreatment includes heat preservation at T0, and the heat preservation time is 0.3 to 0.7 hours. The heat preservation time of the first pretreatment can be 0.3 hours, 0.5 hours or 0.7 hours. The heat preservation time of the first pretreatment within a suitable range can ensure that the chemical bonds inside the chitosan gel molecules are broken slowly over a long period of time, and the basic carbon skeleton structure is maintained without being destroyed.

[0066] In some embodiments of the present invention, the chitosan gel is heated to T0 for the first pretreatment, and then heated to the first temperature T1 for the second pretreatment: the value range of the first temperature T1 is 380-420°C. The first temperature T1 can be 380°C, 400°C or 420°C. The first temperature T1 can ensure a relatively stable and complete basic carbon skeleton within a suitable range, which is beneficial to improving the flexibility of the final flexible current collector material.

[0067] In some embodiments of the present invention, the chitosan gel is heated to T0 for a first pretreatment, and then heated to a first temperature T1 for a second pretreatment: the heating rate to the first temperature T1 is less than or equal to 1°C / min. The heating rate to the first temperature T1 can be 0.2°C / min, 0.6°C / min, 0.8°C / min or 1°C / min. The heating rate to the first temperature T1 is within a suitable range to ensure that a relatively stable and complete basic carbon skeleton is obtained, which is beneficial to improving the flexibility of the final flexible current collector material.

[0068] In some embodiments of the present invention, the chitosan gel is heated to T0 for a first pretreatment, and then heated to a first temperature T1 for a second pretreatment: the second pretreatment includes keeping warm at the first temperature T1, and the keeping warm time is 0.3 to 0.7 hours. The keeping warm time of the second pretreatment can be 0.3 hours, 0.5 hours or 0.7 hours. The keeping warm time of the second pretreatment within a suitable range can ensure that the chemical bonds inside the chitosan gel molecules are broken slowly for a long time, maintain the carbon skeleton structure from being destroyed, and help improve the flexibility of the final flexible current collector material.

[0069] In some embodiments of the present invention, the carbonization treatment of the pretreated chitosan gel to obtain the flexible current collector material includes: heating the pretreated chitosan gel to a second temperature T2 for a first carbonization treatment, and then heating it to a third temperature T3 for a second carbonization treatment to obtain the flexible current collector material.

[0070] In the technical solution of the present invention, the carbonization treatment is divided into two steps of heating, the purpose of which is to prevent the embrittlement of the carbonaceous structure during the high-temperature carbonization process, which is beneficial to improving the flexibility of the final flexible current collector material and making the preparation process also have good repeatability and operability.

[0071] In some embodiments of the present invention, the chitosan gel that has completed the pretreatment is heated to a second temperature T2 for a first carbonization treatment, and then heated to a third temperature T3 for a second carbonization treatment, to obtain the flexible current collector material: the second temperature T2 has a value range of 580 to 620°C. The second temperature T2 can be 580°C, 600°C, 615°C or 620°C. The second temperature T2 can ensure that the first carbonization process is mild within a suitable range, gradually remove the remaining moisture and volatile substances, and begin to form a carbon structure at the same time, completing the initial carbonization degradation, but not causing structural damage too quickly, thereby reducing the probability of embrittlement of the carbonaceous structure during the high-temperature carbonization process.

[0072] In some embodiments of the present invention, the chitosan gel that has completed the pretreatment is heated to a second temperature T2 for a first carbonization treatment, and then heated to a third temperature T3 for a second carbonization treatment, to obtain the flexible current collector material: the heating rate of heating to the second temperature T2 is less than or equal to 2°C / min. The heating rate of heating to the second temperature T2 can be 0.2°C / min, 0.6°C / min, 1.8°C / min or 2°C / min. The slower the heating rate, the better. This can ensure that the first carbonization process is relatively mild, gradually remove the remaining moisture and volatile substances, and begin to form a carbon structure at the same time, but not too fast to cause structural damage, thereby reducing the probability of embrittlement of the carbonaceous structure during the high-temperature carbonization process.

[0073] In some embodiments of the present invention, the chitosan gel that has completed the pretreatment is heated to a second temperature T2 for a first carbonization treatment, and then heated to a third temperature T3 for a second carbonization treatment, to obtain the flexible current collector material: the first carbonization treatment includes heat preservation at the second temperature T2, and the heat preservation time is 1.8 to 2.2 hours. The heat preservation time of the first carbonization treatment can be 1.8 hours, 2 hours or 2.2 hours. The heat preservation time of the first carbonization treatment within a suitable range can ensure that the first carbonization treatment process can fully remove the remaining moisture and volatile substances and form a more stable carbon structure.

[0074] In some embodiments of the present invention, the chitosan gel that has completed the pretreatment is heated to a second temperature T2 for a first carbonization treatment, and then heated to a third temperature T3 for a second carbonization treatment, to obtain the flexible current collector material: the third temperature T3 has a value range of 780 to 820°C. The third temperature T3 can be 780°C, 800°C or 820°C. The third temperature T3 can effectively control the pyrolysis rate within a suitable range, promote deeper crosslinking between molecules and densification of the carbon structure, fully and stably carbonize the chitosan, and reduce internal stress at the same time, ensuring that the carbonization is sufficient but not excessive, thereby obtaining a carbon material with a more uniform structure and better performance.

[0075] In some embodiments of the present invention, the chitosan gel that has completed the pretreatment is heated to a second temperature T2 for a first carbonization treatment, and then heated to a third temperature T3 for a second carbonization treatment, to obtain the flexible current collector material: the heating rate of heating to the third temperature T3 is less than or equal to 1°C / min. The heating rate of heating to the third temperature T3 can be 0.2°C / min, 0.6°C / min, 0.8°C / min or 1°C / min. The heating rate of heating to the third temperature T3 can effectively control the pyrolysis rate within a suitable range, promote deeper crosslinking between molecules and densification of the carbon structure, and reduce internal stress at the same time, ensuring sufficient carbonization but not over-carbonization, thereby obtaining a carbon material with a more uniform structure and better performance.

[0076] In some embodiments of the present invention, the chitosan gel that has completed the pretreatment is heated to a second temperature T2 for a first carbonization treatment, and then heated to a third temperature T3 for a second carbonization treatment, to obtain the flexible current collector material: the second carbonization treatment includes heat preservation at a second temperature T2, and the heat preservation time is 0.8 to 1.2 hours. The heat preservation time of the second carbonization treatment can be 1.2 hours, 1.2 hours or 1.2 hours, and the heat preservation time of the second carbonization treatment can ensure sufficient carbonization within an appropriate range.

[0077] In some embodiments of the present invention, the chitosan gel is prepared by the following steps:

[0078] S11, obtaining a chitosan solution;

[0079] S12, mixing the chitosan solution and the cross-linking agent for chemical cross-linking, so that at least part of the chitosan is chemically cross-linked to obtain a first chitosan gel;

[0080] S13, mixing the first chitosan gel and a solution containing monovalent hydrogen ions for physical crosslinking, so that at least part of the chitosan is physically crosslinked to obtain a second chitosan gel;

[0081] S14, washing the second chitosan gel with an alcohol reagent and water in sequence, cooling, and drying to obtain a chitosan gel.

[0082] In the technical scheme of the present invention, chemical crosslinking connects chitin molecules in the form of covalent bonds, strengthens the network structure of chitin, and improves its mechanical strength and chemical resistance. In step S12, some chitin molecules react with the crosslinking agent to form stable chemical bonds. In step S13, the first chitin gel is mixed with a solution containing monovalent hydrogen ions. Among them, the role of the monovalent hydrogen ions may be to promote the formation of hydrogen bonds between chitin molecules and achieve physical crosslinking. Physical crosslinking does not involve the formation of covalent bonds, but strengthens the internal connection of chitin through intermolecular forces such as hydrogen bonds and van der Waals forces. This process can supplement chemical crosslinking to ensure that even the chitin parts that are not directly involved in chemical crosslinking can be tightly combined through physical action, further improving the overall stability and integrity of the chitin gel. In step S14, first wash with an alcohol reagent to remove unreacted crosslinking agents, low molecular weight substances and possible impurities, and then wash with water to remove alcohol residues. After washing, the gel needs to be cooled and dried. Cooling helps to stabilize the gel structure, and drying removes moisture so that the gel reaches the desired physical state for subsequent processing.

[0083] It should be noted that the molecular weight of chitosan in the present invention is (203.19)n, wherein 203.19 is the molecular weight of the chitosan monomer unit, i.e., the molecular weight of chitosan is the molecular weight of its basic unit N-acetylamino-D-glucose 203.19 multiplied by the number of repeating units n, and the number of repeating units can be 100, 120 or 200, etc. The mass concentration of chitosan in the chitosan solution is 30-35 g / L, and its mass concentration can be 30 g / L, 33 g / L or 35 g / L, and its mass concentration within this range can ensure that a better carbonized skeleton is obtained.

[0084] It should be noted that the conditions for chemical cross-linking are: adding the cross-linking agent dropwise into the chitosan solution at 0° C. to obtain the first chitosan gel.

[0085] In some embodiments of the present invention, step S11 includes: S111, mixing chitosan, alkali, urea, thiourea and water, and preparing a chitosan solution by adopting a cyclic freeze-thaw technology.

[0086] In the technical solution of the present invention, the freeze-thaw cycle technology is used to obtain a colorless and transparent chitosan solution, which is not turbid and free of impurities, and ensures that the chitosan solution is fully dissolved.

[0087] In some embodiments of the present invention, in step S111, the mass ratio of chitosan, alkali, urea, thiourea and water is (0.5-3): (9-11): (3-5): (0.5-1.5): (80-90). The mass ratio of chitosan, alkali, urea, thiourea and water can be 0.5:9:3:0.5:80, 3:10:4:1:85 or 2:11:5:1.5:90. The mass ratio within the appropriate range can ensure that chitosan is fully dissolved to form a colorless and transparent chitosan solution.

[0088] In some embodiments of the present invention, in step S111, the freezing temperature in the cyclic freeze-thaw technology is -40 to -60°C. The freezing temperature in the cyclic freeze-thaw technology can be -40°C, -50°C or -60°C. The freezing temperature in the cyclic freeze-thaw technology can ensure that the chitosan solution is frozen and solidified quickly within a suitable range, and uniform and fine ice crystals are quickly formed, thereby reducing damage to the molecular structure of chitosan.

[0089] It should be noted that the freezing temperature provided by the present invention is a preferred solution. In actual operation, the effect of the present invention can be achieved as long as the temperature is lower than the freezing point of the chitosan solution.

[0090] In some embodiments of the present invention, in step S111, the freezing time in the cyclic freeze-thaw technology is 4 to 12 hours. The freezing time in the cyclic freeze-thaw technology can be 4 hours, 8 hours or 12 hours. The freezing time in the cyclic freeze-thaw technology can ensure that the chitosan solution is fully frozen within an appropriate range.

[0091] In some embodiments of the present invention, in step S111, the thawing temperature in the cyclic freeze-thaw technique is 20-25° C. The thawing temperature in the cyclic freeze-thaw technique may be 20° C., 22° C. or 25° C. The thawing temperature in the cyclic freeze-thaw technique within a suitable range may help to promote the chitosan molecules to aggregate or reorganize more closely through physical action, thereby increasing the stability of chitosan in the solvent.

[0092] In some embodiments of the present invention, in step S111, the thawing time in the cyclic freeze-thaw technology is 2.5 to 3.5 hours. The thawing time in the cyclic freeze-thaw technology can be 2.5 hours, 3 hours or 3.5 hours. The thawing time in the cyclic freeze-thaw technology can ensure that the chitosan solution solid is thawed more fully within a suitable range.

[0093] In some embodiments of the present invention, in step S111, the number of cycles in the cyclic freeze-thaw technique is 3 to 5. The number of cycles in the cyclic freeze-thaw technique can be 3, 4 or 5. The number of cycles in the cyclic freeze-thaw technique within an appropriate range can ensure that the chitosan solution is colorless and transparent, that is, the chitosan is fully dissolved in the solution.

[0094] In some embodiments of the present invention, in step S12, the volume ratio of the chitosan solution to the crosslinking agent is (18-22):1. The volume ratio of the chitosan solution to the crosslinking agent can be 18:1, 20:1 or 22:1. The volume ratio of the chitosan solution to the crosslinking agent within a suitable range can ensure that during the chemical crosslinking process, the chitosan molecules can be appropriately interconnected, neither excessively nor insufficiently, so as to achieve a suitable crosslinking density. Excessive crosslinking may cause the chitosan gel to become hard and brittle, while insufficient crosslinking may cause the chitosan gel structure to become loose, and the physical and chemical stability to decrease.

[0095] In some embodiments of the present invention, in step S12, the chemical cross-linking time is 0.5 to 1 hour. The chemical cross-linking time can be 0.5 hours, 0.7 hours or 1 hour. The chemical cross-linking time within a suitable range can ensure that the chitosan molecules have a good cross-linking density.

[0096] In some embodiments of the present invention, in step S12, the cross-linking agent includes any one of epichlorohydrin and epichlorohydrin. The cross-linking agent can be epichlorohydrin or epichlorohydrin. Compared with other cross-linking agents, the above cross-linking agent has better efficiency in chemical reaction and good compatibility with chitin.

[0097] In some embodiments of the present invention, in step S13, the physical crosslinking time is 15 to 25 seconds. The physical crosslinking time can be 15 seconds, 20 seconds or 25 seconds. The physical crosslinking time within a suitable range can cause some chitin molecular chains to be forced to be arranged in parallel in a liquid environment through strong self-cohesion, thereby forming a more compact structure.

[0098] In some embodiments of the present invention, in step S13, the solution containing monovalent hydrogen ions includes any one of hydrochloric acid and acetic acid. Compared with other solutions containing monovalent hydrogen ions, the above solution can more accurately control the pH value of the solution, thereby controlling the degree of physical cross-linking.

[0099] In some embodiments of the present invention, in step S14, the cooling method includes liquid nitrogen freezing. Compared with other cooling methods, liquid nitrogen freezing can promote rapid cooling of chitosan gel and maintain the microstructure unchanged.

[0100] In some embodiments of the present invention, in step S14, the drying method includes freeze drying. Compared with other drying methods, freeze drying directly removes water through the sublimation process, avoiding the destruction of the material structure during the evaporation of water, so that the chitosan gel after drying maintains good porosity and looseness.

[0101] The present invention also proposes an application, in which the flexible current collector material prepared by the method for preparing the flexible current collector material is applied to a wearable device. The flexible current collector material has all the technical solutions of the method for preparing the flexible current collector material, and therefore also has all the beneficial effects brought by the above technical solutions, which will not be repeated here one by one.

[0102] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.

[0103] Example 1

[0104] A method for preparing a flexible current collector material comprises the following steps:

[0105] (1) Obtain chitosan solution: Mix crude chitosan raw material powder (purchased from Zhejiang Jinke Pharmaceutical Co., Ltd. without prior purification) with NaOH, urea, thiourea, and deionized water in a mass ratio of 3:10:4:1:85, and stir with a magnetic stirrer at room temperature for 30 minutes to dissolve NaOH, urea, and thiourea to promote uniform mixing of the raw materials. Then place the mixed solution in a low-temperature box precooled to -60°C for 12 hours, then take it out and thaw it at room temperature for 3 hours, and then place it in a magnetic stirrer for 1 hour (the first stirring requires manual assistance with a glass rod). This cycle is repeated 5 times to form a colorless and transparent chitosan solution. The obtained transparent chitosan solution is centrifuged at 8000 rpm in a 0°C constant temperature centrifuge for 10 minutes to obtain a chitosan solution without bubbles and impurities.

[0106] (2) Preparation of chitosan gel: In a constant temperature ice water bath at 0°C, under continuous magnetic stirring at a constant speed of 500 rpm, 50 mL of crosslinking agent epichlorohydrin was dripped dropwise into 1000 g of chitosan solution through a constant pressure dropping funnel within 30 minutes for chemical crosslinking to obtain the first chitosan gel. Then, the first chitosan gel was quickly placed in a 0.1 M hydrochloric acid solution for 20 seconds for physical crosslinking to obtain the second chitosan gel. Then, the second chitosan gel was immersed in ethanol and deionized water cylinders for 2 hours and 48 hours respectively, and the liquid circulation was kept flowing continuously to thoroughly wash away the residual acid, alkali and other reagents.

[0107] The washed second chitosan gel was placed in liquid nitrogen for rapid cooling to maintain the microstructure unchanged, and then the frozen second chitosan gel was placed in a freeze drying oven at -70°C for drying for 24 hours to obtain chitosan gel.

[0108] (3) Chitosan gel pretreatment and carbonization treatment procedure: The freeze-dried chitosan gel was subjected to programmed temperature control in a N2 protected tube furnace. The procedure is as follows:

[0109] First pretreatment: heating from room temperature to 300°C at a rate of 1°C / min and keeping at this temperature for 0.5h;

[0110] Second pretreatment: heating from 300°C to 400°C at a heating rate of 1°C / min, and keeping the temperature for 0.5h;

[0111] First carbonization treatment: heating from 400°C to 600°C at a heating rate of 2°C / min and keeping at this temperature for 2h;

[0112] Second carbonization treatment: heating from 600°C to 800°C at a heating rate of 1°C / min and keeping at this temperature for 1h.

[0113] Example 2

[0114] A method for preparing a flexible current collector material comprises the following steps:

[0115] (1) Obtain chitosan solution: Mix crude chitosan raw material powder (purchased from Zhejiang Jinke Pharmaceutical Co., Ltd. without prior purification) with NaOH, urea, thiourea, and deionized water in a mass ratio of 0.5:11:5:1.5:90, and stir with a magnetic stirrer at room temperature for 30 minutes to dissolve NaOH, urea, and thiourea to promote uniform mixing of the raw materials. Then place the mixed solution in a low-temperature box precooled to -40°C for 4 hours, then take it out and thaw it at 20°C for 2.5 hours, and then place it in a magnetic stirrer and stir for 1 hour (the first stirring requires manual assistance with a glass rod). This cycle is repeated 3 times to form a colorless and transparent chitosan solution. The obtained transparent chitosan solution is centrifuged at 8000 rpm in a 0°C constant temperature centrifuge for 10 minutes to obtain a chitosan solution without bubbles and impurities.

[0116] (2) Preparation of chitosan gel: In a constant temperature ice water bath at 0°C, under continuous magnetic stirring at a constant speed of 500 rpm, the crosslinking agent epichlorohydrin was dripped into the chitosan solution drop by drop through a constant pressure dropping funnel within 45 minutes for chemical crosslinking, wherein the volume ratio of the chitosan solution to the crosslinking agent was 18:1, to obtain the first chitosan gel. The first chitosan gel was then quickly placed in a 0.1M hydrochloric acid solution for 15 seconds for physical crosslinking to obtain the second chitosan gel. The second chitosan gel was then immersed in ethanol and deionized water cylinders for 2 hours and 48 hours respectively, and the liquid circulation was kept flowing continuously to thoroughly wash away the residual acid, alkali and other reagents.

[0117] The washed second chitosan gel was placed in liquid nitrogen for rapid cooling to maintain the microstructure unchanged, and then the frozen second chitosan gel was placed in a freeze drying oven at -70°C for drying for 24 hours to obtain chitosan gel.

[0118] (3) Chitosan gel pretreatment and carbonization treatment procedure: The freeze-dried chitosan gel was subjected to programmed temperature control in a N2 protected tube furnace. The procedure is as follows:

[0119] First pretreatment: heating from 20°C to 280°C at a heating rate of 0.1°C / min, and keeping warm for 0.3h;

[0120] Second pretreatment: heating from 280°C to 380°C at a heating rate of 0.1°C / min, and keeping the temperature for 0.3h;

[0121] First carbonization treatment: heating from 380°C to 580°C at a heating rate of 0.1°C / min and keeping the temperature for 1.8h;

[0122] Second carbonization treatment: increase the temperature from 580°C to 820°C at a heating rate of 0.1°C / min and keep the temperature for 0.8h.

[0123] Example 3

[0124] A method for preparing a flexible current collector material comprises the following steps:

[0125] (1) Obtain chitosan solution: Mix crude chitosan raw material powder (purchased from Zhejiang Jinke Pharmaceutical Co., Ltd. without prior purification) with NaOH, urea, thiourea, and deionized water in a mass ratio of 3:9:3:0.5:80, and stir with a magnetic stirrer at room temperature for 30 minutes to dissolve NaOH, urea, and thiourea to promote uniform mixing of the raw materials. Then place the mixed solution in a low-temperature box precooled to -60°C for 12 hours, then take it out and thaw it at 25°C for 3.5 hours, and then place it in a magnetic stirrer for 1 hour (the first stirring requires manual assistance with a glass rod). This cycle is repeated 5 times to form a colorless and transparent chitosan solution. The obtained transparent chitosan solution is centrifuged at 8000 rpm in a 0°C constant temperature centrifuge for 10 minutes to obtain a chitosan solution without bubbles and impurities.

[0126] (2) Preparation of chitosan gel: In a constant temperature ice water bath at 0°C, under continuous magnetic stirring at a constant speed of 500 rpm, the crosslinking agent epichlorohydrin was dripped into the chitosan solution drop by drop through a constant pressure dropping funnel within 60 minutes for chemical crosslinking, wherein the volume ratio of chitosan solution to crosslinking agent was 22:1, and the first chitosan gel was obtained. Then, the first chitosan gel was quickly placed in a 0.1M acetic acid solution for 25 seconds for physical crosslinking to obtain a second chitosan gel. Then, the second chitosan gel was immersed in ethanol and deionized water cylinders for 2 hours and 48 hours respectively, and the liquid circulation was kept flowing continuously to thoroughly wash away the residual acid, alkali and other reagents.

[0127] The washed second chitosan gel was placed in liquid nitrogen for rapid cooling to maintain the microstructure unchanged, and then the frozen second chitosan gel was placed in a freeze drying oven at -70°C for drying for 24 hours to obtain chitosan gel.

[0128] (3) Chitosan gel pretreatment and carbonization treatment procedure: The freeze-dried chitosan gel was subjected to programmed temperature control in a N2 protected tube furnace. The procedure is as follows:

[0129] First pretreatment: heating from 25°C to 320°C at a rate of 0.5°C / min, keeping warm for 0.7h;

[0130] Second pretreatment: heating from 320°C to 420°C at a heating rate of 0.5°C / min, and keeping the temperature for 0.7h;

[0131] First carbonization treatment: heating from 420°C to 620°C at a heating rate of 1.5°C / min and keeping at this temperature for 2.2h;

[0132] Second carbonization treatment: heat from 620°C to 820°C at a heating rate of 0.5°C / min and keep warm for 1.2h.

[0133] Comparative Example 1

[0134] Compared with Example 1, Comparative Example 1 is the same as Example 1 except that the first carbonization treatment and the second carbonization treatment are directly performed.

[0135] Performance Testing

[0136] The flexible current collector material prepared in Example 1 was observed by scanning electron microscopy and its flexibility was characterized. The specific detection method is as follows:

[0137] 1) Scanning electron microscope observation: The microscopic morphology of the current collector material obtained in Example 1 was observed by field emission scanning electron microscope (FE-SEM, JEOL JSM-7500F) at an accelerating voltage of 5 kV and a magnification of 10000, confirming that it has a network-like porous structure composed of a lamellar structural unit and a three-dimensionally oriented fiber skeleton. The results are as follows Figure 1 shown.

[0138] 2) Characterization of flexibility: Select a piece of prepared current collector material (size about 1.5*1.5cm 2 ), manually squeeze the two ends of the material sample toward the middle to make the middle bulge, further use tweezers to clamp the material sample, and gently press the tweezers to make the sample further bulge outward and bend. After the sample is bent by external force, the sample can still maintain structural integrity, without structural damage such as fragmentation, showing good flexibility characteristics. The results are as follows Figure 2 shown.

[0139] In summary, the structure of the flexible current collector material prepared by the preparation method of the flexible current collector material provided by the present invention is looser and more orderly, and has better flexibility while maintaining a certain mechanical strength; at the same time, the stable structure and mechanical properties of the flexible current collector material can be more accurately controlled, thereby enhancing the repeatability and operability of the experimental process.

[0140] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.

Claims

1. A method for preparing a flexible current collector material, characterized in that: The following steps are involved: The chitosan gel is heated to a first temperature T1 for pretreatment, wherein the first temperature T1 is lower than the carbonization temperature of the chitosan gel; The chitosan gel that has undergone the pretreatment is carbonized to obtain the flexible current collector material.

2. The method for preparing the flexible current collector material according to claim 1, characterized in that: The pretreatment of heating the chitosan gel to a first temperature T1 comprises: The chitosan gel is heated to T0 for a first pretreatment, and then heated to a first temperature T1 for a second pretreatment, wherein T0<the first temperature T1<the carbonization temperature of the chitosan gel.

3. The method for preparing the flexible current collector material according to claim 2, characterized in that: The chitosan gel is heated to T0 for a first pretreatment, and then heated to a first temperature T1 for a second pretreatment: The value range of T0 is 280-320° C.; and / or, The heating rate to T0 is less than or equal to 1°C / min, and / or, The first pretreatment includes heat preservation at T0, and the heat preservation time is 0.3 to 0.7 hours; and / or, The first temperature T1 has a value range of 380-420° C.; and / or, The heating rate to the first temperature T1 is less than or equal to 1°C / min; The second pretreatment includes keeping warm at a first temperature T1, and the keeping warm time is 0.3 to 0.7 hours.

4. The method for preparing the flexible current collector material according to claim 1, characterized in that: The step of carbonizing the pretreated chitosan gel to obtain the flexible current collector material comprises: The chitosan gel that has completed the pretreatment is heated to a second temperature T2 for a first carbonization treatment, and then heated to a third temperature T3 for a second carbonization treatment to obtain the flexible current collector material.

5. The method for preparing the flexible current collector material according to claim 4, characterized in that: The chitosan gel that has completed the pretreatment is heated to a second temperature T2 for a first carbonization treatment, and then heated to a third temperature T3 for a second carbonization treatment to obtain the flexible current collector material: The second temperature T2 has a value range of 580-620° C.; and / or, The heating rate of heating to the second temperature T2 is less than or equal to 2°C / min; and / or, The first carbonization treatment includes heat preservation at a second temperature T2, the heat preservation time is 1.8 to 2.2 hours; and / or, The third temperature T3 has a value range of 780-820° C.; and / or, The heating rate of heating to the third temperature T3 is less than or equal to 1°C / min; and / or, The second carbonization treatment includes heat preservation at a second temperature T2, and the heat preservation time is 0.8 to 1.2 hours.

6. The method for preparing the flexible current collector material according to claim 1, characterized in that: The chitosan gel is prepared by the following steps: S11, obtaining a chitosan solution; S12, mixing the chitosan solution and the cross-linking agent for chemical cross-linking, so that at least part of the chitosan is chemically cross-linked to obtain a first chitosan gel; S13, mixing the first chitosan gel and a solution containing monovalent hydrogen ions for physical crosslinking, so that at least part of the chitosan is physically crosslinked to obtain a second chitosan gel; S14, washing the second chitosan gel with an alcohol reagent and water in sequence, cooling, and drying to obtain a chitosan gel.

7. The method for preparing the flexible current collector material according to claim 6, characterized in that: Step S11 includes: S111. Mix chitosan, alkali, urea, thiourea and water, and prepare a chitosan solution by adopting a freeze-thaw cycle technique.

8. The method for preparing the flexible current collector material according to claim 7, characterized in that: In step S111, the mass ratio of chitosan, alkali, urea, thiourea and water is (0.5-3): (9-11): (3-5): (0.5-1.5): (80-90); and / or, The freezing temperature in the cyclic freeze-thaw technology is -40 to -60°C; and / or, The freezing time in the cyclic freeze-thaw technology is 4 to 12 hours; and / or, The thawing temperature in the freeze-thaw cycle technique is 20-25°C; and / or, The thawing time in the cyclic freeze-thaw technology is 2.5 to 3.5 hours; and / or, The number of cycles in the cyclic freeze-thaw technique is 3 to 5 times.

9. The method for preparing the flexible current collector material according to claim 6, characterized in that: In step S12, the volume ratio of the chitosan solution to the cross-linking agent is (18-22):1; and / or, In step S12, the chemical cross-linking time is 0.5 to 1 hour; and / or, In step S12, the cross-linking agent includes any one of epichlorohydrin and epichlorohydrin, and / or, In step S13, the physical cross-linking time is 15 to 25 seconds; and / or, In step S13, the solution containing monovalent hydrogen ions includes any one of hydrochloric acid and acetic acid; and / or, In step S14, the cooling method includes freezing with liquid nitrogen; and / or, In step S14, the drying method includes freeze drying.

10. An application, wherein the flexible current collector material prepared by the method for preparing a flexible current collector material according to any one of claims 1 to 9 is applied to a wearable device.

Citation Information

Patent Citations

  • Chemical and physical double-cross-linking high-strength chitin gel material and preparation method thereof

    CN104387597A

  • Carbon aerogel prepared from chitin aerogel and preparation method thereof

    CN105502346A

  • Preparation method of sulfur / carbon aerogel composite material

    CN112142034A

  • Method for efficiently preparing chitin membrane material

    CN114907592A

  • Self-supporting flexible amorphous carbon-based negative electrode material and preparation method and application thereof

    CN117658129A