Method for regenerating and repairing graphite after wet lithium extraction of waste lithium battery

By carrying out multi-step cleaning and calcination treatment on the graphite residue after wet lithium extraction from used lithium batteries, the problem of impurity contamination and structural damage of graphite materials after decommissioning is solved, the regeneration and repair of high-purity graphite is realized, and the recycling cost is reduced. It has potential value for recycling in battery production.

CN118851167APending Publication Date: 2024-10-29GANNAN NORMAL UNIV

Patent Information

Application Number
CN202410855152.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The graphite anode material in used lithium batteries is difficult to directly recycle due to impurity contamination and structural damage after retirement, resulting in resource waste and environmental pollution.

Method used

A method of regenerating and repairing graphite after wet lithium extraction from waste lithium batteries is adopted. The graphite waste residue is broken into pieces and then subjected to multi-step cleaning and calcination in sodium hydroxide, hydrochloric acid and hydrogen peroxide solutions to remove impurities and repair the graphite structure. Obtain high-purity graphite material that can be used in battery grade.

Benefits of technology

It achieves the efficient removal of impurities and structural repair of graphite, improves the recovery rate and quality of graphite, reduces costs, conforms to the concept of green, low-carbon and sustainable development, and has the potential value of recycling in battery production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851167A_ABST
    Figure CN118851167A_ABST
Patent Text Reader

Abstract

The invention discloses a regeneration and repair method of graphite after wet lithium extraction of waste lithium batteries, which comprises the following specific steps: crushing graphite waste residue after wet lithium extraction into powder, immersing into a sodium hydroxide solution, stirring and cleaning; the graphite powder obtained after alkali washing in the first step is added into a hydrochloric acid solution to be stirred and leached; adding hydrochloric acid, sulfuric acid and hydrogen peroxide into the graphite powder subjected to acid pickling in the step 2, leaching in an ultrasonic environment, and drying; and 3, loading the graphite powder dried in the step 3 into a porcelain boat, and calcining by using a tubular furnace to obtain graphite. The reagents and the reaction method used in the method are relatively simple and feasible, the cost is relatively low, and the economic pressure of waste lithium ion battery graphite recovery is relieved; the graphite regenerated and repaired by the method is high in carbon content and graphitization rate, and other indexes meet the requirements of battery grade graphite.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of solid waste resource recovery, and in particular to a method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries. Background Art

[0002] As we all know, waste graphite contains a lot of harmful substances, such as heavy metals, electrolytes and organic matter. Moreover, the stacking of these substances also requires a large amount of land space, and will also cause groundwater and soil pollution. If they are not effectively treated, they will threaten the ecological environment and human health.

[0003] In modern society, with the rapid growth of demand for lithium-ion batteries, a large number of scrapped batteries will inevitably be generated. According to statistics, the content of graphite in medium-sized hybrid vehicles, plug-in hybrid vehicles (PHEVs) and electric vehicles can reach about 4kg, 8kg and 47kg respectively. Faced with the advent of a large number of lithium-ion battery retirements, the recycling and resource circulation of graphite negative electrode materials needs to be solved urgently. The discarding or incineration of waste graphite will bring serious environmental risks including particle pollution and greenhouse gas (GHGs) emissions. Therefore, the increasing scarcity of graphite resources makes the intelligent recycling or reuse of waste graphite particularly necessary. It is of great significance to carry out research on the recovery and reuse of graphite materials in waste batteries. On the one hand, it can realize the recycling and high-value utilization of graphite negative electrode materials and alleviate the pressure caused by resource shortages; on the other hand, it helps solve the environmental pollution caused by discarded lithium batteries.

[0004] In the prior art, lithium-ion batteries use a wet method to recover valuable metals. Specifically, the retired lithium-ion battery electrode active materials are dissolved after pre-treatment and pre-processing, so that valuable metals such as Li, Co, Ni, and Mn are dissolved in the solution in the form of ions, and the dissolved metal ions are separated from the solution by chemical precipitation, solvent extraction or ion exchange.

[0005] There is a large amount of scrapped graphite in the battery waste slag (graphite waste slag) after separating the valuable metals. These graphites still have recycling value, but the scrapped graphite cannot be directly recycled. On the one hand, there are still a small amount of heavy metals, electrolytes and organic matter in the scrapped graphite. These impurities will have a certain impact on the reuse of the scrapped graphite, and some methods are needed to remove the impurities. On the other hand, the physical and chemical structure of the scrapped graphite is severely damaged during the battery charging and discharging cycle, and it needs to be repaired to exert its original performance. Summary of the invention

[0006] In order to solve the above technical problems, the purpose of the present invention is to provide a method with low cost and high recovery rate.

[0007] In order to achieve the above-mentioned object of the invention, the technical solution of the present invention is:

[0008] A method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries, the specific steps are:

[0009] Step 1: crush the graphite waste residue after wet lithium extraction into powder, immerse it in sodium hydroxide solution, stir and wash it;

[0010] Step 2, adding the graphite powder after alkali washing in step 1 into a hydrochloric acid solution and stirring to leach;

[0011] Step 3: adding hydrochloric acid, sulfuric acid and hydrogen peroxide to the graphite powder after acid washing in step 2, leaching and drying under ultrasonic environment;

[0012] Step 4: Put the graphite powder dried in step 3 into a porcelain boat and calcine it in a tubular furnace to obtain graphite.

[0013] In the above technical scheme, the graphite content in the graphite waste slag after wet lithium extraction is 60-70%, and it also contains F, P, Al, Ni, C, Cu, Mn and Li.

[0014] According to the preferred technical solution, the waste graphite slag in step 1 is sieved through a 100-mesh sieve, the concentration of the sodium hydroxide solution is 1 to 1.5 mol / L, the solid-liquid ratio of the waste graphite slag to the sodium hydroxide solution is 1:10, the leaching time is ≥1h, and the mass loss of the waste graphite slag is 29 to 31%.

[0015] According to the preferred technical solution, the concentration of the hydrochloric acid solution in step 2 is 4 mol / L, the reaction temperature is 40° C., the solid-liquid ratio of the graphite powder to the hydrochloric acid solution is 1:8, and the mass loss of the graphite powder is 6 to 8.5%.

[0016] The preferred technical solution is that the concentration of the hydrochloric acid solution in step 3 is 3 mol / L, the reaction temperature is 40°C, the solid-liquid ratio of graphite powder to hydrochloric acid solution is 1:10, the volume ratio of hydrochloric acid, sulfuric acid and hydrogen peroxide is 6:3:1, and the concentration of hydrogen peroxide is 30%. Step 3 is carried out under an ultrasonic environment, the ultrasonic power is 300w, the ultrasonic time is 20min, and the mass loss of graphite powder is 4.5%.

[0017] In the above technical solution, the graphite obtained in step 4 has a fixed carbon content of ≥99.5%, a graphitization degree of ≥95%, and a particle size / D 50 Range 8~20μm, tap density ≥1.00g / cm 3 , ash content ≤ 0.100%, moisture ≤ 0.2%, specific surface area range 2~5m 2 / g, compacted density 1.2~2.0g / cm 3 , magnetic material content ≤0.5ppm.

[0018] The advantages of the present invention are:

[0019] 1. The reagents and reaction methods used in the present invention are relatively simple and easy to implement, and the cost is low, which reduces the economic pressure on recycling graphite from waste lithium-ion batteries;

[0020] 2. The carbon content and graphitization rate of the graphite regenerated and repaired by the present invention are high, and other indicators meet the requirements of battery-grade graphite;

[0021] 3. The graphite waste slag of the present invention has abundant sources and conforms to the green, low-carbon and sustainable development concept;

[0022] 4. Since the present invention has strong operability and low cost, it has certain potential application value in the field of graphite recycling in battery production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for use in the description of the embodiments will be briefly introduced below. The accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0024] The present invention will be further described below in conjunction with the accompanying drawings and embodiments:

[0025] Figure 1 This is the SEM image of graphite residue after wet lithium extraction from waste lithium batteries;

[0026] Figure 2 This is a SEM image of the graphite after regeneration and repair in Example 1;

[0027] Figure 3 This is the PXRD pattern of graphite waste residue after wet lithium extraction from waste lithium batteries;

[0028] Figure 4 : is the PXRD pattern of the graphite after regeneration and repair in Example 1;

[0029] Figure 5 This is the XPS image of graphite residue after wet lithium extraction from waste lithium batteries;

[0030] Figure 6 This is the XPS graph of the graphite after regeneration and repair in Example 1;

[0031] Figure 7 This is the Raman image of graphite residue after wet lithium extraction from waste lithium batteries;

[0032] Figure 8 is the Raman graph of the graphite after regeneration and repair in Example 1;

[0033] Fig. 9This is the particle size distribution diagram of the graphite after regeneration and repair in Example 1;

[0034] Fig.10 Magnetic field measurement data of graphite after regeneration and repair in Example 1;

[0035] Fig.11 Surface area data of graphite after regeneration and repair in Example 1;

[0036] Fig.12 Example 1: Pore volume data of regenerated and repaired graphite. DETAILED DESCRIPTION

[0037] Embodiment 1:

[0038] The method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries comprises the following steps:

[0039] Step 1: weigh 2g of graphite waste residue after wet lithium extraction, put it into a 500mL beaker, add 20mL of 1mol / L hydrogen peroxide solution and a rotor, seal the cup mouth with plastic wrap, put it into a constant temperature magnetic stirring water bath pot for stirring, the water temperature is 30°C, the speed is 200r / min, and stir for 30min.

[0040] Step 2: Take out from the magnetic stirring water bath, filter, rinse with water, put the filter residue back into the original beaker, add 16mL of 4mol / L hydrochloric acid, and bathe in a constant temperature water bath for 4h at a temperature of 40°C and a speed of 200r / min.

[0041] Step 3: Take out the mixture from the magnetic stirring water bath, rinse with water, put the residue back into the original beaker, add 12mL of 3mol / L hydrochloric acid solution, 6mL of concentrated sulfuric acid, and 2mL of 30% hydrogen peroxide, and bathe in a constant temperature water bath for 3h at 40°C and 200r / min. After taking out, place it in an ultrasonic cleaner for 20min of ultrasonic treatment, filter, rinse with water, and dry the residue in a blast drying oven.

[0042] Step 4: put the dried filter residue into a porcelain boat, place it in a muffle furnace, and calcine it at 1050° C. for 3 hours to obtain graphite.

[0043] The graphite content is 99%.

[0044] In Example 1, the metal is removed better and the graphite purification effect is further improved.

[0045] like Figure 1 , 2By comparison, it can be seen that the SEM image of the waste slag after lithium extraction shows that the microscopic morphology of the waste slag powder presents an irregular block structure, and the aggregates are composed of small particles of different sizes; the graphite particles after regeneration and repair show a better particle structure, and the surface of the particle structure is smooth, and there is no obvious adhesion material on the surface, indicating that high-purity graphite samples can be obtained.

[0046] like Figure 3 , 4 By comparison, it can be seen that the main diffraction peaks of the PXRD spectrum of the waste residue are consistent with those of iron phosphate and graphite, indicating that the main component of the waste residue is graphite, and it also contains some oxides of Co, Ni, Mn, and calcium sulfate; the regenerated and repaired graphite was tested by PXRD, and the test results showed that a strong graphite characteristic peak (002) was exhibited at 2θ=26.5°, indicating that the purified graphite still maintains the layered structure of graphite, and its layered structure is not damaged after acid washing and high temperature treatment. According to the interplanar spacing d(002), the degree of graphitization is calculated to be 96%.

[0047] like Figure 5 , 6 By comparison, it can be seen from the XPS full spectrum of the waste slag that the main elements contained in the waste slag are C, O, F, Cu, Co, Ni, Fe, Al, etc.; from the XPS full spectrum of the regenerated and repaired graphite, it can be seen that the element type contained in the purified sample is C, and the signals of other elements have basically disappeared.

[0048] like Figure 7 , 8 By comparison, it can be seen that in the Raman spectrum of the waste residue, D (1300cm -1 ) belt, G(1600cm -1 ) belt and 2D(2650cm -1 ) band is the characteristic peak of graphite, D band represents the defects of graphite crystal, and G band represents the carbon atom sp 2 Hybridized in-plane stretching vibration, and I D / I G is greater than 1, indicating that the graphite purity is high. In addition, the peaks of other components in the Raman spectrum are negligible, indicating that the waste contains more graphite. The graphite after regeneration and repair, and I D / I G It is equal to 0.42, indicating that the disorder of purified graphite is reduced, the degree of graphitization is improved, and the Raman peaks of other components disappear.

[0049] like Fig. 9 It can be seen that the particle size distribution of the regenerated and repaired graphite was tested, and the D 10 At 4.85μm, D 50At 18.65μm, D 90 At 98.23 μm, in addition, compared with commercial graphite, the particle size distribution of the purified graphite sample is wider, which further indicates that the impurities contained on the graphite surface are effectively removed.

[0050] like Fig.10 It can be seen that the magnetic susceptibility of the regenerated and repaired graphite was measured at 300K in the magnetic field range of -80 to 80kOe using AC magnetic susceptibility, but no obvious magnetic signal was observed. Therefore, it is shown that the regenerated and repaired graphite sample does not have magnetic properties.

[0051] like Fig.11 , Fig.12 It can be seen that the regenerated and repaired graphite was subjected to BET test, and the results are shown in the figure below. It can be seen from the figure that the N 2 The adsorption-desorption curve belongs to the standard H3 type hysteresis loop, and the Langmuir specific surface area of ​​the sample is 0.963m 2 / g, BET specific surface area is 2.639m 2 / g, and the pore volume is 0.002cc / g.

[0052] This embodiment produces obvious economic benefits, and the purified and repaired graphite has a higher content and better quality, and has good utilization value and commercial value. The graphite purified and repaired by the method of the present invention can be used to prepare battery-grade graphite to recycle the graphite in ternary lithium batteries, which is beneficial to saving energy and materials and protecting the environment, and produces significant beneficial effects.

[0053] Embodiment 2:

[0054] The method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries comprises the following steps:

[0055] Step 1: weigh 2g of graphite waste residue after wet lithium extraction, put it into a 500ml beaker, add 20mL of 1mol / L hydrogen peroxide solution and a rotor, seal the cup mouth with plastic wrap, put it into a constant temperature magnetic stirring water bath pot for stirring, the water temperature is 30°C, the speed is 200r / min, and stir for 1h.

[0056] Step 2: Take out the product from the magnetic stirring water bath, filter it, rinse it with water, put the filter residue back into the original beaker, add 20 mL of 3 mol / L hydrochloric acid, and bathe it in a constant temperature water bath for 4 hours at a temperature of 40°C and a speed of 200 r / min.

[0057] Step 3: Take out the mixture from the magnetic stirring water bath, rinse with water, put the residue back into the original beaker, add 13mL of 3mol / L hydrochloric acid solution, 6ml of concentrated sulfuric acid, and 1ml of 30% hydrogen peroxide, and bathe in a constant temperature water bath for 3h at 40°C and 200r / min. After taking out, place it in an ultrasonic cleaner for 5min of ultrasonic treatment, filter, rinse with water, and dry the residue in a blast drying oven.

[0058] Step 4: put the dried filter residue into a porcelain boat, place it in a muffle furnace, and calcine it at 1050° C. for 3 hours to obtain graphite.

[0059] The graphite content is 98.5%

[0060] In Example 2, the amount of reagents used was reduced, and the amount of hydrogen peroxide used was increased while the solid-liquid ratio remained unchanged. This was done to enhance the corrosiveness of hydrochloric acid and to leach more carbon-coated metals.

[0061] Embodiment 3:

[0062] The method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries comprises the following steps:

[0063] Step 1: weigh 2g of graphite waste residue after wet lithium extraction, put it into a 500mL beaker, add 20ml of 4mol / L hydrochloric acid solution and a rotor, seal the cup mouth with plastic wrap, put it into a constant temperature magnetic stirring water bath and stir it at a water temperature of 40°C and a speed of 200r / min for 4h.

[0064] Step 2: Take out, rinse with water appropriately, put the filter residue back into the original beaker, add 8mL of 3mol / l hydrochloric acid, 2mL of 30% hydrogen peroxide and 10mL of concentrated sulfuric acid, and bathe in a constant temperature water bath for 2h at a temperature of 40°C and a speed of 200r / min.

[0065] Step 3: Take out, rinse with water appropriately, put the filter residue back into the original beaker, add 20mL of 1mol / L sodium hydroxide solution, and bathe in a constant temperature water bath for 30min at 30℃ and 200r / min. Take out, rinse the mixture with pure water into a suction flask, rinse with water until the filtrate is almost colorless, and put the filter residue into a blast drying oven for drying.

[0066] Step 4: put the dried filter residue into a porcelain boat, place it in a muffle furnace, and calcine it at 1050° C. for 3 hours to obtain graphite.

[0067] The graphite content is 98.5%.

Claims

1. A method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries, characterized in that: The specific steps are: Step 1, crushing the graphite waste residue after wet lithium extraction into powder, immersing it in a sodium hydroxide solution, stirring and washing it, and obtaining graphite powder; Step 2, adding the graphite powder after alkali washing in step 1 into a hydrochloric acid solution and stirring to leach; Step 3: adding hydrochloric acid, sulfuric acid and hydrogen peroxide to the graphite powder after acid washing in step 2, leaching and drying under ultrasonic environment; Step 4: Put the graphite powder dried in step 3 into a porcelain boat and calcine it in a tubular furnace to obtain graphite.

2. The method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries according to claim 1, characterized in that: The concentration of the sodium hydroxide solution in step 1 is 1-1.5 mol / L, the solid-liquid ratio of the graphite waste slag to the sodium hydroxide solution is 1:10, and the leaching time is ≥1h.

3. The method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries according to claim 2, characterized in that: The mass loss of the graphite waste slag after alkali washing in step 1 is 29-31%.

4. The method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries according to claim 1, characterized in that: The concentration of the hydrochloric acid solution in step 2 is 4 mol / l, the reaction temperature is 40° C., and the solid-liquid ratio of graphite powder to hydrochloric acid solution is 1:

8.

5. The method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries according to claim 4, characterized in that: The mass loss of the graphite powder after acid washing in step 2 is 6-8.5%.

6. The method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries according to claim 1, characterized in that: The concentration of the hydrochloric acid solution in step three is 3 mol / l, the reaction temperature is 40°C, the solid-liquid ratio of graphite powder to hydrochloric acid solution is 1:10, the volume ratio of hydrochloric acid, sulfuric acid and hydrogen peroxide is 6:3:1, and the concentration of hydrogen peroxide is 30%; step three is carried out under an ultrasonic environment, the ultrasonic power is 300w, and the ultrasonic time is 20min.

7. The method for regenerating and repairing graphite after wet lithium extraction from waste lithium batteries according to claim 6, characterized in that: The mass loss of the graphite powder after mixed acid washing in step 3 is 4.5%.

Citation Information

Patent Citations

  • Method for recovering and restoring anode material graphite of waste lithium ion battery

    CN101710632A

  • Method for recovering graphite from scrapped lithium ion battery

    CN111072023A

  • Method for recycling and regenerating electrode material from negative electrode of waste lithium battery

    CN116639688A

  • Method for purification and lattice reconstruction of graphite in power battery

    US20210376305A1

Cited By

  • Waste battery graphite-based regenerated active material as well as preparation and application thereof

    CN122370542A