Silicon-carbon negative electrode material and preparation method thereof

By preparing photovoltaic waste silicon into binder-free silicon-carbon anode material, the structural problems and resource waste caused by the volume change of silicon-based materials in lithium-ion batteries are solved, high energy density and cycle stability are achieved, and the cost is reduced. production costs and environmental pollution.

CN118851180AInactive Publication Date: 2024-10-29QINGDAO UNIV

Patent Information

Application Number
CN202411057800.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The energy density of graphite anode materials in existing lithium-ion batteries is insufficient, and the volume change of silicon-based anode materials during the lithium insertion/delithiation process causes structural cracks and powdering, affecting cycle stability and service life. At the same time, photovoltaic silicon waste cannot be effectively utilized, causing resource waste and environmental pollution.

Method used

Using photovoltaic waste silicon as raw material, binder-free silicon-carbon anode materials are prepared through crushing, pickling, alcohol washing, calcination, ball milling and high-pressure electrospinning processes to build a 3D porous carbon network structure to solve the problem of volume expansion and improve battery performance. energy density.

Benefits of technology

It achieves high energy density and improved cycle stability of lithium-ion battery anode materials, solves the problem of structural cracking of silicon-based materials, and reduces production costs and environmental pollution by reusing photovoltaic waste silicon.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851180A_ABST
    Figure CN118851180A_ABST
Patent Text Reader

Abstract

The invention relates to a silicon-carbon negative electrode material and a preparation method thereof, and belongs to the field of new energy materials and energy storage. The method takes photovoltaic waste silicon as a raw material, and comprises the following specific preparation processes: firstly, sequentially carrying out acid pickling and ethanol washing on the photovoltaic waste silicon, then carrying out ball-milling refining, and calcining in an inert atmosphere after ball-milling to obtain submicron silicon powder; the preparation method comprises the following steps: dissolving submicron silicon powder, polyvinylpyrrolidone and polyacrylonitrile in N, N-dimethylformamide according to a certain proportion, and carrying out ball milling and mixing to obtain a spinning solution; performing high-voltage electrostatic spinning to obtain a fiber membrane, and performing high-temperature carbonization on the fiber membrane in an inert atmosphere to obtain the silicon-carbon negative electrode material which can be directly used for the negative electrode of the lithium ion battery. The silicon-carbon negative electrode material prepared by the method has excellent electrochemical performance, and has the characteristic that a binder and a current collector do not need to be used while photovoltaic waste silicon is recycled, so that the production cost is effectively saved, and the actual demand is favorably met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of new energy materials and energy storage, and specifically relates to a silicon-carbon negative electrode material and a preparation method thereof. Background Art

[0002] As the most important energy storage technology since the 21st century, lithium-ion batteries have been deeply used in many fields of modern society, such as electric vehicles, portable electronic devices, medical equipment, etc. In recent years, with the rapid development of various technologies and the replacement of various equipment, the requirements for the energy density of lithium-ion batteries have become higher and higher. However, the theoretical specific capacity of the widely used graphite negative electrode material is only 372 mAh / g, which is increasingly difficult to meet the demand for lithium-ion battery energy density from all walks of life. Therefore, it is urgent to develop a new generation of high-energy-density lithium-ion battery negative electrode materials.

[0003] Theoretically, silicon has an extremely high specific capacity (4200mAh / g), far exceeding the widely used commercial graphite anode, which makes it a key candidate material for improving battery energy density. However, despite its significant theoretical advantages, its practical application faces many challenges. The main problem is the huge volume change (up to 300%-400%) of silicon during the lithium insertion / extraction process. This severe volume effect can lead to structural fracture and pulverization of the active material, as well as repeated fracture and regrowth of the solid electrolyte interface layer (SEI), which in turn affects the cycle stability, energy efficiency and service life of the battery.

[0004] With the development of the new energy industry, the manufacture and use of crystalline silicon solar cells are becoming more and more widespread. In 2023 alone, the global production of photovoltaic-grade polysilicon will reach 1.5 million tons. However, a large amount of silicon waste is generated during the cutting and polishing of photovoltaic silicon wafers. It contains high-purity silicon, accounting for about 40% of the raw materials of silicon wafers, which results in hundreds of thousands of tons of high-purity silicon materials being wasted every year. If these silicon wastes are not treated or treated unreasonably, they will cause a lot of resource waste and environmental pollution. This is the shortcoming of the existing technology.

[0005] In view of this, it is very necessary for the present invention to provide a silicon-carbon negative electrode material and a preparation method thereof to solve the above-mentioned defects existing in the prior art. Summary of the invention

[0006] The purpose of the present invention is to overcome the shortcomings of the prior art by incorporating photovoltaic waste silicon into the design of lithium-ion battery negative electrode materials, and to provide a silicon-carbon negative electrode material and a preparation method thereof. The use of this method to prepare silicon-carbon negative electrode materials using photovoltaic waste silicon as the main raw material can not only solve the problem of photovoltaic waste treatment, reduce the cost of photovoltaic cells, and promote the sustainable use of clean energy, but also solve the problem of structural fragmentation and pulverization caused by volume expansion of silicon-based negative electrodes during lithium extraction and insertion, and at the same time, the characteristics of not needing to use binders and current collectors can greatly improve the energy density of the battery.

[0007] To achieve the above object, the present invention provides the following solutions: The present invention provides a method for preparing a silicon-carbon negative electrode material, comprising the following steps: Step 1) After the photovoltaic waste silicon is initially crushed, it is acid-washed and alcohol-washed in sequence, and after drying, it is calcined in an inert gas atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; Step 2) ball-milling the purified silicon powder to obtain submicron silicon powder; Step 3) ball-milling submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile in N,N-dimethylformamide to obtain a spinning solution, forming the spinning solution into a fiber membrane through a high-voltage electrospinning process, and subjecting the fiber membrane to a high-temperature carbonization treatment under an inert atmosphere to obtain a binder-free silicon-carbon negative electrode material that can be directly used for the negative electrode of a lithium-ion battery.

[0008] The photovoltaic waste silicon described in step 1) is silicon waste generated during the cutting and polishing of silicon wafers in the photovoltaic industry production process. In addition to silicon, it contains impurities of elements such as Fe, Al, O, and N. The photovoltaic waste silicon exists in the form of silicon cakes, which are initially crushed by a crusher and then sieved with a 150-mesh sieve. Too large a particle size will affect the subsequent pickling effect and ball milling.

[0009] The acid solution used in the acid washing in step 1) is an aqueous solution of hydrochloric acid or sulfuric acid with a concentration of 0.1 mol / L to 1.0 mol / L; the alcohol solution used in the alcohol washing is ethanol or methanol.

[0010] In the pickling treatment in step 1), the material-liquid ratio of photovoltaic waste silicon to acid solution is 0.1-1 kg / L.

[0011] In the acid washing treatment described in step 1), the photovoltaic waste silicon is placed in an acid solution and stirred at 200-800 rpm by an electric stirrer for 1-4 hours; after the acid washing, the photovoltaic waste silicon is filtered and washed with deionized water to neutrality, and then washed with an alcohol solution.

[0012] The drying in step 1) is performed in a vacuum drying oven at a drying temperature of 100° C. for a drying time of 10 h.

[0013] The inert gas in step 1) is argon or nitrogen, the calcination time is 1 to 3 hours, and the temperature is 600 to 900°C.

[0014] The acid pickling described in step 1) is to remove inorganic impurities such as iron, aluminum and their oxides remaining in the photovoltaic waste silicon, and the high-temperature calcination under an inert atmosphere is to remove organic impurities in the photovoltaic waste silicon without oxidation of the photovoltaic waste silicon.

[0015] In step 2), the ball milling is wet milling with ethanol as a grinding aid; the ratio of purified photovoltaic waste silicon powder to grinding aid liquid is 0.1-0.5 kg / L; the ball-to-material ratio of ball milling is 10-30:1, the ball milling speed is 300-700 rpm, and the ball milling time is 20-45 h; the particle size of the submicron photovoltaic silicon powder after ball milling is 100-300 nm. If the particle size of the submicron silicon powder after ball milling is too large, it will make it difficult for the silicon particles to enter the carbon nanowires during electrospinning, ultimately resulting in poor battery cycle stability.

[0016] In step 3), the mass ratio of submicron silicon powder to the total weight of polyvinyl pyrrolidone and polyacrylonitrile is 1-4:10; the mass ratio of polyvinyl pyrrolidone to polyacrylonitrile is 1:9-3:7; the mass fraction of polyvinyl pyrrolidone and polyacrylonitrile in N,N-dimethylformamide is 8-15wt%; the ball milling speed of the spinning solution ball milling mixing is 100-300rpm, and the time is 0.5-2h.

[0017] The molecular weights of polyvinyl pyrrolidone and polyacrylonitrile used in step 3) are 1,300,000 and 150,000, respectively.

[0018] In step 3), polyvinyl pyrrolidone is added to improve the dispersibility of submicron silicon powder in the spinning solution, and is spun into fibers simultaneously with polyacrylonitrile; ball milling of the spinning solution is to quickly and efficiently mix the spinning solution, save production time and improve the dispersibility of submicron silicon powder in the spinning solution.

[0019] In step 3), the voltage of the high-voltage electrospinning process is 17-21 kV, the spinning propulsion rate is 0.5-1 ml / h, and the receiving distance is 10-20 cm.

[0020] The inert gas described in step 3) is argon or nitrogen, the carbonization temperature is 700-1000°C, the carbonization time is 1-3h, and the heating rate is 3-10°C / min; the silicon-carbon composite material after carbonization is a composite silicon carbon fiber membrane with certain flexibility, which can be directly applied to the negative electrode of lithium-ion batteries.

[0021] The present invention also provides a silicon-carbon negative electrode material, which is prepared by the above steps and can be directly applied to the negative electrode of a lithium ion battery without using a binder and a current collector.

[0022] Compared with the prior art, the present invention has the following beneficial effects: 1) The present invention converts cheap photovoltaic waste silicon into negative electrode materials for lithium-ion batteries, successfully achieving efficient recycling of waste, solving the problem of photovoltaic waste treatment, reducing environmental pollution, and also effectively reducing the production cost of silicon-carbon negative electrode materials for lithium-ion batteries, thus promoting the sustainable development of the clean energy industry.

[0023] 2) By adopting specific steps to purify and submicronize photovoltaic waste silicon, and at the same time using the electrospinning process to construct a 3D porous carbon network structure that effectively provides strain elasticity for the expansion / contraction of silicon during lithium insertion / delithiation, it effectively solves the structural fragmentation and pulverization problems of silicon-based negative electrode materials caused by volume expansion during charging and discharging, and significantly improves the cycle stability and service life of silicon-carbon negative electrode materials.

[0024] 3) The binder-free silicon-carbon negative electrode material preparation method proposed in the present invention abandons the dependence on binders and current collectors in traditional processes, which not only simplifies the production process, but also reduces the proportion of inactive substances, so that the battery per unit mass or volume can accommodate more active substances, thereby achieving an increase in battery energy density. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.

[0026] Figure 1 .Scanning electron microscope image of the photovoltaic waste silicon raw material used in the present invention.

[0027] Figure 2 .Scanning electron microscope image and particle size distribution diagram of the submicron silicon powder prepared in Example 1 of the present invention.

[0028] Figure 3 .Scanning electron microscope image of the binder-free silicon-carbon negative electrode material prepared in Example 1 of the present invention.

[0029] Figure 4 .A graph showing the capacity of the binder-free silicon-carbon negative electrode material prepared in Example 1 of the present invention as a function of the number of cycles. DETAILED DESCRIPTION

[0030] The following will be a comprehensive and detailed analysis of the technical solution of the present invention by describing the specific embodiments of the present invention. It should be pointed out that the embodiments listed here only constitute a part of all the embodiments of the present invention, not all the embodiments. Any other embodiments derived by ordinary technicians in this field without creative work based on the disclosure of the present invention should be understood to fall within the scope of protection claimed by the present invention.

[0031] Example 1 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.1 mol / L hydrochloric acid solution with a solid-liquid ratio of 0.5 kg / L, use an electric stirrer to stir and react at a speed of 500 rpm for 2 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 700°C in an argon atmosphere for 2 hours to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.2 kg / L, and ball milling for 30 hours at a ball-to-material ratio of 15:1 and a ball milling speed of 500 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 2g, 3g and 7g, and then added to 100g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 200rpm for 1h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 19kV, at a propulsion speed of 0.8ml / h and a collection distance of 15cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 800℃, and the carbonization time was 2h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0032] 4) Preparation of lithium-ion half-cell: The silicon-carbon negative electrode material carbonized in step 3) is directly applied to the lithium-ion half-cell. The entire battery assembly process is completed in a glove box filled with high-purity argon with a water pressure and oxygen pressure of less than 0.1ppm. A CR2016 battery shell is used to assemble the lithium battery, and a porous polypropylene membrane soaked in electrolyte is used as a diaphragm to separate the working electrode and the counter electrode lithium sheet. The electrolyte is composed of 1 mol / L lithium hexafluorophosphate (LiPF6) dissolved in dimethyl carbonate (DMC) and ethylene carbonate (EC) (DMC) (1:1, v / v). After assembly, the battery is pressed using an MSK-110 button battery sealer and placed statically for 4.5 hours before electrochemical testing. The test results were obtained using the Blue Power Battery Test System CT2001A. At a current density of 1.0 A / g, its initial discharge capacity was 1318.8 mAh / g. After 90 cycles, its capacity could still reach 823.6 mAh / g, demonstrating its high capacity and cycle stability at high current density.

[0033] Example 2 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.5 mol / L sulfuric acid solution with a solid-liquid ratio of 0.1 kg / L, use an electric stirrer to stir and react at a speed of 200 rpm for 4 hours, and after the reaction, use a vacuum filtration device to filter out the photovoltaic waste silicon, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous methanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 600°C for 2 hours in an argon atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.1 kg / L, and ball milling for 20 hours at a ball-to-material ratio of 10:1 and a ball milling speed of 700 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 3g, 2g and 8g, and then added to 100g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 100rpm for 2h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 21kV, at a propulsion speed of 1ml / h and a collection distance of 18cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 900℃, and the carbonization time was 1.5h. After the carbonization was completed, a binder-free silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0034] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1657.2 mAh / g, and after 90 cycles, its capacity can still reach 954.3 mAh / g, showing high capacity and cycle stability at high current density.

[0035] Example 3 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 1 mol / L hydrochloric acid solution with a material-liquid ratio of 0.2 kg / L, use an electric stirrer to stir and react at a speed of 800 rpm for 1 hour, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 600°C in an argon atmosphere for 1.5 hours to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.5 kg / L, and ball milling for 20 hours at a ball-to-material ratio of 20:1 and a ball milling speed of 400 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 1g, 1g and 9g, and then added to 90g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 300rpm for 0.5h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 17kV, at a propulsion speed of 1ml / h and a collection distance of 10cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 1000℃, and the carbonization time was 1.5h. After the carbonization was completed, a binder-free silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0036] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1089.4 mAh / g, and after 90 cycles, its capacity can still reach 711.6 mAh / g, showing high capacity and cycle stability at high current density.

[0037] Example 4 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.5 mol / L hydrochloric acid solution with a material-liquid ratio of 1 kg / L, use an electric stirrer to stir and react at a speed of 600 rpm for 3 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 900°C for 1 hour in an argon atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.4 kg / L, and ball milling for 20 hours at a ball-to-material ratio of 30:1 and a ball milling speed of 700 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 2g, 2g and 8g, and then added to 120g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 100rpm for 2h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 20kV, at a propulsion speed of 0.6ml / h and a collection distance of 16cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 800℃, and the carbonization time was 2h. After the carbonization was completed, a binder-free silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0038] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1289.7 mAh / g, and after 90 cycles, its capacity can still reach 789.6 mAh / g, showing high capacity and cycle stability at high current density.

[0039] Example 5 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.6 mol / L sulfuric acid solution with a material-liquid ratio of 0.3 kg / L, use an electric stirrer to stir and react at a speed of 300 rpm for 3 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous methanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 800°C for 2 hours in a nitrogen atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.2 kg / L, and ball milling for 25 hours at a ball-to-material ratio of 20:1 and a ball milling speed of 600 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 3g, 2g and 8g, and then added to 130g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 100rpm for 2h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 21kV, at a propulsion speed of 0.7ml / h and a collection distance of 15cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 800℃, and the carbonization time was 2h. After the carbonization was completed, a binder-free silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0040] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1308.4 mAh / g, and after 90 cycles, its capacity can still reach 801.6 mAh / g, showing high capacity and cycle stability at high current density.

[0041] Example 6 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 1 mol / L hydrochloric acid solution with a solid-liquid ratio of 1 kg / L, use an electric stirrer to stir and react at a speed of 800 rpm for 4 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 900°C for 3 hours in a nitrogen atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.5 kg / L, and ball milling for 45 hours at a ball-to-material ratio of 30:1 and a ball milling speed of 700 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 4g, 3g and 7g, and then added to 95g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 300rpm for 2h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 21kV, at a propulsion speed of 1.0ml / h and a collection distance of 20cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in a nitrogen atmosphere, the carbonization temperature was 1000℃, and the carbonization time was 3h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0042] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1207.6 mAh / g, and after 90 cycles, its capacity can still reach 784.0 mAh / g, showing high capacity and cycle stability at high current density.

[0043] Example 7 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.1 mol / L sulfuric acid solution with a material-liquid ratio of 0.1 kg / L, use an electric stirrer to stir and react at a speed of 200 rpm for 1 hour, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous methanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 600°C for 1 hour in an argon atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.1 kg / L, and ball milling for 20 hours at a ball-to-material ratio of 10:1 and a ball milling speed of 300 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 1g, 1g and 9g, and then added to 135g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 100rpm for 0.5h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 17kV, at a propulsion speed of 0.5ml / h and a collection distance of 10cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 700℃, and the carbonization time was 1h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0044] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1179.3 mAh / g, and after 90 cycles, its capacity can still reach 695.6 mAh / g, showing high capacity and cycle stability at high current density.

[0045] Example 8 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.8 mol / L sulfuric acid solution with a solid-liquid ratio of 0.4 kg / L, use an electric stirrer to stir and react at a speed of 700 rpm for 2 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 800°C for 1 hour in a nitrogen atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.3 kg / L, and ball milling for 30 hours at a ball-to-material ratio of 15:1 and a ball milling speed of 700 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 4g, 2g and 8g, and then added to 120g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 200rpm for 1h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 20kV, at a propulsion speed of 1ml / h and a collection distance of 15cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 800℃, and the carbonization time was 2h. After the carbonization was completed, a binder-free silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0046] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1279.5 mAh / g, and after 90 cycles, its capacity can still reach 754.3 mAh / g, showing high capacity and cycle stability at high current density.

[0047] Example 9 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.2 mol / L hydrochloric acid solution with a solid-liquid ratio of 0.4 kg / L, use an electric stirrer to stir and react at a speed of 600 rpm for 3 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 650°C for 1 hour in an argon atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.4 kg / L, and ball milling for 20 hours at a ball-to-material ratio of 30:1 and a ball milling speed of 700 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 3g, 3g and 7g, and then added to 110g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 200rpm for 2h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 20kV, at a propulsion speed of 0.5ml / h and a collection distance of 18cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 900℃, and the carbonization time was 2h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0048] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1307.6 mAh / g, and after 90 cycles, its capacity can still reach 767.3 mAh / g, showing high capacity and cycle stability at high current density.

[0049] Example 10 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.5 mol / L sulfuric acid solution with a solid-liquid ratio of 0.5 kg / L, use an electric stirrer to stir and react at a speed of 500 rpm for 2 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous methanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 800°C for 1 hour in an argon atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.5 kg / L, and ball-milling for 27 hours at a ball-to-material ratio of 20:1 and a ball milling speed of 500 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 4 g, 1 g and 9 g, and then added to 130 g of N, N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 100 rpm for 2 h to make it evenly mixed; high-voltage electrospinning was performed under a high voltage of 19 kV, at a propulsion speed of 1.0 ml / h and a collection distance of 15 cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 800°C, and the carbonization time was 2 h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0050] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1315.6 mAh / g, and after 90 cycles, its capacity can still reach 795.6 mAh / g, showing high capacity and cycle stability at high current density.

[0051] Embodiment 11 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.6 mol / L hydrochloric acid solution with a solid-liquid ratio of 0.4 kg / L, use an electric stirrer to stir and react at a speed of 600 rpm for 2.5 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 900°C for 2 hours in a nitrogen atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.4 kg / L, and ball-milling for 30 hours at a ball-to-material ratio of 25:1 and a ball milling speed of 600 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 3g, 2g and 8g, and then added to 125g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 100rpm for 2h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 20kV, at a propulsion speed of 0.9ml / h and a collection distance of 16cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 900℃, and the carbonization time was 3h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0052] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1279.7 mAh / g, and after 90 cycles, its capacity can still reach 758.9 mAh / g, showing high capacity and cycle stability at high current density.

[0053] Example 12 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.7 mol / L hydrochloric acid solution with a solid-liquid ratio of 0.3 kg / L, use an electric stirrer to stir the reaction at a speed of 700 rpm for 3.0 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous methanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 900°C for 2 hours in an argon atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.3 kg / L, and ball-milling for 40 hours at a ball-to-material ratio of 30:1 and a ball milling speed of 700 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 4g, 3g and 7g, and then added to 110g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 200rpm for 0.5h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 21kV, at a propulsion speed of 0.9ml / h and a collection distance of 16cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 1000℃, and the carbonization time was 3h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0054] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1358.7 mAh / g, and after 90 cycles, its capacity can still reach 806.9 mAh / g, showing high capacity and cycle stability at high current density.

[0055] Example 13 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.8 mol / L hydrochloric acid solution with a solid-liquid ratio of 0.3 kg / L, use an electric stirrer to stir and react at a speed of 800 rpm for 3.5 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 600°C for 3 hours in a nitrogen atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.2 kg / L, and ball-milling for 25 hours at a ball-to-material ratio of 10:1 and a ball milling speed of 400 rpm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 1g, 1g and 9g, and then added to 120g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 200rpm for 2h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 21kV, at a propulsion speed of 0.8ml / h and a collection distance of 17cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 800℃, and the carbonization time was 2h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0056] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1406.2 mAh / g, and after 90 cycles, its capacity can still reach 748.5 mAh / g, showing high capacity and cycle stability at high current density.

[0057] Embodiment 14 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.9 mol / L sulfuric acid solution with a material-liquid ratio of 0.2 kg / L, use an electric stirrer to stir and react at a speed of 300 rpm for 4 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 600°C for 3 hours in an argon atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.1 kg / L, and ball-milling for 30 hours at a ball-to-material ratio of 15:1 and a ball-milling speed of 300 pm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 4g, 1g and 9g, and then added to 120g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 300rpm for 0.5h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 17kV, at a propulsion speed of 0.7ml / h and a collection distance of 18cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 800℃, and the carbonization time was 2h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0058] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1287.7 mAh / g, and after 90 cycles, its capacity can still reach 794.1 mAh / g, showing high capacity and cycle stability at high current density.

[0059] Embodiment 15 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 1.0 mol / L hydrochloric acid solution with a solid-liquid ratio of 0.1 kg / L, use an electric stirrer to stir and react at a speed of 350 rpm for 3 hours, and after the reaction, use a vacuum filtration device to filter out the photovoltaic waste silicon, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 700°C in an argon atmosphere for 2.5 hours to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.5 kg / L, and ball-milling for 35 hours at a ball-to-material ratio of 20:1 and a ball milling speed of 500 pm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 4g, 2g and 8g, and then added to 110g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 300rpm for 0.5h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 18kV, at a propulsion speed of 0.6ml / h and a collection distance of 19cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 700℃, and the carbonization time was 2.5h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0060] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1249.8 mAh / g, and after 90 cycles, its capacity can still reach 749.2 mAh / g, showing high capacity and cycle stability at high current density.

[0061] Example 16 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.1 mol / L sulfuric acid solution with a material-liquid ratio of 1.0 kg / L, use an electric stirrer to stir and react at a speed of 400 rpm for 2 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous methanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 800°C for 2 hours in a nitrogen atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.4 kg / L, and ball-milling for 40 hours at a ball-to-material ratio of 25:1 and a ball milling speed of 600 pm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 1g, 2g and 8g, and then added to 110g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 300rpm for 1h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 19kV, at a propulsion speed of 0.8ml / h and a collection distance of 10cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in a nitrogen atmosphere, the carbonization temperature was 750℃, and the carbonization time was 3h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0062] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1305.5 mAh / g, and after 90 cycles, its capacity can still reach 766.0 mAh / g, showing high capacity and cycle stability at high current density.

[0063] Embodiment 17 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.2 mol / L hydrochloric acid solution with a solid-liquid ratio of 0.9 kg / L, use an electric stirrer to stir and react at a speed of 450 rpm for 3 hours, and after the reaction, use a vacuum filtration device to filter out the photovoltaic waste silicon, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 600°C in an argon atmosphere for 2.5 hours to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.3 kg / L, and ball-milling for 45 hours at a ball-to-material ratio of 30:1 and a ball-milling speed of 700 pm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 2g, 3g and 7g, and then added to 120g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 100rpm for 2h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 20kV, at a propulsion speed of 0.7ml / h and a collection distance of 12cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 800℃, and the carbonization time was 1h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0064] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1297.1 mAh / g, and after 90 cycles, its capacity can still reach 728.7 mAh / g, showing high capacity and cycle stability at high current density.

[0065] Embodiment 18 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.3 mol / L hydrochloric acid solution with a solid-liquid ratio of 0.8 kg / L, use an electric stirrer to stir and react at a speed of 500 rpm for 4 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous methanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 900°C for 3 hours in an argon atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.2 kg / L, and ball-milling for 30 hours at a ball-to-material ratio of 15:1 and a ball milling speed of 500 pm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 3g, 1g and 9g, and then added to 110g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 200rpm for 2h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 21kV, at a propulsion speed of 0.6ml / h and a collection distance of 18cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 850℃, and the carbonization time was 1.5h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0066] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1367.0 mAh / g, and after 90 cycles, its capacity can still reach 796.2 mAh / g, showing high capacity and cycle stability at high current density.

[0067] Embodiment 19 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.4 mol / L sulfuric acid solution with a solid-liquid ratio of 0.6 kg / L, use an electric stirrer to stir and react at a speed of 550 rpm for 2 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous ethanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 850°C for 1.5 hours in a nitrogen atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.1 kg / L, and ball-milling for 25 hours at a ball-to-material ratio of 20:1 and a ball milling speed of 300 pm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 4 g, 1 g and 9 g, and then added to 130 g of N, N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 300 rpm for 2 h to make it evenly mixed; high-voltage electrospinning was performed under a high voltage of 20 kV, at a propulsion speed of 0.8 ml / h and a collection distance of 20 cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in a nitrogen atmosphere, the carbonization temperature was 900°C, and the carbonization time was 2 h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0068] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1297.5 mAh / g, and after 90 cycles, its capacity can still reach 742.3 mAh / g, showing high capacity and cycle stability at high current density.

[0069] Embodiment 20 1) Use a pulverizer to crush the photovoltaic waste silicon cake, and then use a 150-mesh sieve to sieve it, and crush the unsieved photovoltaic waste silicon again until it is completely sieved; dissolve the sieved photovoltaic waste silicon powder in a 0.5 mol / L sulfuric acid solution with a solid-liquid ratio of 0.4 kg / L, use an electric stirrer to stir and react at a speed of 700 rpm for 3 hours, and use a vacuum filtration device to filter out the photovoltaic waste silicon after the reaction, and use deionized water to wash it three times until the photovoltaic waste silicon suspension is neutral, and then use anhydrous methanol to wash it twice; after the alcohol washing is completed, use a vacuum drying oven to vacuum dry it at 100°C for 10 hours, and after drying, use a vacuum tube furnace to calcine at 650°C for 1 hour in an argon atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; 2) adding anhydrous ethanol to the purified silicon powder prepared in step 1) at a material-liquid ratio of 0.5 kg / L, and ball-milling for 30 hours at a ball-to-material ratio of 25:1 and a ball-milling speed of 400 pm to obtain submicron silicon powder; 3) Submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile were mixed in masses of 2g, 3g and 7g, and then added to 100g of N,N-dimethylformamide to prepare a spinning solution, and the spinning solution was ball-milled at a speed of 250rpm for 2h to make it evenly mixed; high-voltage electrospinning was carried out under a high voltage of 19kV, at a propulsion speed of 1.0ml / h and a collection distance of 15cm to make the spinning solution into a fiber membrane; the fiber membrane was subjected to high-temperature carbonization treatment in an argon atmosphere, the carbonization temperature was 1000℃, and the carbonization time was 2.5h. After the carbonization was completed, a silicon-carbon negative electrode material based on photovoltaic silicon cutting waste was obtained.

[0070] 4) The preparation and performance testing methods of the lithium ion half-cell are the same as those in Example 1. The results are as follows: at a current density of 1.0 A / g, its initial discharge capacity is 1375.9 mAh / g, and after 90 cycles, its capacity can still reach 784.4 mAh / g, showing high capacity and cycle stability at high current density.

[0071] The present invention also provides a silicon-carbon negative electrode material, which is prepared by the steps of the above embodiments. The silicon-carbon negative electrode material can be directly applied to the negative electrode of a lithium-ion battery without using a binder and a current collector.

[0072] Comparative Example 1 Same as Example 1, except that the polyvinyl pyrrolidone used in step 3) is replaced by polyacrylonitrile of the same mass; the test results are: at a current density of 1.0 A / g, its initial discharge capacity is 1254.6 mAh / g, and after 90 cycles, its capacity is 675.6 mAh / g. Comparative Example 2 The same as Example 1, except that the operation of ball milling the spinning solution to make it uniformly mixed in step 3) is changed to magnetic stirring the spinning solution at a rotation speed of 500 rpm for 12 hours, and then ultrasonically treating the spinning solution at a power of 100 W for 20 minutes; the test results are: at a current density of 1.0 A / g, its first discharge capacity is 1308.2 mAh / g, and its capacity after 90 cycles is 729.3 mAh / g.

Claims

1. A method for preparing a silicon-carbon negative electrode material, characterized in that: The following steps are involved: Step 1) After the photovoltaic waste silicon is initially crushed, it is acid-washed and alcohol-washed in sequence, and after drying, it is calcined in an inert gas atmosphere to remove impurities in the photovoltaic waste silicon powder to obtain purified silicon powder; Step 2) ball-milling the purified silicon powder to obtain submicron silicon powder; Step 3) ball-milling submicron silicon powder, polyvinyl pyrrolidone and polyacrylonitrile in N,N-dimethylformamide to obtain a spinning solution, forming the spinning solution into a fiber membrane through a high-voltage electrospinning process, and subjecting the fiber membrane to a high-temperature carbonization treatment under an inert atmosphere to obtain a silicon-carbon negative electrode material that can be directly used for the negative electrode of a lithium-ion battery.

2. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: The acid used in the acid washing in step 1) is a hydrochloric acid solution or a sulfuric acid solution with a concentration of 0.1 mol / L to 1.0 mol / L; the alcohol solution used in the alcohol washing is ethanol or methanol.

3. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: The inert gas in step 1) is argon or nitrogen, the calcination time is 1 to 3 hours, and the calcination temperature is 600 to 900°C.

4. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: In step 2), the ball milling speed during ball milling is 300-700 rpm, and the ball milling time is 20-45 hours; the particle size distribution of the obtained submicron silicon powder is 100-300 nm.

5. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: In step 3), the mass ratio of submicron silicon powder to the total weight of polyvinyl pyrrolidone and polyacrylonitrile is 1 to 4:10; the mass ratio of polyvinyl pyrrolidone to polyacrylonitrile is 1:9 to 3:

7.

6. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: In step 3), the mass fraction of polyvinyl pyrrolidone and polyacrylonitrile in N,N-dimethylformamide is 8-15wt%; the spinning solution is ball-milled at a speed of 100-300rpm for 0.5-2h.

7. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: The voltage of the high-voltage electrospinning process in step 3) is 17-21 kV, the spinning propulsion rate is 0.5-1 ml / h, and the receiving distance is 10-20 cm.

8. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: The inert gas in step 3) is argon or nitrogen, the carbonization temperature is 700-1000° C., and the carbonization time is 1-3 hours.

9. A silicon-carbon negative electrode material prepared by the method according to any one of claims 1 to 8, characterized in that: It can be directly applied to the negative electrode of lithium-ion batteries without the use of binders and current collectors.

Citation Information

Patent Citations

  • Silicon carbon anode material based on photovoltaic waste silicon and preparation method thereof

    CN110474032A

  • Preparation method of Si / SiC / C nanofiber membrane, battery negative electrode and lithium ion battery

    CN113097469A

  • Silicon-carbon interlocking flexible self-supporting negative electrode material, preparation method and application

    CN114204000A

Cited By

  • Lithium-intercalated silicon carbon material, preparation method thereof and application of lithium-intercalated silicon carbon material in lithium ion battery

    CN120767318A