Preparation method of high-first-effect sanding silicon-carbon negative electrode material

By sanding micron silicon in the lithium battery anode material and dispersing polymerized magnesium oxide and graphite in a disperser to form an MgSiO3 layer, the side reaction problem caused by the volume expansion and fragmentation of micron silicon is solved, significantly improving the quality of silicon carbon anode materials. efficiency and electrochemical performance.

CN118851189APending Publication Date: 2024-10-29XUANCHENG SILIKO NEW MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410936468.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The micron silicon in existing lithium battery anode materials is broken due to volume expansion, forming an exposed interface and side reactions with the dispersion medium, which reduces the first effect of the silicon-carbon anode composite material and limits its large-scale application.

Method used

Micron silicon is sanded in an organic medium to obtain nano silicon, and the polymerized magnesium oxide and graphite are evenly dispersed in a high-speed disperser to form an MgSiO3 layer. The dispersion and dielectric constant of MgO are improved through the polymerization of dopamine monomers, and combined with high-temperature roasting to prepare high-temperature polymers. The first effective silicon carbon anode material.

Benefits of technology

The presence of the MgSiO3 layer reduces the proportion of the dead phase, improves the first efficiency of the silicon-carbon anode material, and improves the dispersion of MgO through dopamine polymerization, significantly improving the electrochemical performance of the material.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a sanding silicon-carbon negative electrode material of a lithium battery, in particular to a preparation method of a high-first-efficiency sanding silicon-carbon negative electrode material, which comprises the following steps: sanding micron silicon in an organic medium to obtain nano silicon; uniformly dispersing polymerized magnesium oxide in nano silicon in a high-speed dispersion machine; uniformly dispersing nano silicon-magnesium oxide, graphite and an organic carbon source in a high-speed dispersion machine; carrying out spray drying; and roasting in a carbonization furnace at a high temperature of 800-1200 DEG C. According to the invention, the MgSiO3 layer exists between the nanometer silicon and the carbon layer formed by splitting decomposition of the organic matter, and the existence of the MgSiO3 layer can change the SiO2 phase into a passivation layer, so that the proportion of the formed deadline phase is reduced, and the first effect of the silicon-carbon negative electrode is further improved. Meanwhile, the dopamine monomer and MgO are polymerized, and polydopamine is polymerized on the surface of MgO to form and introduce an active functional group, so that the dielectric constant of MgO is improved, the dispersity of MgO is greatly improved, and an MgSiO3 layer can be more effectively formed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a sand-ground silicon-carbon negative electrode material for a lithium battery, in particular to a preparation method of a sand-ground silicon-carbon negative electrode material with high initial efficiency. Background Art

[0002] At present, the negative electrode material of lithium batteries is mainly graphite, but with the rapid development of the new energy industry, the graphite negative electrode with lower theoretical capacity has been difficult to meet the needs of the industry. Silicon negative electrode has been increasingly concerned by the industry due to its high theoretical capacity, but micron silicon has a large volume expansion, which greatly limits its application. In response to this, the academic and industrial circles have developed sand-milled nano-silicon and dispersed it on the surface of graphite for carbon coating to prepare silicon-carbon negative electrode composite materials. However, during the sand-milling process, micron silicon is constantly broken to form a new exposed interface, which causes silicon to react with the dispersion medium to form a silicon dioxide layer, which makes the prepared silicon-carbon negative electrode composite material have a lower initial efficiency, thus limiting its large-scale application. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a high initial-effect sand-milled silicon-carbon negative electrode material to solve the problems raised in the above-mentioned background technology.

[0004] To achieve the above object, the present invention provides the following technical solutions:

[0005] A method for preparing a high initial efficiency sand-ground silicon-carbon negative electrode material comprises the following steps:

[0006] Step 1: Grind micron silicon in an organic medium to obtain nano silicon;

[0007] Step 2: Disperse the polymerized magnesium oxide evenly in the nano-silicon in a high-speed disperser;

[0008] Step 3: Evenly disperse nano silicon-magnesium oxide, graphite and organic carbon source in a high-speed disperser;

[0009] Step 4: spray drying;

[0010] Step 5: Calcine at 800-1200℃ in a carbonization furnace.

[0011] The reaction between polymerized magnesium oxide and nano-silicon is as follows: MgO+SiO2=MgSiO3.

[0012] As a preferred embodiment of the present invention, the preparation method of the polymerized magnesium oxide is as follows: immersing magnesium oxide particles in a solution containing dopamine monomer, stirring continuously for 1-2 hours under ice water bath conditions to obtain a mixed dispersed solution, heating the mixed dispersed solution to 35-38°C, controlling the pH value to 8.5 and stirring for 5-6 hours, obtaining a precipitate, washing, drying, and grinding to less than 50um to obtain polymerized magnesium oxide powder.

[0013] As a preferred embodiment of the present invention, the mass ratio of the magnesium oxide particles to the dopamine monomer is 23-26:1.

[0014] As a preferred embodiment of the present invention, the Dv50 of the micron silicon in Step 1 is 1-20 um.

[0015] As a preferred embodiment of the present invention, the sand grinding in Step 1 adopts a sand grinder, and the grinding time is 5-20 hours.

[0016] As a preferred embodiment of the present invention, the organic carbon source in Step 3 is one or more of asphalt, resin, glucose and sucrose.

[0017] As a preferred embodiment of the present invention, the dispersing time of the high-speed disperser in Step 3 is 1-5h.

[0018] As a preferred embodiment of the present invention, the organic medium in Step 1 includes alcohol, isopropanol, ethylene glycol, and acetone, and the solid content of the slurry is between 3-30wt% after the medium is added.

[0019] As a preferred embodiment of the present invention, the mass ratio of the polymerized magnesium oxide to the nano-silicon in Step 2 is 1-5wt%.

[0020] As a preferred embodiment of the present invention, the mass ratio of graphite to nano-silicon in Step 3 is 0.5-3:1, and the organic carbon source accounts for 6-18wt% of the mass of the nano-silicon.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] In the present invention, there is a MgSiO3 layer between the nano-silicon and the carbon layer formed by the decomposition of organic matter. The presence of this MgSiO3 layer can make the SiO2 phase transform into a passivation layer, reduce the proportion of the dead phase formed, and thus improve the primary effect of the silicon-carbon negative electrode. At the same time, through the polymerization of dopamine monomer and MgO, polydopamine is polymerized on the surface of MgO to form an active functional group, improve its dielectric constant, greatly improve the dispersibility of MgO, and can more effectively form a MgSiO3 layer. DETAILED DESCRIPTION

[0023] The technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention. In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are conventional methods in the art unless otherwise specified.

[0024] The preparation method of the polymerized magnesium oxide used in the following embodiments of the present invention is as follows: 250 g of magnesium oxide particles are immersed in 1000 mL of a solution containing 10 g of dopamine monomer, and the mixture is stirred for 1.5 h in an ice-water bath to obtain a mixed dispersed solution. The mixed dispersed solution is heated to 36° C., the pH value is controlled to be 8.5 and stirred for 5 h. The precipitate is washed, dried, and ground to less than 50 um to obtain polymerized magnesium oxide powder.

[0025] Example 1

[0026] (1) Add micron silicon with a Dv50 of 15 μm into a high-speed disperser, and add alcohol so that the solid content of the slurry is 5 wt%;

[0027] (2) grinding with a sand mill for 12 hours to obtain nano-silicon;

[0028] (3) Adding 1 wt% of nano-silicon to a high-speed disperser and dispersing at high speed for 1 hour;

[0029] (4) adding graphite at a ratio of 2 times that of nano-silicon to a high-speed disperser, and adding asphalt at a ratio of 8 wt % of nano-silicon;

[0030] (5) High-speed dispersion for 3 h and spray drying;

[0031] (6) Carry out carbonization roasting at 1050°C in a carbonization furnace for 2 h;

[0032] (7) Cool naturally and discharge the material to obtain silicon-carbon negative electrode material 1.

[0033] Example 2

[0034] (1) Add micron silicon with a Dv50 of 15 μm into a high-speed disperser, and add a certain amount of isopropanol so that the solid content of the slurry is 5 wt%;

[0035] (2) grinding with a sand mill for 12 hours to obtain nano-silicon;

[0036] (3) Adding 2 wt% of nano-silicon to a high-speed disperser and dispersing at high speed for 1 hour;

[0037] (4) adding graphite at a ratio of 2 times that of nano-silicon to a high-speed disperser, and adding resin at a ratio of 6 wt % of nano-silicon;

[0038] (5) High-speed dispersion for 3 h and spray drying;

[0039] (6) Carry out carbonization roasting at 1050°C in a carbonization furnace for 2 h;

[0040] (7) Cool naturally and discharge the material to obtain silicon-carbon negative electrode material 2.

[0041] Example 3

[0042] (1) Add micron silicon with a Dv50 of 15 μm into a high-speed disperser, and add a certain amount of alcohol so that the solid content of the slurry is 5 wt%;

[0043] (2) grinding with a sand mill for 12 hours to obtain nano-silicon;

[0044] (3) Adding 5 wt% of nano-silicon to a high-speed disperser and dispersing at high speed for 1 hour;

[0045] (4) adding graphite at a ratio of 2 times that of nano-silicon to a high-speed disperser, and adding asphalt at a ratio of 5wt% of nano-silicon;

[0046] (5) High-speed dispersion for 3 h and spray drying;

[0047] (6) Carry out carbonization roasting at 1050°C in a carbonization furnace for 2 h;

[0048] (7) cooling naturally and discharging the material to obtain the silicon-carbon negative electrode material 3;

[0049] Comparative Example 1

[0050] (1) Add micron silicon with a Dv50 of 15 μm into a high-speed disperser, and add a certain amount of alcohol so that the solid content of the slurry is 5 wt%;

[0051] (2) grinding with a sand mill for 12 hours to obtain nano-silicon;

[0052] (3) adding graphite at a ratio of 2 times that of nano-silicon to a high-speed disperser, and adding asphalt at a ratio of 5wt% of nano-silicon;

[0053] (4) High-speed dispersion for 3 h and spray drying;

[0054] (5) Carry out carbonization roasting at 1050°C in a carbonization furnace for 2 h;

[0055] (6) Cool naturally and discharge the material to obtain the silicon-carbon negative electrode material 4.

[0056] Comparative Example 2

[0057] (1) Add micron silicon with a Dv50 of 15 μm into a high-speed disperser, and add a certain amount of alcohol so that the solid content of the slurry is 5 wt%;

[0058] (2) Grinding with a sand mill for 12 hours;

[0059] (3) Add MgO with a nano-silicon ratio of 5 wt% into a high-speed disperser and disperse at high speed for 1 hour;

[0060] (4) adding graphite at a ratio of 2 times that of nano-silicon to a high-speed disperser, and adding asphalt at a ratio of 5wt% of nano-silicon;

[0061] (5) High-speed dispersion for 3 h and spray drying;

[0062] (6) Carry out carbonization roasting at 1050°C in a carbonization furnace for 2 h;

[0063] (7) Cool naturally and discharge the material to obtain the silicon-carbon negative electrode material 5.

[0064] The silicon-carbon negative electrode materials 1-5 were tested for 0.1C gram capacity and their first efficiency, and the test results are shown in the following table:

[0065] serial number 0.1C gram capacity (mAh / g) First effect (%) Example 1 1460 83.7 Example 2 1410 85.4 Example 3 1370 91.3 Comparative Example 1 1480 80.1 Comparative Example 2 1420 81.3

[0066] It is not difficult to see from the data in the table that as the proportion of polymerized magnesium oxide increases, the proportion of MgSiO3 formed after calcination increases, thereby improving the initial effect of the silicon-carbon negative electrode material. However, the effect of magnesium oxide that has not been polymerized with dopamine is significantly reduced.

[0067] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited by the above embodiments. The above embodiments and descriptions are only preferred examples of the present invention and are not intended to limit the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a high initial efficiency sand-milled silicon-carbon negative electrode material, It is characterized in that The steps include: Step 1: Grind micron silicon in an organic medium to obtain nano silicon; Step 2: Disperse the polymerized magnesium oxide evenly in the nano-silicon in a high-speed disperser; Step 3: Evenly disperse nano silicon-magnesium oxide, graphite and organic carbon source in a high-speed disperser; Step 4: spray drying; Step 5: Calcine at 800-1200℃ in a carbonization furnace.

2. The method for preparing the high initial efficiency sand-ground silicon-carbon negative electrode material according to claim 1, Features: The preparation method of the polymerized magnesium oxide is as follows: immersing magnesium oxide particles in a solution containing dopamine monomers, stirring continuously for 1-2 hours under ice-water bath conditions to obtain a mixed dispersed solution, heating the mixed dispersed solution to 35-38° C., controlling the pH value to 8.5 and stirring for 5-6 hours, washing and drying the precipitate, and grinding it to less than 50 um to obtain polymerized magnesium oxide powder.

3. The method for preparing the high initial efficiency sand-ground silicon-carbon negative electrode material according to claim 2, Features: The mass ratio of the magnesium oxide particles to the dopamine monomer is 23-26:

1.

4. The method for preparing the high initial efficiency sand-ground silicon-carbon negative electrode material according to claim 1, Features: The Dv50 of the micron silicon in Step 1 is 1-20 um.

5. The method for preparing the high initial efficiency sand-ground silicon-carbon negative electrode material according to claim 1, Features: The sand grinding in Step 1 uses a sand grinder, and the grinding time is 5-20 hours.

6. The method for preparing the high initial efficiency sand-ground silicon-carbon negative electrode material according to claim 1, Features: The organic carbon source in Step 3 is one or more of asphalt, resin, glucose and sucrose.

7. The method for preparing the high initial efficiency sand-ground silicon-carbon negative electrode material according to claim 1, Features: The dispersion time of the high-speed disperser in Step 3 is 1-5 hours.

8. The method for preparing the high initial efficiency sand-ground silicon-carbon negative electrode material according to claim 1, Features: The organic medium in Step 1 includes alcohol, isopropanol, ethylene glycol, and acetone. After the medium is added, the solid content of the slurry is between 3-30wt%.

9. The method for preparing the high initial efficiency sand-ground silicon-carbon negative electrode material according to claim 1, Features: The mass ratio of the polymerized magnesium oxide in the step 2 to the nano-silicon is 1-5wt%.

10. The method for preparing the high initial efficiency sand-ground silicon-carbon negative electrode material according to claim 1, Features: The mass ratio of graphite to nano-silicon in Step 3 is 0.5-3:1, and the organic carbon source accounts for 6-18wt% of the mass of the nano-silicon.

Citation Information

Patent Citations

  • Method for preparing silicon-carbon negative electrode by combining sanding with spray drying

    CN117199264A

  • A noiseproof structure for a cooling tower

    KR102210939B1