Ternary lithium positive electrode target material of thin-film lithium battery, preparation method and thin-film lithium battery
Through ball milling and molding of mixed powders of lithium salt, cobalt tetroxide, nickel oxide, zirconium oxide and other materials, combined with multi-stage sintering and annealing treatments, the problem of insufficient research on cathode targets for all-solid-state thin-film lithium batteries was solved, and excellent thin-film lithium batteries were prepared Ternary lithium cathode target improves battery safety and capacity retention.
Patent Information
- Application Number
- CN202310475794.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-26
- Publication Date
- 2024-10-29
AI Technical Summary
In the existing technology, there is little research on cathode targets for all-solid-state thin film lithium batteries, and it is difficult to provide cathode targets with excellent performance, which affects the overall performance of lithium batteries.
The mixed powder of lithium salt, cobalt tetroxide, nickel oxide and zirconium oxide is ball milled and molded, combined with multi-stage sintering and annealing treatments to prepare a uniform, segregation-free ternary lithium cathode target for thin film lithium batteries.
It achieves the composition uniformity and grain consistency of the ternary lithium cathode target for thin film lithium batteries, improves the safety and capacity retention rate of lithium batteries, facilitates subsequent machining, and supports the expansion and boosting of battery packs.
Smart Images

Figure CN118851284A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium batteries, and in particular to a ternary lithium positive electrode target material for a thin-film lithium battery, a preparation method and a thin-film lithium battery. Background Art
[0002] At present, all-solid-state thin-film lithium batteries, as another development direction of lithium batteries, have the advantages of high power density, low self-discharge rate, excellent charge and discharge cycle performance, arbitrary design of shape and size, no solution leakage, no explosion, and safe use. They have received extensive attention at home and abroad in recent years. However, there are few studies on the positive electrode target materials of all-solid-state thin-film lithium batteries. How to provide a positive electrode target material with excellent performance for all-solid-state thin-film lithium batteries is still an urgent problem to be solved. Summary of the invention
[0003] In view of the above situation, the present invention aims to provide a preparation technology and application of a ternary lithium positive electrode target material for a thin-film lithium battery. The present invention can provide a ternary lithium positive electrode target material for an all-solid-state thin-film lithium battery.
[0004] The purpose of the present invention is mainly achieved through the following technical solutions:
[0005] In one aspect, the present invention provides a method for preparing a ternary lithium cathode target material for a thin-film lithium battery, comprising the following steps:
[0006] Step 1, mixing lithium salt powder with cobalt tetroxide, manganese dioxide and nickel oxide powder to obtain a mixed powder; the mass ratio of lithium salt, cobalt tetroxide, manganese dioxide and nickel oxide is 10-12:18-21:18-21:45-48;
[0007] Step 2, putting the mixed powder into a ball mill and mixing it with zirconium oxide balls, and then adding a dispersant to continue mixing and ball milling;
[0008] Step 3, then add a binder into the ball mill and continue ball milling;
[0009] Step 4: The ball-milled synthetic powder is sieved through a 500-mesh sieve. The sieved synthetic powder is weighed and poured into a vibrating mold, pressurized, and formed into a molded blank.
[0010] Step 5, placing the blank into a cold isostatic press, applying pressure and maintaining the pressure, to obtain a ternary lithium cathode target blank after cold isostatic pressing;
[0011] Step 6: Place the ternary lithium cathode target material into an atmosphere sintering furnace or a vacuum sintering furnace, perform multiple stages of heat preservation and multiple stages of cooling, and then naturally cool it to room temperature to obtain a ternary lithium cathode target material for a thin-film lithium battery.
[0012] Furthermore, in step 1, the lithium salt includes one or more of lithium oxide, lithium carbonate and lithium nitrate.
[0013] Further, in step 6, the step of using an atmosphere sintering furnace includes:
[0014] S601, placing the ternary lithium cathode target material into an atmosphere sintering furnace, always introducing N2+Ar mixed gas, raising the temperature from room temperature to 195-205°C, and keeping the temperature for 6.5-7.5h;
[0015] S602, heating up to 495-505°C again, introducing N2+Ar mixed gas all the time, and keeping warm for 17.5-18.5h;
[0016] S603, heating up to 685-695°C again, introducing N2+Ar mixed gas all the time, and keeping warm for 23.5-24.5h;
[0017] S604, heating up to 745-755°C again, introducing N2+Ar mixed gas all the time, and keeping warm for 17.5-19.5h;
[0018] S605, heating up to 965-975°C again, introducing N2+Ar mixed gas all the time, and keeping warm for 15.5-16.5h;
[0019] S606, slowly cool down to 445-455℃ with the furnace, keep warm for 4.5-5.5h;
[0020] S607, then naturally cool to room temperature in the furnace to obtain a ternary lithium positive electrode target material for a thin-film lithium battery.
[0021] Furthermore, in step 6, the step of using a vacuum sintering furnace includes:
[0022] S601, put the ternary lithium cathode target material into the vacuum sintering furnace, and maintain the vacuum degree of 10 -3 Pa below, raise the temperature from room temperature to 195-205℃, keep warm for 6.5-7.5h;
[0023] S602, raise the temperature to 495-505°C again and keep it warm for 17.5-18.5h;
[0024] S603, raise the temperature to 685-695°C again and keep it warm for 23.5-24.5h;
[0025] S604, raise the temperature to 745-755°C again and keep it warm for 17.5-19.5h;
[0026] S605, raise the temperature to 965-975°C again and keep it warm for 15.5-16.5h;
[0027] S606, slowly cool down to 445-455℃ with the furnace, keep warm for 4.5-5.5h;
[0028] S607, then naturally cool to room temperature in the furnace to obtain a ternary lithium positive electrode target material for a thin-film lithium battery.
[0029] Further, in step 2, the ball milling process includes:
[0030] S201, ball milling at an initial speed of 45-80 rpm for 9.5-10 hours;
[0031] S202, ball mill at a rotation speed of 195-205 rpm for more than 20 hours.
[0032] Furthermore, in step 2, the mass ratio of the dispersant to the mixed powder is controlled to be 2.5 to 3.5:1000.
[0033] Furthermore, in step 3, the ball milling speed is controlled to be 60-70 rpm, and the ball milling time is 14-16 h.
[0034] The present invention also provides a ternary lithium positive electrode target material for a thin-film lithium battery. The ternary lithium positive electrode target material for a thin-film lithium battery is prepared by the above-mentioned preparation method.
[0035] Furthermore, the ternary lithium cathode target material of the thin-film lithium battery needs to be annealed.
[0036] The present invention also provides an all-solid-state thin-film lithium battery, the positive electrode of which is prepared by using the above-mentioned thin-film lithium battery ternary lithium positive electrode target material.
[0037] Compared with the prior art, the present invention can achieve at least one of the following beneficial effects:
[0038] 1) The preparation method of the present invention first mixes lithium salt powder, manganese dioxide and nickel oxide powder to obtain a mixed powder, then mixes the mixed powder with zirconium oxide balls, then adds a dispersant to continue mixing and ball milling; then adds a binder and continues ball milling; the synthetic powder after ball milling is sieved (such as 500 mesh), poured into a vibration mold, pressurized to form a molded blank; the blank is placed in a cold isostatic press and pressurized and maintained to obtain a ternary lithium positive electrode target blank after cold isostatic pressing; finally, the ternary lithium positive electrode target blank is placed in an atmosphere sintering furnace or a vacuum sintering furnace, and after multiple stages of heat preservation and multiple stages of cooling, it is naturally cooled to room temperature with the furnace to obtain a thin film lithium battery ternary lithium positive electrode target. The preparation method of the present invention ensures that a thin film lithium battery ternary lithium positive electrode target is prepared by accurately controlling the proportion of raw materials, the order of adding each raw material, the process parameters of ball milling, the sintering steps and the process parameters of each step.
[0039] 2) The thin-film lithium battery ternary lithium positive electrode target material of the present invention has uniform composition, no segregation, good grain size consistency, controllable grain deviation, no unique phase and defective components, no cracks in the target material, and is convenient for thin film deposition.
[0040] 3) The annealing method of the thin-film lithium battery ternary lithium positive electrode target of the present invention is controlled to be after multiple stages of heat preservation, cooling to 175-185°C with the furnace and continuing to keep warm, and then naturally cooling to room temperature with the furnace to obtain the annealed thin-film lithium battery ternary lithium positive electrode target; and the temperature of each stage of heat preservation needs to be accurately controlled. The thin-film lithium battery ternary lithium positive electrode target obtained by the above annealing method has uniform composition, no segregation, good grain size consistency, controllable grain deviation, no single phase and defective components, no cracks, no stratification, no bulging, no cracking in the target material, convenient processing in subsequent machining, reduced internal stress, high yield rate, and also convenient for thin film deposition in the preparation of all-solid-state thin-film lithium batteries.
[0041] 4) The positive electrode of the all-solid-state thin-film lithium battery of the present invention is prepared using the thin-film lithium battery ternary lithium positive electrode target material of the present invention. The all-solid-state thin-film lithium battery of the present invention has high safety, and also has extremely high capacity and capacity retention rate. In addition, the all-solid-state thin-film lithium battery of the present invention also has excellent interface bonding and coordination, and has very low interface internal resistance. It can easily realize the direct series connection of multiple single-cell batteries, the direct parallel connection of multiple single-cell batteries, and the series and parallel combination of multiple single-cell batteries, which is very convenient to increase the output voltage of the battery, increase the single cell capacity of the battery pack, or achieve a perfect combination of boosting and expansion.
[0042] In the present invention, the above-mentioned technical solutions can also be combined with each other to achieve more preferred combination solutions. Other features and advantages of the present invention will be described in the subsequent description, and some advantages can become obvious from the description, or can be understood by practicing the present invention. The purpose and other advantages of the present invention can be achieved and obtained through the contents particularly pointed out in the description. BRIEF DESCRIPTION OF THE DRAWINGS
[0043] The drawings are only for the purpose of illustrating particular embodiments and are not to be construed as limiting the invention.
[0044] Figure 1 is a schematic diagram of a positive electrode target material according to Example 1 of the present invention;
[0045] Figure 2 is a schematic diagram of a positive electrode target material according to Example 2 of the present invention;
[0046] Figure 3 is a schematic diagram of a positive electrode target material according to Example 3 of the present invention;
[0047] Figure 4 Schematic diagram of the positive electrode target material of Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0048] The preferred embodiments of the present invention are described in detail below, which are mainly used to illustrate the principles of the present invention but not to limit the scope of the present invention.
[0049] The present invention provides a method for preparing a ternary lithium cathode target material for a thin-film lithium battery, comprising the following steps:
[0050] Step 1, mixing lithium salt powder with cobalt tetroxide, manganese dioxide and nickel oxide powder to obtain a mixed powder;
[0051] Step 2, putting the mixed powder into a ball mill and mixing it with zirconium oxide balls, and then adding a dispersant to continue mixing and ball milling;
[0052] Step 3, then add a binder into the ball mill and continue ball milling;
[0053] Step 4: The ball-milled synthetic powder is sieved through a 500-mesh sieve. The sieved synthetic powder is weighed and poured into a vibrating mold, pressurized, and formed into a molded blank.
[0054] Step 5, placing the blank into a cold isostatic press, applying pressure and maintaining the pressure, to obtain a ternary lithium cathode target blank after cold isostatic pressing;
[0055] Step 6: Place the ternary lithium cathode target material into an atmosphere sintering furnace or a vacuum sintering furnace, perform multiple stages of heat preservation and multiple stages of cooling, and then naturally cool it to room temperature to obtain a ternary lithium cathode target material for a thin-film lithium battery.
[0056] Specifically, in the above step 1, the lithium salt may include one or more of lithium oxide, lithium carbonate and lithium nitrate.
[0057] Specifically, in the above step 1, the mass ratio of lithium salt, cobalt tetraoxide, manganese dioxide and nickel oxide is controlled to be 10-12:18-21:18-21:45-48.
[0058] Specifically, in the above step 2, in order to ensure that the mixed powder is evenly mixed, and the particle size of the ground mixed powder is uniform and consistent by controlling the particle size of the zirconia ball, the grain size and structural uniformity of the ternary lithium product after sintering are ensured, and the mixed powder can be broken and fully in close contact, thereby reducing the chemical kinetic barrier during synthesis. Therefore, the particle size of the zirconia ball is controlled to be 0.5mm to 6mm. When the particle size of the zirconia ball is outside this range, the particle size deviation of the mixed powder is large, the mixing is uneven, there are many single substances, and the sintered target cannot be sputtered.
[0059] Specifically, in the above step 2, the ball mill is a hard ceramic tank body.
[0060] Specifically, in the above step 2, the total volume of the zirconia balls is controlled to not exceed 1 / 3 of the volume of the ball mill, and the total volume of the mixed powder is 2 / 5 to 3 / 5 of the volume of the ball mill. Preferably, the total volume of the mixed powder is 1 / 2 of the volume of the ball mill.
[0061] Specifically, in the above step 2, considering that too much dispersant will cause waste, and too little dispersant will cause the powders to self-agglomerate and fail to fully mix and contact, which is not conducive to synthesis and sintering, the mass ratio of dispersant to mixed powder is controlled to be 2.5-3.5:1000.
[0062] Specifically, in the above step 2, the dispersant may include isopropyl alcohol and isoproconazole. Preferably, the mass ratio of isopropyl alcohol to isoproconazole is 1-3:4-6.
[0063] Specifically, in the above step 2, the ball milling process includes:
[0064] S201, ball milling at an initial speed of 45-80 rpm for 9.5-10 hours;
[0065] S202, ball mill at a rotation speed of 195-205 rpm for more than 20 hours.
[0066] Specifically, in the above step 2, the ball milling process first adopts a lower speed ball milling, and then adopts a higher speed ball milling, so that the powder can be mixed evenly, which is convenient for the subsequent synthesis reaction. If the corresponding ball milling parameters are not adopted, the mixing is uneven, there are many single substances, and the sintered target material cannot be sputtered.
[0067] Specifically, in the above step 3, the binder can be polyvinyl butyral. Too much binder will cause waste, and too little binder cannot make the mixed raw material powder fully contact and quickly participate in the chemical reaction during the sintering process. Therefore, the mass ratio of the binder to the mixed powder is controlled to be (0.5-1.0):1000.
[0068] Specifically, in the above step 3, in order to ensure uniform mixing of the powders, the ball milling speed is controlled to be 60 to 70 rpm and the ball milling time is 14 to 16 hours.
[0069] Specifically, in the above step 4, in order to ensure the uniformity of the grain size and crystal phase structure of the ternary lithium product after sintering, the synthetic powder is controlled to pass through a 500-mesh sieve. If it is not within this parameter range, the powder particle size is dispersed, the target material compact has large gaps, and it cannot be completely ceramicized after sintering, and sputtering deposition cannot be performed.
[0070] Specifically, in the above step 4, considering that too high a pressure will have a high requirement on the equipment, and too low a pressure will not work, the pressure is controlled to be 1450-1550 tons to form a molded blank.
[0071] Specifically, in the above step 5, considering that during the cold isostatic pressing process, too high a pressure will have high requirements on the equipment, and too low a pressure will not work, therefore, the pressure is controlled to 295-305Mpa and maintained for 50-70 minutes.
[0072] Specifically, in the above step 6, the step of using an atmosphere sintering furnace includes:
[0073] S601, placing the ternary lithium cathode target material into an atmosphere sintering furnace, always introducing N2+Ar mixed gas, raising the temperature from room temperature to 195-205°C, and keeping the temperature for 6.5-7.5h; wherein the volume ratio of N2 to Ar is 4.5-5.5:5;
[0074] S602, heating up to 495-505°C again, introducing N2+Ar mixed gas all the time, and keeping warm for 17.5-18.5h; wherein the volume ratio of N2 to Ar is 4.5-5.5:5;
[0075] S603, heating up to 685-695°C again, introducing N2+Ar mixed gas all the time, and keeping warm for 23.5-24.5h; wherein the volume ratio of N2 to Ar is 5.5-6.5:4;
[0076] S604, heating up to 745-755°C again, introducing N2+Ar mixed gas all the time, and keeping warm for 17.5-19.5h; wherein the volume ratio of N2 to Ar is 4.5-5.5:5;
[0077] S605, heating up to 965-975°C again, introducing N2+Ar mixed gas all the time, and keeping warm for 15.5-16.5h; wherein the volume ratio of N2 to Ar is 5.5-6.5:4;
[0078] S606, slowly cool down to 445-455℃ with the furnace, keep warm for 4.5-5.5h;
[0079] S607, then naturally cool to room temperature in the furnace to obtain a ternary lithium positive electrode target material for a thin-film lithium battery.
[0080] Specifically, in the above S606 and S607, in order to ensure the uniformity of the microstructure of the obtained ternary lithium positive electrode target, it is necessary to first slowly cool it to 445-455°C with the furnace and keep it warm for 4.5-5.5 hours; then naturally cool it to room temperature with the furnace.
[0081] Specifically, in the above step 6, the step of using a vacuum sintering furnace includes:
[0082] S601, put the ternary lithium cathode target material into the vacuum sintering furnace, and maintain the vacuum degree of 10 -3Pa below, raise the temperature from room temperature to 195-205℃, keep warm for 6.5-7.5h;
[0083] S602, raise the temperature to 495-505°C again and keep it warm for 17.5-18.5h;
[0084] S603, raise the temperature to 685-695°C again and keep it warm for 23.5-24.5h;
[0085] S604, raise the temperature to 745-755°C again and keep it warm for 17.5-19.5h;
[0086] S605, raise the temperature to 965-975°C again and keep it warm for 15.5-16.5h;
[0087] S606, slowly cool down to 445-455℃ with the furnace, keep warm for 4.5-5.5h;
[0088] S607, then naturally cool to room temperature in the furnace to obtain a ternary lithium positive electrode target material for a thin-film lithium battery.
[0089] Specifically, in the above S602-S605, the vacuum degree is always maintained at 10 -3 Below pa.
[0090] Specifically, in the above S606 and S607, in order to ensure the uniformity of the microstructure of the obtained ternary lithium positive electrode target, it is necessary to first slowly cool it to 445-455°C with the furnace and keep it warm for 4.5-5.5 hours; then naturally cool it to room temperature with the furnace.
[0091] Specifically, in the above step 6, the temperature, atmosphere, holding time and other parameters of each stage of the multi-stage heating step in each of the above steps are all controlled in consideration of the chemical reaction kinetics requirements of sintering, and can ensure the uniformity of the composition and grain structure requirements of the synthesized ternary lithium when the chemical reaction of the sintering process is carried out. If the sintering is not within this temperature range, the target material cannot be completely ceramicized, and there are cases where the target material is over-sintered or under-sintered, has multiple holes, is sintered and deformed, and cannot be used at all.
[0092] Specifically, in the above step 6, the obtained thin-film lithium battery ternary lithium positive electrode target material has uniform composition, no segregation, good grain size consistency, controllable grain deviation, no unique phase and defective components, no cracks in the target material, and is convenient for thin film deposition. The grain size of the thin-film lithium battery ternary lithium positive electrode target material is between 346nm and 768nm, the flatness of the target material after sintering is between 0.3mm and 0.7mm, and the relative density of the sintered target material is greater than 96.7%.
[0093] Specifically, the method for preparing the above-mentioned thin-film lithium battery ternary lithium positive electrode target material also includes:
[0094] Step 7: annealing the thin-film lithium battery ternary lithium positive electrode target material of step 6.
[0095] Specifically, step 7 includes the following steps:
[0096] S701, put the thin film lithium battery ternary lithium positive electrode target into the vacuum annealing furnace, and evacuate to 1~1.5×10 - 4 Pa, maintain the vacuum degree for 2.5 to 3.5 hours;
[0097] S702, introduce high-purity nitrogen to make the pressure inside the furnace greater than the atmospheric pressure outside the furnace, maintain it for 25 to 35 minutes, and then evacuate to 1 to 1.5×10 -4 Pa, maintain the vacuum degree for 2.5 to 3.5 hours;
[0098] S703, always introduce H2+Ar mixed gas, raise the temperature from room temperature to 115-125°C, and keep it warm for 4.5-5.5h;
[0099] S704, always introduce H2+Ar mixed gas, raise the furnace temperature to 215-225°C, and keep it warm for 2.5-3.5h;
[0100] S705, always introduce H2+Ar mixed gas, raise the furnace temperature to 345-355°C, and keep it warm for 5.5-6.5h;
[0101] S706, always introduce H2+Ar mixed gas, slowly cool to 175-185℃ with the furnace, and keep warm for 3.5-4.5h;
[0102] S707, then vacuum to 1~1.5×10 -4 Pa, maintain the vacuum degree for 2.5 to 3.5 hours;
[0103] S708, introducing high-purity nitrogen to make the pressure inside the furnace greater than the atmospheric pressure outside the furnace, and then naturally cooling to room temperature with the furnace to obtain the annealed thin-film lithium battery ternary lithium positive electrode target.
[0104] Specifically, in the above steps S703 to S706, the pressure inside the vacuum annealing furnace is always kept greater than the atmospheric pressure outside the furnace.
[0105] Specifically, in the above S703-S706, the volume ratio of H2 to Ar is 6-8:92-94.
[0106] Specifically, considering that the insulation temperature of the above-mentioned thin-film lithium battery ternary lithium cathode target is too low, delamination defects will occur, and the insulation temperature is too high, bulging or cracking will occur. Therefore, after in-depth research, the above-mentioned annealing method is precisely controlled to be three-stage insulation, followed by furnace cooling to 175-185°C and continued insulation, and then naturally cooling to room temperature with the furnace to obtain the annealed thin-film lithium battery ternary lithium cathode target; and the insulation temperature and insulation time of each stage need to be precisely controlled.
[0107] Specifically, the composition of the ternary lithium cathode target material of the thin-film lithium battery after the above annealing treatment is uniform, without segregation, good grain size consistency, controllable grain deviation, no unique phase and defective components, no cracks, no stratification, no bulging, no cracking in the target material, convenient processing during subsequent machining, reducing internal stress, high yield rate, and also convenient for subsequent thin film deposition. If it is not processed within this parameter range, the material is easy to crack during machining, there are a large number of microscopic cracks inside, and large particles of powder will be produced during sputtering deposition.
[0108] The present invention also provides a ternary lithium positive electrode target material for a thin-film lithium battery, which is prepared by the above method.
[0109] The present invention also provides an all-solid-state thin-film lithium battery, the positive electrode of which is prepared by using the above-mentioned thin-film lithium battery ternary lithium positive electrode target material.
[0110] Specifically, the preparation method of the above-mentioned all-solid-state thin-film lithium battery includes:
[0111] Step 1, coating a graphene film on the surface of the copper foil, and continuing to deposit a negative electrode film on the graphene film;
[0112] Step 2, then depositing a solid electrolyte film on the negative electrode film;
[0113] Step 3, depositing a positive electrode thin film on the solid electrolyte film using the above-mentioned thin film lithium battery ternary lithium positive electrode target material;
[0114] Step 4: After formation, an all-solid-state thin-film lithium battery is obtained.
[0115] Specifically, the all-solid-state thin-film lithium battery of the present invention has high safety as well as high capacity and capacity retention rate. For example, the capacity is above 15300mA h (e.g., 15300-44880mA h), and the capacity remains basically unchanged after more than 10,000 cycles. In addition, the all-solid-state thin-film lithium battery of the present invention also has excellent interface bonding and coordination, and has very low interface internal resistance, for example, the interface internal resistance is less than 0.01 ohm / cm 2It is very easy to realize the direct series connection of multiple single-cell batteries, the direct parallel connection of multiple single-cell batteries, and the series and parallel combination of multiple single-cell batteries, which can easily increase the output voltage of the battery, increase the single cell capacity of the battery pack, or achieve a perfect combination of boosting and capacity expansion.
[0116] The following is a further description of the thin film lithium battery ternary lithium cathode target material, preparation method and thin film lithium battery of the present invention in combination with specific embodiments. Wherein, unless otherwise specified, the raw materials used can be obtained from the market.
[0117] Example 1
[0118] This embodiment provides a method for preparing a ternary lithium cathode target material for a thin-film lithium battery, comprising:
[0119] Step 1, mixing lithium salt powder with cobalt tetroxide, manganese dioxide and nickel oxide powder to obtain a mixed powder; the lithium salt is lithium oxide, and the mass ratio of lithium oxide, cobalt tetroxide, manganese dioxide and nickel oxide is 12:20:20:48;
[0120] Step 2, putting the mixed powder into a ball mill and mixing it with zirconium oxide balls with a particle size of 0.6 mm to 1.5 mm, and then adding a dispersant to continue mixing and ball milling; the ball mill is a hard ceramic tank; the total volume of the zirconium oxide balls accounts for 1 / 3 of the volume of the ball mill, and the total volume of the mixed powder accounts for 1 / 2 of the volume of the ball mill; the mass ratio of the dispersant to the mixed powder is 3:1000;
[0121] Specifically, in step 2, the ball milling process includes:
[0122] S201, ball milling at an initial speed of 50 rpm for 10 h;
[0123] S202, ball milling at a speed of 200 rpm for 21 hours;
[0124] Step 3, then add a binder into the ball mill, and ball mill for 15 hours at a rotation speed of 65 rpm; the mass ratio of the binder to the mixed powder is 1:1000;
[0125] Step 4: The ball-milled synthetic powder is sieved through a 500-mesh sieve. The sieved synthetic powder is weighed and poured into a vibrating mold, pressurized to 1500 tons, to form a molded blank;
[0126] Step 5, placing the blank into a cold isostatic press, pressurizing to 300 MPa, and maintaining the pressure for 60 minutes to obtain a ternary lithium cathode target blank after cold isostatic pressing;
[0127] Step 6, placing the ternary lithium cathode target material into an atmosphere sintering furnace for multiple stages of heat preservation and multiple stages of cooling, and then naturally cooling to room temperature with the furnace to obtain a ternary lithium cathode target material for a thin-film lithium battery;
[0128] Step 6 includes:
[0129] S601, placing the ternary lithium cathode target material into an atmosphere sintering furnace, always introducing a N2+Ar (ratio 5:5) mixed gas, raising the temperature from room temperature to 200°C, and keeping the temperature for 7 hours;
[0130] S602, raise the temperature to 500°C again, and introduce N2+Ar (ratio 5:5) mixed gas to keep warm for 18 hours;
[0131] S603, heating up to 690°C again, introducing N2+Ar (ratio 6:4) mixed gas all the time, and keeping warm for 24h;
[0132] S604, raise the temperature to 750°C again, introduce N2+Ar (ratio 5:5) mixed gas all the time, and keep warm for 18 hours;
[0133] S605, heating up to 970°C again, introducing N2+Ar (ratio 6:4) mixed gas all the time, and keeping the temperature for 16 hours;
[0134] S606, slowly cool down to 450℃ with the furnace, keep warm for 5h;
[0135] S607, then naturally cool to room temperature in the furnace to obtain a ternary lithium positive electrode target material for a thin-film lithium battery.
[0136] The thin-film lithium battery ternary lithium positive electrode target material obtained in this embodiment is as follows Figure 1 As shown, the composition of the positive electrode target is uniform, without segregation, the grain size is consistent, the grain deviation is controllable, there is no unique phase and defective components, there is no crack in the target, and it is easy to deposit thin films. Specifically, the grains of the thin film lithium battery ternary lithium positive electrode target of this embodiment are 356nm to 468nm, the flatness of the target after sintering is about 0.35mm, and the relative density of the target after sintering is about 96.9%.
[0137] Example 2
[0138] This embodiment provides a method for preparing a ternary lithium cathode target material for a thin-film lithium battery, comprising:
[0139] Step 1, mixing lithium salt powder with cobalt tetroxide, manganese dioxide and nickel oxide powder to obtain a mixed powder; the lithium salt is lithium carbonate, and the mass ratio of lithium carbonate, cobalt tetroxide, manganese dioxide and nickel oxide is 12:20:20:48;
[0140] Step 2, putting the mixed powder into a ball mill and mixing it with zirconium oxide balls with a particle size of 2 mm to 4.5 mm, and then adding a dispersant to continue mixing and ball milling; the ball mill is a hard ceramic tank; the total volume of the zirconium oxide balls accounts for 1 / 3 of the volume of the ball mill, and the total volume of the mixed powder accounts for 1 / 2 of the volume of the ball mill; the mass ratio of the dispersant to the mixed powder is 3:1000;
[0141] Specifically, in step 2, the ball milling process includes:
[0142] S201, ball milling at an initial speed of 70 rpm for 9.5 h;
[0143] S202, ball milling at a speed of 205 rpm for 22 hours;
[0144] Step 3, then add a binder into the ball mill, and ball mill for 14 hours at a rotation speed of 70 rpm; the mass ratio of the binder to the mixed powder is 1:1000;
[0145] Step 4: The ball-milled synthetic powder is sieved through a 500-mesh sieve. The sieved synthetic powder is weighed and poured into a vibrating mold, which is pressurized to 1510 tons to form a molded blank.
[0146] Step 5, placing the blank into a cold isostatic press, pressurizing to 303 MPa, and maintaining the pressure for 55 minutes to obtain a ternary lithium cathode target blank after cold isostatic pressing;
[0147] Step 6, placing the ternary lithium cathode target material into an atmosphere sintering furnace for multiple stages of heat preservation and multiple stages of cooling, and then naturally cooling to room temperature with the furnace to obtain a ternary lithium cathode target material for a thin-film lithium battery;
[0148] Step 6 includes:
[0149] S601, placing the ternary lithium cathode target material into an atmosphere sintering furnace, always introducing a mixed gas of N2+Ar (ratio 4.5:5), raising the temperature from room temperature to 205°C, and keeping the temperature for 6.7h;
[0150] S602, raise the temperature to 505°C again, and introduce N2+Ar (ratio 5:5) mixed gas to keep warm for 17.5h;
[0151] S603, raise the temperature to 685°C again, introduce N2+Ar (ratio 6:4) mixed gas all the time, and keep warm for 24.5h;
[0152] S604, raise the temperature to 755°C again, introduce N2+Ar (ratio 5:5) mixed gas all the time, and keep warm for 17.6h;
[0153] S605, heating up to 975°C again, introducing N2+Ar (ratio 6:4) mixed gas all the time, and keeping warm for 15.6h;
[0154] S606, slowly cool down to 450℃ with the furnace, keep warm for 5h;
[0155] S607, then naturally cool to room temperature in the furnace to obtain a ternary lithium positive electrode target material for a thin-film lithium battery.
[0156] The thin-film lithium battery ternary lithium positive electrode target material obtained in this embodiment is as follows Figure 2 As shown, the composition of the positive electrode target is uniform, without segregation, the grain size is consistent, the grain deviation is controllable, there is no unique phase and defective components, there is no crack in the target, and it is easy to deposit thin films. Specifically, the grains of the thin film lithium battery ternary lithium positive electrode target of this embodiment are 516nm to 708nm, the flatness of the target after sintering is about 0.4mm, and the relative density of the target after sintering is about 97.1%.
[0157] Example 3
[0158] This embodiment provides a method for preparing a ternary lithium cathode target material for a thin-film lithium battery, wherein steps 1 to 5 are the same as those in embodiment 1 and will not be described in detail herein, and further comprises:
[0159] Step 6, placing the ternary lithium cathode target material into a vacuum sintering furnace, performing multiple stages of heat preservation and multiple stages of cooling, and then naturally cooling to room temperature with the furnace to obtain a ternary lithium cathode target material for a thin-film lithium battery;
[0160] Step 6 includes:
[0161] S601, put the ternary lithium cathode target material into the vacuum sintering furnace, and maintain the vacuum degree of 10 -3 Pa below, raise the temperature from room temperature to 200℃, keep warm for 7h;
[0162] S602, raise the temperature to 500°C again and keep it for 18 hours;
[0163] S603, heating up to 690°C again and keeping warm for 24h;
[0164] S604, raise the temperature to 750°C again and keep it for 18 hours;
[0165] S605, heating up to 970°C again and keeping warm for 16h;
[0166] S606, slowly cool down to 450℃ with the furnace, keep warm for 5h;
[0167] S607, then naturally cool to room temperature in the furnace to obtain a ternary lithium positive electrode target material for a thin-film lithium battery.
[0168] Specifically, in the above S602-S605, the vacuum degree is always maintained at 10 -3 Below pa.
[0169] The thin-film lithium battery ternary lithium positive electrode target material obtained in this embodiment is as follows Figure 3 As shown, the composition of the positive electrode target is uniform, without segregation, good grain size consistency, controllable grain deviation, no unique phase and defective components, no cracks in the target, and easy to deposit thin films. Specifically, the grain size of the thin film lithium battery ternary lithium positive electrode target of this embodiment is 350nm to 428nm, the flatness of the target after sintering is about 0.32mm, and the relative density of the target after sintering is 97.1%.
[0170] Example 4
[0171] This embodiment provides a thin-film lithium battery ternary lithium positive electrode target material. This embodiment anneals the thin-film lithium battery ternary lithium positive electrode target material obtained in Example 1, including:
[0172] S701, put the thin film lithium battery ternary lithium positive electrode target into the vacuum annealing furnace and evacuate to 10 -4 Pa, maintain this vacuum for 3h;
[0173] S702, introduce high-purity nitrogen to make the pressure inside the furnace greater than the atmospheric pressure outside the furnace, maintain for 30 minutes, and then evacuate to 10 -4 Pa, maintain this vacuum for 3h;
[0174] S703, always introduce H2+Ar mixed gas, raise the temperature from room temperature to 120°C, and keep it warm for 5 hours;
[0175] S704, always introduce H2+Ar mixed gas, raise the furnace temperature to 220℃, and keep it warm for 3h;
[0176] S705, H2+Ar mixed gas is introduced all the time, the furnace temperature is raised to 350°C, and kept warm for 6 hours;
[0177] S706, always introduce H2+Ar mixed gas, slowly cool to 180℃ with the furnace, and keep warm for 4h;
[0178] S707, then vacuum to 10 -4 Pa, maintain this vacuum for 3h;
[0179] S708, introducing high-purity nitrogen to make the pressure inside the furnace greater than the atmospheric pressure outside the furnace, and then naturally cooling to room temperature with the furnace to obtain the annealed thin-film lithium battery ternary lithium positive electrode target.
[0180] Specifically, in the above steps S703 to S706, the pressure inside the vacuum annealing furnace is always kept greater than the atmospheric pressure outside the furnace.
[0181] Specifically, in the above S703-S706, the volume ratio of H2 to Ar is 7:93.
[0182] The composition of the ternary lithium cathode target material of the thin-film lithium battery after annealing in this embodiment is uniform, without segregation, good grain size consistency, controllable grain deviation, no single phase and defective components, no cracks, no stratification, no bulging, no cracking in the target material, convenient processing during subsequent machining, reducing internal stress, high yield rate, and also convenient for subsequent thin film deposition. The grains of the ternary lithium cathode target material of the thin-film lithium battery after annealing in this embodiment are 346nm to 398nm, the flatness is about 0.31mm, and the relative density is greater than about 97.7%.
[0183] Example 5
[0184] This embodiment provides an all-solid-state thin-film lithium battery. In this embodiment, a single-cell all-solid-state thin-film lithium battery is deposited. The preparation method includes:
[0185] Step 1: Coat a graphene film (6 μm thick) on a 1 square meter copper foil surface, and continue to deposit a negative electrode film on the graphene film, the thickness of the negative electrode film being 4.5 μm;
[0186] Step 2: Then, a solid electrolyte film is deposited on the negative electrode film, and the thickness of the solid electrolyte film is 1.5 μm;
[0187] Step 3, depositing a positive electrode thin film on the solid electrolyte film using the thin film lithium battery ternary lithium positive electrode target material of the above embodiment 4; the thickness of the positive electrode thin film is 15 μm;
[0188] Step 4: After formation, an all-solid-state thin-film lithium battery is obtained.
[0189] The interfacial internal resistance of the all-solid-state thin-film lithium battery of this embodiment is less than 0.01 ohm / cm 2 , the capacity is 15300 (mAh), the cycle is more than 10000 times, and the capacity remains basically unchanged.
[0190] Example 6
[0191] This embodiment provides an all-solid-state thin-film lithium battery. In this embodiment, two all-solid-state thin-film lithium batteries are deposited in series. The preparation method includes:
[0192] A graphene film (7 μm thick) is coated on a 1 m2 copper foil surface, the thickness of the negative electrode film of each thin-film lithium battery deposited on the graphene film is 5.5 μm, and the thickness of the solid electrolyte film of each battery deposited subsequently is 2.0 μm. The positive electrode film of the thin-film lithium battery deposited by the thin-film lithium battery ternary lithium positive electrode target material of Example 4 is 18.5 μm thick, and the capacity of the obtained battery after formation is 18870 (mA h); the capacity remains basically unchanged after more than 10,000 cycles; the interface internal resistance is less than 0.01 ohm / cm 2 .
[0193] Example 7
[0194] This embodiment provides an all-solid-state thin-film lithium battery. In this embodiment, two all-solid-state thin-film lithium batteries connected in parallel are deposited. The preparation method includes:
[0195] A graphene film (7 μm thick) was coated on the surface of 1 square meter of copper foil, the thickness of the negative electrode film of each battery deposited on the graphene film was 6.5 μm, and the thickness of the solid electrolyte film of each battery deposited subsequently was 2.5 μm. The positive electrode film of the thin film lithium battery deposited by the thin film lithium battery ternary lithium positive electrode target material of Example 4 was 22 μm thick, and the capacity of the obtained battery after formation was 44880 (mA h); the capacity remained basically unchanged after more than 10000 cycles; the interface internal resistance was less than 0.01 ohm / cm 2 .
[0196] Comparative Example 1
[0197] This comparative example provides a method for preparing a ternary lithium cathode target material for a thin-film lithium battery, which is as follows:
[0198] Step 1-step 2, the same as in Example 1;
[0199] Step 3, then add a binder into the ball mill, and ball mill for 15 hours at a rotation speed of 145 rpm; the mass ratio of the binder to the mixed powder is 1:1000;
[0200] Step 4: The ball-milled synthetic powder is sieved through a 500-mesh sieve. The sieved synthetic powder is weighed and poured into a vibrating mold, pressurized to 1,200 tons, to form a molded blank;
[0201] Step 5: Place the blank into a cold isostatic press, pressurize to 100 MPa, and maintain the pressure for 40 minutes. However, a suitable ternary lithium cathode target blank cannot be obtained.
[0202] The process parameters of this comparative example are not suitable, and the ternary lithium positive electrode target material for thin-film lithium batteries cannot be obtained.
[0203] Comparative Example 2
[0204] This comparative example provides a method for preparing a ternary lithium cathode target material for a thin-film lithium battery, which is as follows:
[0205] In step 2 of this comparative example, the particle size of the zirconia balls is 0.3 to 15 mm; the remaining steps are the same as those of Example 1.
[0206] The positive electrode target material of this comparative example is Figure 4 As shown, the target material has a large grain deviation, uneven mixing, and many single substances, and the sintered target material cannot be sputtered.
[0207] Comparative Example 3
[0208] This comparative example provides a method for preparing a ternary lithium cathode target material for a thin-film lithium battery, which is as follows:
[0209] In step 2 of this comparative example, the ball milling process directly adopts 130 rpm ball milling for 19 hours; the remaining steps are the same as those in Example 1.
[0210] In this comparative example, the powders are not mixed evenly, and there are many single substances, so the sintered target cannot be sputtered.
[0211] Comparative Example 4
[0212] This comparative example provides a method for preparing a ternary lithium cathode target material for a thin-film lithium battery, which is as follows:
[0213] In step 4 of this comparative example, the synthetic powder is controlled to pass through a 300-mesh sieve; the remaining steps are the same as those of Example 1.
[0214] The target material compact of this comparative example has large gaps and cannot be completely ceramicized after sintering, and cannot be sputtered and deposited.
[0215] Comparative Example 5
[0216] This comparative example provides a method for preparing a ternary lithium cathode target material for a thin-film lithium battery, which is as follows:
[0217] In step 6 of this comparative example, S602-S607 are directly performed; the remaining steps are the same as those in Example 1.
[0218] The target material of this comparative example cannot be completely ceramicized and cannot be used at all.
[0219] Comparative Example 6
[0220] This comparative example provides a method for preparing a ternary lithium cathode target material for a thin-film lithium battery. The preparation method of this comparative example is substantially the same as that of Example 4, except that:
[0221] In step S703 of this comparative example, H2+Ar mixed gas is always introduced, and the temperature is raised from room temperature to 190°C and kept for 3 hours;
[0222] S704, H2+Ar mixed gas is introduced all the time, the furnace temperature is raised to 250°C, and kept warm for 2h;
[0223] S705, H2+Ar mixed gas is introduced all the time, the furnace temperature is raised to 390°C, and kept warm for 5 hours;
[0224] S706, always introduce H2+Ar mixed gas, slowly cool to 180℃ with the furnace, and keep warm for 4h;
[0225] S707, then vacuum to 10-4 Pa, maintain this vacuum for 3h;
[0226] S708, introducing high-purity nitrogen to make the pressure inside the furnace greater than the atmospheric pressure outside the furnace, and then naturally cooling to room temperature with the furnace to obtain the annealed thin-film lithium battery ternary lithium positive electrode target.
[0227] The positive electrode target material of this comparative example is stratified after annealing, and the target material is prone to cracking during machining.
[0228] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with the technical field within the technical scope disclosed by the present invention should be covered within the protection scope of the present invention.
Claims
1. A method for preparing a ternary lithium cathode target material for a thin-film lithium battery. It is characterized in that The steps include: Step 1, mixing lithium salt powder with cobalt tetroxide, manganese dioxide and nickel oxide powder to obtain a mixed powder; the mass ratio of lithium salt, cobalt tetroxide, manganese dioxide and nickel oxide is 10-12:18-21:18-21:45-48; Step 2, putting the mixed powder into a ball mill and mixing it with zirconium oxide balls, and then adding a dispersant to continue mixing and ball milling; Step 3, then add a binder into the ball mill and continue ball milling; Step 4: The ball-milled synthetic powder is sieved through a 500-mesh sieve. The sieved synthetic powder is weighed and poured into a vibrating mold, pressurized, and formed into a molded blank. Step 5, placing the blank into a cold isostatic press, applying pressure and maintaining the pressure, to obtain a ternary lithium cathode target blank after cold isostatic pressing; Step 6: Place the ternary lithium cathode target material into an atmosphere sintering furnace or a vacuum sintering furnace, perform multiple stages of heat preservation and multiple stages of cooling, and then naturally cool it to room temperature to obtain a ternary lithium cathode target material for a thin-film lithium battery.
2. The preparation method according to claim 1, It is characterized in that In step 1, the lithium salt includes one or more of lithium oxide, lithium carbonate and lithium nitrate.
3. The preparation method according to claim 1, It is characterized in that In step 6, the step of using an atmosphere sintering furnace includes: S601, put the ternary lithium cathode target material into the atmosphere sintering furnace, and always pass N 2 +Ar mixed gas, raise the temperature from room temperature to 195-205℃, keep warm for 6.5-7.5h; S602, raise the temperature to 495-505℃ again, and keep N 2 +Ar mixed gas, keep warm for 17.5~18.5h; S603, raise the temperature to 685-695℃ again, and keep N 2 +Ar mixed gas, keep warm for 23.5~24.5h; S604, raise the temperature to 745-755℃ again, and keep N 2 +Ar mixed gas, keep warm for 17.5~19.5h; S605, raise the temperature to 965-975℃ again, and keep N 2 +Ar mixed gas, keep warm for 15.5~16.5h; S606, slowly cool down to 445-455℃ with the furnace, keep warm for 4.5-5.5h; S607, then naturally cool to room temperature in the furnace to obtain a ternary lithium positive electrode target material for a thin-film lithium battery.
4. The preparation method according to claim 1, It is characterized in that In step 6, the step of using a vacuum sintering furnace includes: S601, put the ternary lithium cathode target material into the vacuum sintering furnace, and maintain the vacuum degree of 10 -3 Pa below, raise the temperature from room temperature to 195-205℃, keep warm for 6.5-7.5h; S602, raise the temperature to 495-505°C again and keep it warm for 17.5-18.5h; S603, raise the temperature to 685-695°C again and keep it warm for 23.5-24.5h; S604, raise the temperature to 745-755°C again and keep it warm for 17.5-19.5h; S605, raise the temperature to 965-975°C again and keep it warm for 15.5-16.5h; S606, slowly cool down to 445-455℃ with the furnace, keep warm for 4.5-5.5h; S607, then naturally cool to room temperature in the furnace to obtain a ternary lithium positive electrode target material for a thin-film lithium battery.
5. The preparation method according to claim 1, It is characterized in that In step 2, the ball milling process includes: S201, ball milling at an initial speed of 45-80 rpm for 9.5-10 hours; S202, ball mill at a rotation speed of 195-205 rpm for more than 20 hours.
6. The preparation method according to claim 1, It is characterized in that In the step 2, the mass ratio of the dispersant to the mixed powder is controlled to be 2.5-3.5:1000.
7. The preparation method according to any one of claims 1 to 6, It is characterized in that In the step 3, the ball milling speed is controlled to be 60-70 rpm, and the ball milling time is 14-16 h.
8. A ternary lithium cathode target material for a thin-film lithium battery. It is characterized in that The thin-film lithium battery ternary lithium positive electrode target material is prepared by the preparation method described in any one of claims 1-7.
9. The thin-film lithium battery ternary lithium cathode target material according to claim 8, It is characterized in that The thin-film lithium battery ternary lithium positive electrode target material also needs to be annealed.
10. An all-solid-state thin-film lithium battery, It is characterized in that The positive electrode of the all-solid-state thin-film lithium battery is prepared using the thin-film lithium battery ternary lithium positive electrode target material according to claim 9.
Citation Information
Cited By
Preparation method of low-temperature carbon-coated gamma-MnO2 and aqueous zinc ion battery