Nanofiber polymer mortar on surface of PS (polystyrene) backing plate as well as preparation method and application of nanofiber polymer mortar
By surface modification of modified zirconia nanofibers and cilastatin sodium, combined with polymer emulsion, cement and sand, a nanofiber polymer mortar suitable for PS backing boards was prepared, which solved the PS problems in the existing technology. The problem of insufficient performance of the backing board is achieved, and efficient adhesion and frost resistance are improved.
Patent Information
- Application Number
- CN202411050394.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-29
AI Technical Summary
The existing polymer mortar is not suitable for the surface of the PS backing board and cannot effectively improve the flame retardant and mechanical properties of the PS backing board, which limits its application in the fields of building thermal insulation, cold preservation, and moisture-proofing.
Use modified zirconia nanofibers and cilastatin sodium surface modification, combine polymer emulsion with cement and sand, and prepare nanofiber polymer mortar on the surface of the PS backing board by stirring evenly to improve its dispersion stability and adhesion. performance.
It achieves excellent adhesion and frost resistance of the polymer mortar on the surface of the PS backing board, improving the stability and performance of the product.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the field of polymer mortar preparation, and in particular to a PS backing plate surface nanofiber polymer mortar and a preparation method and application thereof. Background Art
[0002] PS sheet is a plastic sheet made of polystyrene resin through plasticization, extrusion and foaming, also known as polystyrene sheet. Due to its light material, it is widely used in advertising production and interior decoration. At the same time, PS sheet also has high strength and corrosion resistance, and is easy to process. It can be cut, formed, hot bent and other processing techniques as needed. Its surface is smooth and flat, and can be sprayed, printed and other surface treatments. It has good performance when applied to outdoor materials. Secondly, PS sheet also has good thermal insulation and sound insulation properties. It is used to make ceilings, wall decorative panels, partitions, etc. It is not only beautiful, but also can play a role in heat insulation and sound insulation, improving the comfort of the indoor environment.
[0003] Although the comprehensive performance of PS is very excellent, the flame retardant and mechanical properties of PS boards are average, which greatly limits the application scope of PS composite materials in the fields of exterior wall insulation, roof insulation, moisture-proofing, etc. In order to improve the performance of PS, many researchers will coat its surface with polymer mortar.
[0004] Polymer mortar is a new building material in recent years. It is made by mixing cement, aggregate and organic polymers that can be dispersed in water. The polymer can be a homopolymer formed by the polymerization of one monomer, or a copolymer formed by the polymerization of two or more monomers. The polymer must form a film on the surface of cement particles under environmental conditions, and form a strong bond between the cement body and the aggregate. The cross-linked network formed must have the ability to prevent the occurrence of microcracks and prevent the expansion of cracks. Polymer mortar can waterproof, protect, repair and reinforce the main body of the building. It has great application prospects in water conservancy, municipal administration, roads and bridges, underground and other fields, and is expected to become a new green cementitious material to replace cement.
[0005] In recent years, polymer mortar has been widely used as a concrete repair material. For example, the invention patent with application number 201810636651.8 discloses a high-performance polymer mortar and its preparation method. The raw materials of the polymer mortar include: silicate cement, quartz sand, water reducer, antioxidant, polymer, lignocellulose, defoamer, calcium carbonate whisker, and inorganic nanoparticles. The preparation method is to first activate the quartz sand, calcium carbonate whisker and inorganic nanoparticles, then add the water reducer, antioxidant, polymer, lignocellulose and defoamer to the silicate cement, stir evenly, add the activated mixture, and stir evenly to obtain. The invention patent with application number 201810271268.7 discloses a special cement-based polymer mortar for repair and its preparation method. The mortar includes the following raw materials: Wudalianchi volcanic mud, silicone resin polyether emulsion, sodium tripolyphosphate, polyacrylamide, calcium chloride, adhesive additive, water reducer, foaming agent and anti-radiation agent. The preparation method is obtained by mixing and grinding the raw materials. The performance of the polymer mortar involved in the above two patents is not suitable for the surface of PS backing board and cannot be constructed by pouring.
[0006] In summary, there is an urgent need for a polymer mortar to be used on the surface of the PS backing board to solve some shortcomings of the existing PS backing board as a building insulation, cold insulation and moisture-proof material. Summary of the invention
[0007] In order to improve the dispersion stability of zirconium oxide nanofibers in polymer mortar and the obtained polymer mortar layer has excellent adhesion performance on the PS backing board, and finally achieve the use stability and frost resistance of the PS backing board product, the present invention provides a PS backing board surface nanofiber polymer mortar and its preparation method and application.
[0008] A nanofiber polymer mortar for the surface of a PS backing plate comprises the following components in parts by weight: 70-110 parts of fast-hardening sulphoaluminate cement, 50-75 parts of polymer emulsion, 7-14 parts of intumescent flame retardant, 15-35 parts of modified zirconia nanofibers, 5-7 parts of mica powder, 100-200 parts of quartz sand and 0.5-10 parts of functional additives; wherein the modified zirconia nanofibers are obtained by modifying zirconia nanofibers with sodium cilastatin.
[0009] In some embodiments of the present invention, the polymer emulsion is obtained by mixing an acrylate emulsion and an epoxy emulsion in a mass ratio of 1-2:0.3-1.1; wherein the viscosity of the acrylate emulsion is less than 100 mPa·s; and the viscosity of the epoxy emulsion is 500-1500 mPa·s. Specifically, the acrylate emulsion may be Dow PRIMAL ST-954, PRIMAL NW5118, PRIMAL TR407, etc.; the epoxy emulsion may be Gene JE-9064, Green GL1900, Changsha Kaijian's KJ-998, Mingzhou Chemical's MZ-20, etc.
[0010] In some embodiments of the present invention, the intumescent flame retardant is obtained by mixing pentaerythritol and ammonium polyphosphate in a mass ratio of 3-4:2.5-5.5.
[0011] In some embodiments of the present invention, the preparation process of modified zirconia nanofibers comprises the following steps: adding zirconia nanofibers to an organic solvent to prepare a suspension, then adding sodium cilastatin, stirring evenly at room temperature, dripping 98% concentrated sulfuric acid, heating to reflux, reacting for 3-5 hours, and after the reaction is completed, cooling the reaction system to room temperature and centrifuging, washing the obtained precipitate with ethanol, and drying it in an oven to obtain the modified zirconia nanofibers.
[0012] Furthermore, the organic solvent is at least one of benzene, toluene, xylene, n-hexane and cyclohexane.
[0013] Furthermore, the preparation of the zirconium oxide nanofibers can be carried out according to a method well known to those skilled in the art, specifically, the following steps can be followed: tetrabutyl zirconate is dissolved in acetic acid, then slowly added to a solution containing polyvinyl pyrrolidone and polymethyl methacrylate, stirred evenly, and a spinning precursor solution is prepared. Tetrabutyl zirconate-polyvinyl pyrrolidone-polymethyl methacrylate composite nanofibers are prepared by electrospinning at room temperature, and then placed in a muffle furnace for calcination at 600°C to obtain zirconium oxide nanofibers.
[0014] Furthermore, the mass ratio of the zirconium oxide nanofibers to cilastatin sodium is 1:0.5-1.
[0015] Furthermore, the mass of the concentrated sulfuric acid used is 12-15% of the total mass of the nano-silicon dioxide particles and cilastatin sodium.
[0016] Furthermore, the heating reflux temperature is 90-110°C.
[0017] In some embodiments of the present invention, the mica powder has a fineness of 1200 mesh or above. Specifically, it can be purchased from Shifeng Mining Processing Plant in Lingshou County, Hebei Province, Anhui Ge Rui New Materials Technology Co., Ltd., etc.
[0018] In some embodiments of the present invention, the functional additive is at least one of a defoamer, a retarder, a water reducer, and an expander. The defoamer may be GS-938, GS-5820, GS-5881, GS-5018, etc. of GS Chemical; the retarder may be a borate, a phosphate, a gluconate, etc.; the water reducer may be a lignin sulfonate, a polycarboxylic acid, etc., with a water reduction rate of 10-20%; the expander may be at least one of anhydrous calcium sulfoaluminate, gypsum, and calcium oxide.
[0019] In some embodiments of the present invention, the grade of the rapid-hardening sulphoaluminate cement is 43 or above; the maximum particle size of the quartz sand is less than 2.38 mm, and the fineness modulus is between 1.5 and 2.0.
[0020] The preparation method of the nanofiber polymer mortar on the surface of the PS backing plate described above comprises the following steps: S1: mixing the rapid hardening sulphoaluminate cement, the intumescent flame retardant, the mica powder and the quartz sand in the raw material components uniformly to prepare a dry powder; S2: adding modified zirconia nanofibers and functional additives into the polymer emulsion and mixing them evenly to prepare a pre-dispersed emulsion; S3: Put the dry powder, pre-dispersed emulsion and water into a mixer and mix them for 3-5 minutes until they are uniform, thereby obtaining the nanofiber polymer mortar on the surface of the PS backing plate.
[0021] In the present invention, the surface of the modified zirconia nanofibers used carries carboxylic acid anions, cyclopropane groups, amide groups, etc. introduced by sodium cilastatin. The inventors have found through experiments that when the amount of sodium cilastatin introduced is too much, it will affect the dispersion uniformity of the resulting coating; and the bonding force between its double bonds and amide groups and cement and sand will be affected by the carboxylic acid anions, thereby weakening the bonding strength of the resulting polymer mortar to the PS backing board. Therefore, in the present invention, when preparing the modified zirconia nanofibers, the mass ratio of sodium cilastatin to zirconia nanofibers used is 0.5-1:1.
[0022] The present invention also provides the use of the above-mentioned nanofiber polymer mortar as a building material on the surface of a PS backing board.
[0023] Beneficial effects: Compared with the prior art, the present invention creatively uses sodium cilastatin to modify the surface of zirconium oxide nanofibers. On the one hand, the dispersion compatibility of zirconium oxide nanofibers in the polymer mortar system is improved. On the other hand, the bonding force formed between double bonds, amide groups and polymer emulsions, cement and sand is utilized to make the obtained nanofiber polymer mortar have excellent adhesion and frost resistance on the PS backing board. DETAILED DESCRIPTION
[0024] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0025] The following is an exemplary description of the preparation process of the modified zirconium oxide nanofibers used in the examples: Preparation of zirconia nanofibers: 1100 parts of tetrabutyl zirconate were dissolved in 100 parts of acetic acid, and then slowly added to a mixed aqueous solution containing 12.5% (m / V) polyvinyl pyrrolidone and 10% (m / V) polyvinyl pyrrolidone, and stirred evenly to obtain a spinning precursor solution. Under the conditions of room temperature 25°C and humidity 35%, the spinning voltage was controlled to be 12kV, and the distance between the spinning needle and the receiving plate was 10cm. Tetrabutyl zirconate-polyvinyl pyrrolidone-polyvinyl pyrrolidone composite nanofibers were prepared by electrospinning, and then placed in a muffle furnace at 600°C for calcination to obtain zirconium oxide nanofibers.
[0026] Modified zirconia nanofiber-1 100 g of zirconium oxide nanofibers were added to 100 ml of toluene to prepare a suspension, and then 50 g of cilastatin sodium was added. After stirring evenly at room temperature, 12 g of 98% concentrated sulfuric acid was added dropwise, and the mixture was heated to 90° C. and refluxed for 3 hours. After the reaction was completed, the reaction system was cooled to room temperature and centrifuged. The resulting precipitate was washed with ethanol and dried in an oven to obtain the modified zirconium oxide nanofiber-1.
[0027] Modified zirconia nanofiber-2 100 g of zirconium oxide nanofibers were added to 100 ml of n-hexane to prepare a suspension, and then 80 g of cilastatin sodium was added. After stirring evenly at room temperature, 24.5 g of 98% concentrated sulfuric acid was added dropwise, and the mixture was heated to 100° C. and refluxed for 4 hours. After the reaction was completed, the reaction system was cooled to room temperature and centrifuged. The resulting precipitate was washed with ethanol and dried in an oven to obtain the modified zirconium oxide nanofiber-2.
[0028] Modified zirconia nanofiber-3 100 g of zirconium oxide nanofibers were added to 100 ml of cyclohexane to prepare a suspension, and then 100 g of cilastatin sodium was added. After stirring evenly at room temperature, 30 g of 98% concentrated sulfuric acid was added dropwise, and the mixture was heated to 110° C. and refluxed for 5 hours. After the reaction was completed, the reaction system was cooled to room temperature and centrifuged. The obtained precipitate was washed with ethanol and dried in an oven to obtain the modified zirconium oxide nanofiber-3.
[0029] Zirconia Nanofiber-4 The preparation process is the same as that of modified zirconia nanofiber-3, except that the mass of cilastatin sodium used is 110 g.
[0030] Example 1 S1: 70 parts of fast-hardening sulphoaluminate cement, 7 parts of intumescent flame retardant (pentaerythritol: ammonium polyphosphate = 3:4), 5 parts of mica powder and 100 parts of quartz sand are mixed uniformly to obtain a dry powder; S2: 15 parts of modified zirconia nanofiber-1, 0.5 parts of defoamer GS-938, 2 parts of retarder sodium borate, 5 parts of water reducer sodium lignin sulfonate, are added to 50 parts of polymer emulsion (acrylate PRIMAL ST-954: epoxy emulsion JE-9064 = 1:0.5) and mixed evenly to prepare a pre-dispersed emulsion; S3: Put the dry powder, pre-dispersed emulsion and water (add in appropriate amount according to the required consistency) into a mixer and mix and stir for 3-5 minutes until a uniform state is obtained to obtain the nanofiber polymer mortar on the surface of the PS backing plate.
[0031] Example 2 S1: 90 parts of fast-hardening sulphoaluminate cement, 10 parts of intumescent flame retardant (pentaerythritol: ammonium polyphosphate = 3:2.5), 6 parts of mica powder and 150 parts of quartz sand are mixed uniformly to obtain a dry powder; S2: 25 parts of modified zirconia nanofiber-2, 2 parts of defoamer GS-5881, 2 parts of retarder sodium phosphate, 4 parts of water reducer sodium lignin sulfonate, are added to 60 parts of polymer emulsion (acrylate PRIMAL NW5118: epoxy emulsion GL1900 = 1.5:1) and mixed evenly to prepare a pre-dispersed emulsion; S3: Put the dry powder, pre-dispersed emulsion and water (add in appropriate amount according to the required consistency) into a mixer and mix and stir for 3-5 minutes until a uniform state is obtained to obtain the nanofiber polymer mortar on the surface of the PS backing plate.
[0032] Example 3 S1: 110 parts of fast-hardening sulphoaluminate cement, 14 parts of intumescent flame retardant (pentaerythritol: ammonium polyphosphate = 4:5.5), 7 parts of mica powder and 200 parts of quartz sand are mixed uniformly to obtain a dry powder; S2: 35 parts of modified zirconia nanofiber-3, 2 parts of defoamer GS-5881, 2 parts of retarder sodium gluconate, and 4 parts of water reducer sodium lignin sulfonate are added to 75 parts of polymer emulsion (acrylate PRIMAL TR407: epoxy emulsion KJ-998 = 2:1.1) and mixed evenly to prepare a pre-dispersed emulsion; S3: Put the dry powder, pre-dispersed emulsion and water (add in appropriate amount according to the required consistency) into a mixer and mix and stir for 3-5 minutes until a uniform state is obtained to obtain the nanofiber polymer mortar on the surface of the PS backing plate.
[0033] Example 4 Similar to Example 3, except that modified zirconia nanofiber-3 is replaced by modified zirconia nanofiber-4.
[0034] Example 5 Similar to Example 3, except that the acrylic emulsion PRIMAL TR407 is replaced by Hubei Xinyuhong BA201 (viscosity of 154 mPa·s).
[0035] Comparative Example 1 Similar to Example 3, except that the modified zirconia nanofiber-3 is replaced by an equal amount of zirconia nanofibers.
[0036] The polymer mortars obtained in the above Examples 1-5 and Comparative Example 1 were coated, and the following performance tests were performed after hardening: Dispersion stability: Mix the coating and let it stand for 24 hours to observe whether stratification occurs and calculate the sedimentation rate; 28d bonding strength: in accordance with the national standard GB / T11969-2008 "High-performance polymer modified dry-mixed mortar for construction"; Frost resistance: It is carried out in accordance with the national standard GB / T11969-2008 "High-performance polymer modified dry-mixed mortar for construction", and is measured by the mass loss rate.
[0037] The test results are detailed in Table 1:
[0038] From the results in Table 1, it can be seen that when the amount of the modifier sodium cilastatin used in the modified zirconia nanofibers exceeds the preferred ratio, the dispersion stability and bonding strength of the resulting polymer mortar will deteriorate (the sedimentation rate increases from 11.7% in Example 3 to 21.5%; the bonding strength weakens from 2.3MPa to 2.1MPa); when the viscosity of the acrylic emulsion used exceeds 100mPa·s, the bonding strength of the resulting polymer mortar will also deteriorate. This may be due to the increase in the molecular chains of sodium cilastatin, the enhanced molecular forces between the modified zirconia nanofibers, which affects the dispersion stability of the system. Due to poor dispersibility, the solidified layer cannot be hardened uniformly when it is formed, and the bonding strength is weakened when subjected to external forces; the increase in the viscosity of the acrylic emulsion will also affect the dispersion of the modified zirconia nanofibers in the system.
[0039] In summary, the nanofiber polymer mortar on the surface of the PS backing board provided by the present invention has excellent bonding strength and frost resistance on the PS backing board.
Claims
1. A PS backing board surface nanofiber polymer mortar, characterized in that: The invention comprises the following raw materials in parts by weight: 70-110 parts of fast-hardening sulphoaluminate cement, 50-75 parts of polymer emulsion, 7-14 parts of expansion flame retardant, 15-35 parts of modified zirconia nanofiber, 5-7 parts of mica powder, 100-200 parts of quartz sand and 0.5-10 parts of functional additive; wherein the modified zirconia nanofiber is obtained by modifying zirconia nanofiber with sodium cilastatin.
2. The nanofiber polymer mortar on the surface of the PS backing board according to claim 1, characterized in that: The polymer emulsion is obtained by mixing an acrylate emulsion and an epoxy emulsion in a mass ratio of 1-2:0.3-1.1; wherein the viscosity of the acrylate emulsion is less than 100 mPa·s, and the viscosity of the epoxy emulsion is 500-1500 mPa·s.
3. The nanofiber polymer mortar on the surface of the PS backing board according to claim 1, characterized in that: The intumescent flame retardant is obtained by mixing pentaerythritol and ammonium polyphosphate in a mass ratio of 3-4:2.5-5.
5.
4. The nanofiber polymer mortar on the surface of the PS backing board according to claim 1, characterized in that: The preparation process of the modified zirconia nanofiber comprises the following steps: adding the zirconia nanofiber into an organic solvent to prepare a suspension, then adding sodium cilastatin, stirring evenly at room temperature, dripping 98% concentrated sulfuric acid, heating under reflux, reacting for 3-5 hours, and after the reaction is completed, cooling the reaction system to room temperature and centrifuging, washing the obtained precipitate with ethanol, and drying it in an oven to obtain the modified zirconia nanofiber.
5. The nanofiber polymer mortar on the surface of the PS backing board according to claim 4, characterized in that: The organic solvent is at least one of benzene, toluene, xylene, n-hexane and cyclohexane.
6. The nanofiber polymer mortar on the surface of the PS backing board according to claim 4, characterized in that: The mass ratio of the zirconium oxide nanofibers to sodium cilastatin is 1:0.5-1; the mass of the concentrated sulfuric acid used is 12-15% of the total mass of the zirconium oxide nanofibers and sodium cilastatin; and the heating reflux temperature is 90-110°C.
7. The nanofiber polymer mortar on the surface of the PS backing board according to claim 4, characterized in that: The fineness of the mica powder is 1200 mesh or above.
8. The nanofiber polymer mortar on the surface of the PS backing board according to claim 1, characterized in that: The functional additive is at least one of an expander, a water reducer, a retarder and a defoamer.
9. The method for preparing nanofiber polymer mortar on the surface of PS backing board according to any one of claims 1 to 8, characterized in that: The following steps are involved: S1: mixing the rapid hardening sulphoaluminate cement, the intumescent flame retardant, the mica powder and the quartz sand in the raw material components uniformly to prepare a dry powder; S2: adding modified zirconia nanofibers and functional additives into the polymer emulsion and mixing them evenly to prepare a pre-dispersed emulsion; S3: Put the dry powder, pre-dispersed emulsion and water into a mixer and mix them for 3-5 minutes until they are uniform, thereby obtaining the nanofiber polymer mortar on the surface of the PS backing plate.
10. Application of the nanofiber polymer mortar on the surface of the PS backing board according to any one of claims 1 to 8 in the field of construction.
Citation Information
Patent Citations
Fiber-reinforced heat preservation and insulation material and preparation method thereof
CN104860577A
Seawater-resistant reinforced concrete admixture and preparation method thereof
CN111333366A
Polymer mortar and preparation method thereof
CN111620655A
Thermal insulation mortar and preparation method thereof
CN117164286A
High-ductility cement-based composite material and preparation method thereof
CN117209228A