Depth-controllable concrete surface etching agent and preparation method thereof

The depth-controllable concrete etcher addresses the issue of uncontrollable etching depth by using a temperature-sensitive component to release the etching agent at specific temperatures, ensuring uniform and stable etching for decorative concrete surfaces.

CN118851796BActive Publication Date: 2024-12-03CNBM ZHONGYAN TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411338190.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-25
Publication Date
2024-12-03
Estimated Expiration
2044-09-25

AI Technical Summary

Technical Problem

Existing concrete surface etchants face issues with uncontrollable etching depth due to temperature fluctuations and uneven penetration, affecting the decorative quality of concrete surfaces.

Method used

A depth-controllable concrete surface etcher composed of an etching component, special emulsion, and temperature-sensitive component, which ensures uniform penetration and controlled etching depth by releasing the etching component at specific temperatures.

Benefits of technology

Achieves uniform and controllable etching depth, enhancing decorative quality and stability of concrete surfaces, with improved storage and bonding properties.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of building material admixtures, and in particular to a depth-controllable concrete surface etchant and a preparation method thereof. An etching component with a retarding effect is used as a main ingredient, supplemented with a special emulsion and a temperature-sensitive component, and the etching component is dispersed and partially wrapped, so that not only the storage stability is improved, but also the penetration stability and bonding ability on the unhydrated surface of the concrete are improved to achieve uniform penetration, and the etching component is released after the concrete is heated to form an etching surface with controllable depth. A colorant is added to improve the coloring and decorative effect, and a preservative can extend the shelf life of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building material admixtures, in particular to a depth-controllable concrete surface etchant and a preparation method thereof. Background Art

[0002] Concrete is a commonly used engineering material, widely used in various buildings, roads, bridges, tunnels and other fields. Decorative concrete is based on cast-in-place concrete, with a colored surface layer and a protective layer attached.

[0003] The important link in the preparation process of decorative concrete is mainly through surface treatment, supplemented by creative design of color, texture, and grain, and the combination of patterns and colors. It can create the laying effect of various bricks, tiles, rocks, wood and other materials, which has the characteristics of beautiful graphics, lasting color, solid texture, wear resistance and durability.

[0004] Washed sand flooring is a common concrete surface treatment process. The common construction method is to construct a decorative layer on the concrete surface, that is, to integrate colored dry-mixed sand into the concrete at the corresponding position according to the design plan. However, it is not easy to expose the surface sand and gravel naturally after molding to form a unique decorative effect.

[0005] Therefore, in the initial setting stage of concrete, passivation treatment technology is often used, and in the subsequent maintenance and cleaning process, the ideal decorative effect is gradually presented. Therefore, concrete surface etchants are developed and applied, also known as surface retarders. They are sprayed on the surface of concrete in the mold to extend the setting time of cement slurry on the concrete surface. After the concrete under the surface hardens, the concrete surface is washed or polished to remove the retarded surface slurry and expose a certain depth of sand and gravel aggregates.

[0006] However, in actual application, the surface etching depth of washed sand is uneven. One important aspect is that its use process is still relatively extensive, and the depth of cement slurry on the concrete surface after spraying is uncontrollable. In addition, cement hydration in concrete will generate heat. In addition, the external temperature of concrete is not constant. Changes in temperature will directly affect the setting time of cement. When the temperature rises, the setting time of cement is shortened, and when the temperature decreases, the setting time of cement is prolonged. Therefore, the penetration depth of the concrete surface etchant is actually greatly affected by temperature, which makes the etching depth of the concrete surface difficult to control. This is a technical problem not found in the prior art. Summary of the invention

[0007] In view of the problems existing in the prior art, the present invention provides a depth-controllable concrete surface etcher, which uses an etching component with a retarding effect as a main ingredient, supplemented by a special emulsion and a temperature-sensitive component, to disperse and partially encapsulate the etching component, thereby improving not only the storage stability, but also the penetration stability and bonding ability on the unhydrated surface of the concrete, achieving uniform penetration, and releasing the etching component after the concrete is heated to form an etching surface with controllable depth. A colorant is added to improve the coloring and decorative effect, and a preservative can extend the shelf life of the product.

[0008] Specifically, the depth-controllable concrete surface etcher of the present invention is composed of the following raw materials in parts by weight: 10-15 parts of emulsion, 25-35 parts of etching components, 1-10 parts of temperature-sensitive components, 0.05-0.1 parts of colorants, 0.05-1 parts of preservatives, and 40-65 parts of water.

[0009] Preferably, the emulsion is at least one of vinyl acetate-ethylene copolymer emulsion, acrylate monomer copolymer emulsion, silicone resin modified acrylic polymer emulsion, and paraffin emulsion.

[0010] The surface etchant of the present invention adds a special emulsion and a temperature-sensitive component. The compounding of the emulsion and the temperature-sensitive component can make the etching component penetrate evenly and form a film on the concrete surface, and can prevent the evaporation of surface water, so that the etching component can be evenly distributed on the concrete surface. Compared with the slow-setting etching effect immediately produced by directly using the etching component, the present invention can achieve a deeper etching depth.

[0011] Preferably, the etching component is at least one of an organic retarder and an inorganic retarder.

[0012] Preferably, the organic retarder is at least one of citric acid, sodium citrate, sodium gluconate, sugar, sorbitol, maltodextrin and ethylenediaminetetramethylenephosphonic acid.

[0013] Preferably, the inorganic retarder is at least one of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, trisodium phosphate, and sodium dihydrogen phosphate.

[0014] Preferably, the temperature-sensitive component is at least one of polylactic acid-block-poly N-isopropylacrylamide, poly N-isopropylacrylamide copolymer, and isopropylacrylamide polymer hydrogel.

[0015] The amphiphilic block copolymer of the temperature-sensitive component of the present invention can self-assemble to form ordered aggregates through affinity-disappointment interactions. As the temperature rises, the isopropyl acrylamide products are transformed from a homogeneous system to a heterogeneous system. When the chemically cross-linked copolymer is heated to about 32°C, the volume suddenly shrinks, part of the hydrogen bonds are destroyed, and the solvation layer of the hydrophobic part of the macromolecular chain is destroyed. At this time, the macromolecule changes from a loose coil structure to a compact colloid structure, thereby generating temperature sensitivity.

[0016] During the heat release process of cement hydration, as the concrete gradually heats up, or as the concrete is affected by the external temperature, the temperature-sensitive component can be used as a micro-control system to release the coated etching component when the temperature rises, thereby obtaining an etching surface of almost equal depth and reducing the temperature effect; and the etching depth can be controlled by controlling the temperature of the concrete. For example, when the etching depth needs to be controlled to be shallow, the concrete temperature can be increased to the sensing temperature of the temperature-sensitive component in a short time. When the etching depth needs to be controlled to be deeper, the time it takes to increase the concrete temperature to the sensing temperature of the temperature-sensitive component can be extended.

[0017] Preferably, the colorant is at least one of an organic aqueous raw material and titanium dioxide.

[0018] Preferably, the preservative is at least one of benzoic acid, sodium benzoate, sorbic acid and potassium sorbate.

[0019] Preferably, the water is at least one of tap water and deionized water.

[0020] The present invention is named as a concrete surface etchant according to industry practice, but it can be used for surface etching of cement-based materials such as mortar, paste, concrete, etc.

[0021] The present invention also relates to a method for preparing the above-mentioned depth-controllable concrete surface etchant, which specifically comprises the following steps:

[0022] 1) Weigh each raw material by weight,

[0023] 2) Add the etching components and water into the constant temperature reactor and mix them evenly.

[0024] 3) Add the temperature-sensitive components into the reactor and mix evenly, add the emulsion and mix evenly.

[0025] 4) Add colorant and preservative into the reactor and mix well.

[0026] 5) Discharge and pack.

[0027] Preferably, in step 2), the temperature of the thermostatic reactor is 20-22°C.

[0028] The present invention has the following technical advantages:

[0029] 1. The present invention adopts emulsion and temperature-sensitive component compound to partially encapsulate the etching component, and has good permeability and stability.

[0030] 2. The surface etchant of the present invention has uniform and controllable etching depth, and the concrete surface etched by the surface etchant has good decorative effect.

[0031] 3. The surface etchant of the present invention has a simple preparation process, and the product has uniform texture, viscous state, good anti-sagging property, stable properties and long storage time. DETAILED DESCRIPTION

[0032] In order to characterize the technical effect of the present invention, a surface etching agent was prepared and its use effect was tested. During the test, the mix ratio of cement was 310kg / m 3 , fly ash 75 kg / m 3 , fine aggregate 864.8 kg / m 3 , coarse aggregate 975.2 kg / m 3 , total water 175 kg / m 3 , the surface of concrete with an admixture content of 1.5% was etched, and the concrete was tested in a standard environment of 25°C and a high-temperature environment of 45°C. During the test, the overall thickness of the specimen was measured with a vernier caliper after the concrete hardened and demolded. Then, the same water pressure, the same brushing tool, strength and brushing time were maintained, and the thickness of the specimen after brushing was measured again with a vernier caliper to compare the etching depth.

[0033] Example 1

[0034] The surface etchant is composed of the following raw materials in parts by weight: 15 parts of acrylic ester monomer copolymer emulsion, 10 parts of citric acid, 20 parts of sodium gluconate, 5 parts of isopropyl acrylamide polymer hydrogel, 0.07 parts of titanium dioxide, 0.07 parts of potassium sorbate, and 50 parts of water.

[0035] After testing, the surface etchant has a uniform texture and good anti-sagging performance. The etching depth in the standard environment is 0.60mm, and the etching is overall uniform. The etching depth in the high-temperature environment is 0.58mm, and the etching is overall uniform.

[0036] Example 2

[0037] The surface etchant is composed of the following raw materials in parts by weight: 5 parts of vinyl acetate-ethylene copolymer emulsion, 9 parts of acrylic ester monomer copolymer emulsion, 8 parts of sodium hexametaphosphate, 20 parts of ethylenediaminetetramethylenephosphonic acid, 6 parts of poly (N-isopropylacrylamide) copolymer, 0.05 parts of titanium dioxide, 0.08 parts of potassium sorbate and 52 parts of water.

[0038] After testing, the surface etchant has a uniform texture and good anti-sagging performance. The etching depth in the standard environment is 1.12mm, and the etching is overall uniform. The etching depth in the high-temperature environment is 1.15mm, and the etching is overall uniform.

[0039] Example 3

[0040] The surface etchant is composed of the following raw materials in parts by weight: 6 parts of vinyl acetate-ethylene copolymer emulsion, 9 parts of acrylic ester monomer copolymer emulsion, 12 parts of white sugar, 15 parts of ethylenediaminetetramethylenephosphonic acid, 3 parts of poly (N-isopropylacrylamide) copolymer, 4 parts of isopropylacrylamide polymer hydrogel, 0.06 parts of titanium dioxide, 0.07 parts of potassium sorbate and 51 parts of water.

[0041] After testing, the surface etchant has a uniform texture and good anti-sagging performance. The etching depth in the standard environment is 1.54mm, and the etching is overall uniform. The etching depth in the high-temperature environment is 1.52mm, and the etching is overall uniform.

[0042] Comparative Example 1

[0043] The surface etchant is composed of the following raw materials in parts by weight: 10 parts of citric acid, 20 parts of sodium gluconate, 0.07 parts of titanium dioxide, 0.07 parts of potassium sorbate, and 70 parts of water.

[0044] After testing, the surface etchant has a uniform texture and is easy to flow. The etching depth in the standard environment is 0.45mm, the etching is uneven, the etching depth in the high temperature environment is 0.26mm, and some surfaces are not etched.

[0045] Comparative Example 2

[0046] The surface etchant is composed of the following raw materials in parts by weight: 10 parts of citric acid, 20 parts of sodium gluconate, 5 parts of isopropyl acrylamide polymer hydrogel, 0.07 parts of titanium dioxide, 0.07 parts of potassium sorbate and 65 parts of water.

[0047] After testing, the surface etchant is easy to delaminate, the anti-sagging performance is average, the etching depth in the standard environment is 0.77mm, the etching is locally too deep, the etching depth in the high temperature environment is 0.50mm, and the etching is uneven.

[0048] Comparative Example 3

[0049] The surface etchant is composed of the following raw materials in parts by weight: 15 parts of acrylic ester monomer copolymer emulsion, 10 parts of citric acid, 20 parts of sodium gluconate, 0.07 parts of titanium dioxide, 0.07 parts of potassium sorbate, and 55 parts of water.

[0050] After testing, the surface etchant has a uniform texture, low viscosity, general anti-sagging properties, an etching depth of 0.51mm in a standard environment, and uneven etching; an etching depth of 0.24mm in a high-temperature environment, and uneven etching.

[0051] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A depth-controllable concrete surface etcher, characterized in that: The composition is composed of the following parts by weight of raw materials: 10-15 parts of emulsion, 25-35 parts of etching component, 1-10 parts of temperature-sensitive component, 0.05-0.1 parts of colorant, 0.05-1 parts of preservative, and 40-65 parts of water; The emulsion is a vinyl acetate - ethylene copolymer emulsion, an acrylate monomer copolymer emulsion, a silicone resin modified acrylic polymer emulsion, at least one paraffin emulsion; The etching component is at least one of an organic retarder and an inorganic retarder; The temperature-sensitive component is at least one of polylactic acid-block-poly N-isopropylacrylamide, poly N-isopropylacrylamide copolymer, and isopropylacrylamide polymer hydrogel.

2. The depth-controllable concrete surface etching agent according to claim 1, characterized in that: The organic retarder is at least one of citric acid, sodium citrate, sodium gluconate, sugar, sorbitol, maltodextrin and ethylenediaminetetramethylenephosphonic acid.

3. The depth-controllable concrete surface etching agent according to claim 2, characterized in that: The inorganic retarder is at least one of sodium tripolyphosphate, sodium hexametaphosphate, sodium pyrophosphate, trisodium phosphate, and sodium dihydrogen phosphate.

4. The depth-controllable concrete surface etching agent according to claim 1, characterized in that: The colorant is at least one of an organic water-based raw material and titanium dioxide.

5. The depth-controllable concrete surface etching agent according to claim 1, characterized in that: The preservative is at least one of benzoic acid, sodium benzoate, sorbic acid and potassium sorbate.

6. The depth-controllable concrete surface etching agent according to claim 1, characterized in that: The water is at least one of tap water and deionized water.

7. The method for preparing the depth-controllable concrete surface etching agent according to any one of claims 1 to 6, characterized in that: The steps include: 1) Weigh each raw material by weight, 2) Add the etching components and water into the constant temperature reactor and mix them evenly. 3) Add the temperature-sensitive components into the reactor and mix evenly, add the emulsion and mix evenly. 4) Add colorant and preservative into the reactor and mix well. 5) Discharge and pack.