Composite ink material, preparation method and application thereof, and method for preparing heat conduction part through ink direct writing 3D printing
By optimizing the ratio of silicone rubber resin, thermally conductive filler and curing agent in thermally conductive composite materials, and performing ultrasonic centrifugation treatment, the contradiction between filling amount and mechanical properties in the preparation of thermally conductive composite materials is solved, and high thermal conductivity under low filling amount is achieved. And high elasticity effect, suitable for ink direct writing 3D printing, broadening the molding method of composite materials.
Patent Information
- Application Number
- CN202411102349.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-12
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-12
AI Technical Summary
In the preparation process of existing thermally conductive composite materials, there is a problem that high filling amount leads to a decrease in the mechanical properties of the material, and the viscosity of the printing ink is difficult to control, which affects the 3D printing effect.
Using a preparation method of composite ink materials, including a specific combination of silicone rubber resin, thermally conductive filler and curing agent, and through ultrasonic and centrifugal defoaming treatment, an ink with excellent rheological properties and supportability is prepared for direct ink printing. Write about 3D printing to prepare thermally conductive parts.
It achieves the acquisition of thermally conductive parts with high thermal conductivity and high elasticity under low filling volume, expands the selection range of thermally conductive composite materials with excellent performance in 3D printing, and the process conditions are mature and suitable for large-scale production.
Smart Images

Figure CN118852879A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of 3D printing polymer technology, and in particular to a composite ink material, a preparation method and application thereof, and a method for preparing a thermal conductive part by direct ink writing 3D printing. Background Art
[0002] With the rapid increase in power density of modern electronics, efficient heat dissipation has become an emerging demand for electronic devices including communications, information and energy storage technologies, because the faster the microprocessor cools, the faster it can run, and therefore the better the operating performance. Ultra-high-speed high-frequency devices generate a lot of heat in a small local area, resulting in hot spots with operating power more than ten times higher than its average value. Although the operating temperature in most other areas is relatively low, devices with low thermal conductivity may experience performance deterioration or even failure. Thermally conductive composite materials are materials that can quickly transfer a large amount of heat and can effectively protect and extend the service life of electronic devices. Thermally conductive composite materials mainly include thermally conductive matrix, such as silicone rubber resin, epoxy resin, etc. There are three main types of thermal conductive fillers: metal, inorganic particles and carbon materials. The current limitation of thermally conductive composite materials lies in their preparation process. Most of the current thermally conductive composite materials are manufactured by die casting. In order to obtain high thermal conductivity, a large amount of thermally conductive fillers are usually added, but the high filling amount will lead to the loss of mechanical properties of the material. In order to obtain thermally conductive composite materials with excellent performance, it is necessary to obtain higher thermal conductivity under low filling conditions.
[0003] In recent years, three-dimensional (3D) printing technology of various materials has received increasing attention because it has the potential to provide unique features that cannot be achieved by traditional manufacturing methods, such as simplified manufacturing processes, increased design freedom, novel form factors, reduced weight, and reduced prototype and manufacturing costs. General 3D printing methods include extrusion printing (FDM, DIW, etc.), inkjet printing, and light-curing printing. Among them, DIW is also called automatic injection molding. The ink material is stored in a barrel and connected to a 3-axis CNC platform with a nozzle. The ink is extruded and formed on the surface through a screw or pneumatic pressure control device. It can be modeled through CAD software and input into the printer for pattern construction. The parameters and environment during the printing process will have a great impact on the molding of the material. Compared with other printing technologies, DIW technology has fewer requirements for materials. It only needs to meet the rheological properties required for printing to be printed. It is especially suitable for the printing of thermosetting materials, such as silicone rubber. However, printing ink also has problems such as difficult viscosity control and ink support during printing.
[0004] Based on the defects of current printing ink, it is necessary to improve this. Summary of the invention
[0005] In order to solve the problems in the above background technology, the present invention provides a composite ink material, a preparation method and application thereof, and a method for preparing a thermal conductive part by ink direct writing 3D printing. The composite ink material has good rheology and support properties, and the printed thermal conductive part has good flexibility and thermal conductivity.
[0006] In order to achieve the above-mentioned purpose, the present invention is implemented by adopting the following technical measures.
[0007] In a first aspect, the present invention provides a composite ink material, comprising the following components in parts by weight: ≥600 parts of silicone rubber resin, ≤400 parts of thermal conductive filler, and ≤70 parts of curing agent;
[0008] The total weight of the silicone rubber resin, the thermal conductive filler and the curing agent is 1000 parts.
[0009] Preferably, the silicone rubber resin includes at least one of methyl silicone rubber, methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber and fluorosilicone rubber.
[0010] Preferably, the thermally conductive filler includes at least one of boron nitride, magnesium oxide and aluminum oxide.
[0011] Preferably, the particle size of the thermally conductive filler is 1 to 10 μm;
[0012] And / or, the composite ink material comprises the following components in parts by weight: 600-680 parts of silicone rubber resin, 250-350 parts of thermal conductive filler, and 50-70 parts of curing agent;
[0013] The total weight of the silicone rubber resin, the thermal conductive filler and the curing agent is 1000 parts.
[0014] In a second aspect, the present invention further provides a method for preparing the composite ink material, comprising the following steps:
[0015] Adding thermal conductive filler to silicone rubber resin to obtain silicone rubber mixed liquid;
[0016] A curing agent is added to the silicone rubber mixed liquid, and after mixing, ultrasonication and centrifugation are performed to remove bubbles, so as to obtain a composite ink material.
[0017] Preferably, the centrifugal rate is 1000-6000 r / min and the centrifugal time is 5-30 min.
[0018] Preferably, the ultrasonic time is 5 to 30 minutes.
[0019] In a third aspect, the present invention further provides an application of the composite ink material or the composite ink material prepared by the preparation method in preparing thermal conductive parts by ink direct writing 3D printing.
[0020] In a fourth aspect, the present invention further provides a method for preparing a thermal conductive member by ink direct writing 3D printing, comprising the following steps:
[0021] The composite ink material or the composite ink material prepared by the preparation method is loaded into the syringe of the ink direct writing 3D printing device;
[0022] Set the printing process parameters and print the thermal conductor.
[0023] Preferably, the printing process parameters are: printing extrusion pressure is 0.5-3Mpa, the diameter of the printing needle is 0.7-1.2mm, and the printing speed is 1-3mm / s.
[0024] The present invention has the following beneficial effects compared with the prior art:
[0025] 1. The composite ink material of the present invention comprises a silicone rubber resin, a thermally conductive filler and a curing agent component. The composite ink material of the present invention has excellent shear-thinning rheological properties, good printing ability, good dispersibility, and the printed thermally conductive part has good thermal conductivity and flexibility; in addition, by adjusting the printing speed, the orientation degree of the thermally conductive particles in the composite material can be accurately adjusted, thereby adjusting the thermal conductivity of the obtained thermally conductive part;
[0026] 2. The composite ink material prepared by the present invention is used for ink direct writing printing. The obtained product is a composite material with low filling amount, high thermal conductivity and high elasticity, which is difficult to prepare by other printing methods, and has good tensile strength, which expands the selection range of thermal conductive composite materials with excellent performance for 3D printing;
[0027] 3. The composite ink material prepared by the present invention has moderate viscosity and good supporting force, making it suitable for ink direct writing printing processing, broadening the preparation method of composite material ink, and expanding the molding method of silicone rubber-based composite materials; the composite material ink prepared by the present invention can control the thermal conductivity in different directions by controlling the printing speed and method; the composite ink material preparation method of the present invention has mature process conditions, simple preparation process, low manufacturing cost, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the prior art descriptions. Obviously, the drawings described below are only some embodiments of the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0029] Figure 1 This is a SEM image of the thermal conductive member sample obtained in Application Example 1;
[0030] Figure 2 A schematic diagram of preparing a heat-conducting member by 3D printing of the present invention;
[0031] Figure 3 The thermal conductivity diagram of the thermally conductive member samples obtained in Application Examples 1 to 4;
[0032] Figure 4 The thermal conductivity diagram of the samples of the heat conducting member obtained in Application Examples 2, 5-6;
[0033] Figure 5 The thermal weight loss test diagram of the thermal conductive member samples obtained in Application Examples 2, 5-6;
[0034] Figure 6 The elongation at break diagram of the thermal conductive member samples obtained in Application Examples 1 to 3;
[0035] Figure 7 is the tensile stress diagram of the thermal conductive member samples obtained in Application Examples 1 to 3;
[0036] Figure 8 is a graph showing the change in viscosity of the composite ink material obtained in Examples 1 to 3 as a function of shear rate;
[0037] Fig. 9 The storage modulus and loss modulus of the composite ink material obtained in Examples 1 to 3 vary with oscillation strain. DETAILED DESCRIPTION
[0038] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] It should be noted that the order of description of the following embodiments is not intended to limit the preferred order of the embodiments. In addition, in the description of the present application, the term "including" means "including but not limited to". Various embodiments of the present invention may be in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity and should not be understood as a rigid limitation on the scope of the present invention; therefore, it should be considered that the range description has specifically disclosed all possible sub-ranges and single numerical values within the range. For example, it should be considered that the range description from 1 to 6 has specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the numbered ranges, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated in this article, it is meant to include any cited numbers (fractions or integers) within the indicated range.
[0040] The present invention provides a composite ink material, comprising the following components in parts by weight: silicone rubber resin ≥ 600 parts, thermal conductive filler ≤ 400 parts, curing agent ≤ 70 parts;
[0041] The total weight of the silicone rubber resin, the thermal conductive filler and the curing agent is 1000 parts.
[0042] In some embodiments, the silicone rubber resin can be selected from any type and model of silicone rubber resin sold on the market, or silicone rubber resin prepared according to the prior art. For better explanation and to provide a preferred technical solution, the silicone rubber resin is selected to include at least one of methyl silicone rubber, methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, and fluorosilicone rubber.
[0043] In some embodiments, the thermally conductive filler is selected as a thermally conductive filler that can be prepared as a composite material with silicone rubber resin in the prior art, specifically, a traditional processing field (such as compression molding, casting molding, etc.). In order to better illustrate the present invention and provide a preferred technical solution, the thermally conductive filler includes at least one of boron nitride, magnesium oxide, and aluminum oxide. It should be noted that in order to better disperse the filler in the matrix, the thermally conductive filler needs to be selected as a powder, preferably a thermally conductive filler powder with a particle size of 1 to 10 μm.
[0044] In some embodiments, the composite ink material includes the following components in parts by weight: silicone rubber resin ≥ 600 parts, thermal conductive filler ≤ 400 parts, curing agent ≤ 60 parts;
[0045] The sum of the weight parts of silicone rubber resin, thermal conductive filler and curing agent is 1000 parts;
[0046] In some embodiments, the inventors, through comparative test research results, found that when the addition amount of thermal conductive filler is 300 parts, the obtained composite ink material has the best rheological properties. After 3D printing, the thermal conductive products of the ink have good thermodynamic properties and good mechanical properties. When the number of fillers exceeds 400 parts, the printability of the ink material will be greatly reduced, and the 3D printing processing of the thermal conductive products cannot be carried out.
[0047] In some embodiments, the composite ink material includes the following components in parts by weight: 600-680 parts of silicone rubber resin, 250-350 parts of thermal conductive filler, and 50-70 parts of curing agent;
[0048] The total weight of the silicone rubber resin, the thermal conductive filler and the curing agent is 1000 parts.
[0049] Specifically, in some embodiments, preferably, the thermally conductive filler includes: 50 parts of magnesium oxide and 200-300 parts of boron nitride.
[0050] In some embodiments, the inventors conducted comparative experiments and found that the most suitable printing performance of the ink was obtained when the addition amount of boron nitride was 25%wt and the addition amount of magnesium oxide was 5%wt.
[0051] Furthermore, under the conditions of the composite ink material obtained above, it is preferred that printing is performed using a 0.7 mm needle and at a pressure of 1.5 MPa, the printing speed can be adjusted (1 to 10 mm / s), and the resulting thermal conductor will also have different vertical and in-plane thermal conductivities.
[0052] Generally, the composite ink material of the present invention may also be added with other processing aids such as antioxidants, flame retardants, anti-aging agents, etc. known in the prior art, and other functional fillers such as carbon-based fillers, conductive fillers polyaniline, etc. may also be added according to factors such as actual technical purposes or processing conditions. Those skilled in the art may refer to the prior art to determine the amount of the above-mentioned other functional fillers. However, the premise is that these processing aids and fillers shall not have an adverse effect on the realization of the purpose of the present invention and the achievement of the excellent effects of the present invention.
[0053] Based on the same inventive concept, the present invention also provides a method for preparing the above-mentioned composite ink material, comprising the following steps:
[0054] S1, adding thermal conductive filler to silicone rubber resin to obtain silicone rubber mixed liquid;
[0055] S2. Add a curing agent to the silicone rubber mixture, mix, and then perform ultrasonic and centrifugation to remove bubbles to obtain a composite ink material.
[0056] In some embodiments, the sufficient mixing in step S1 is to allow the thermally conductive filler to be fully dispersed in the silicone rubber matrix to prevent the thermally conductive filler from agglomerating, thereby affecting the thermodynamic properties of the final thermally conductive component. Those skilled in the art can select a suitable mixing and stirring process in the prior art according to the actual process conditions and the weight of the raw materials to be mixed. In order to better illustrate the present invention and provide a technical solution for reference, sufficient mixing can be performed by mixing with a PTFE stirring paddle at a speed of 200 to 300 r / min for 1 to 5 hours.
[0057] In some embodiments, the defoaming treatment in step S2 is performed because air is easily introduced into the mixed liquid during the actual stirring process, and bubbles are generated to eliminate the influence of bubbles in the mixed liquid. In order to better illustrate the present invention and provide a technical solution for reference, a curing agent is added to the silicone rubber mixed liquid, mixed and loaded into a barrel, and then placed in an ultrasonic instrument. The ultrasonic time is 5 to 30 minutes, and the ultrasonic temperature is controlled at 10 to 50°C. After the ultrasonic is completed, the barrel is placed in a centrifuge and the centrifugal speed is set to 1000 to 6000 r / min for 5 to 30 minutes.
[0058] In some embodiments, when the amount of silicone rubber added is 5 to 10 g and the amount of thermal conductive filler added is 3 to 5 g, the shear rate is 1 to 1000 s at room temperature. -1 , the viscosity is 1~300Pa·s, which meets the requirements of ink direct writing printing and has printability.
[0059] In some embodiments, the viscosity of the composite ink material prepared by the present invention is 100-3000 Pa·s, and the storage modulus and loss modulus are 10 2 ~10 5 Pa.
[0060] It should be noted that the viscosity defined in the technical solution of the present invention is obtained through a large number of explorations and experiments to satisfy the printability of the silicone rubber resin matrix / thermal conductive filler system. Those skilled in the art should know that in order to satisfy the requirement of the ink material to be printable for direct ink printing, the required viscosity coefficient standard should be changed according to the specific ink material used, and viscosity is not the only criterion for measuring whether the ink material is printable.
[0061] Based on the same inventive concept, the present invention also provides an application of the above-mentioned composite ink material or the composite ink material prepared by the above-mentioned preparation method in preparing a thermal conductive part by ink direct writing 3D printing.
[0062] The main invention of the present invention is to achieve high thermal conductivity of thermal conductive filler under low filling amount conditions. At the same time, the addition of thermal conductive filler satisfies the ink support required when the silicone rubber resin matrix is used as the ink material. At the same time, silicone rubber resin is selected as the matrix, and it still has good flexibility when part of the thermal conductive filler is added. After defoaming treatment, the ink material has the characteristics of good printing ability, good dispersibility, and strong supporting force. It is applied to ink direct writing printing, and the printed thermal conductive parts have good flexibility and thermal conductivity.
[0063] It is worth noting that the above-mentioned inventive characteristics of the present invention are only applicable to ink direct writing printing, and other 3D printing processes are not applicable to the present invention. For example, when the thermal conductive filler is 30wt%, the selective laser sintering 3D printing technology will not be able to produce good bonding behavior due to the excessively high filler content, while the technology of the present invention will not have the above-mentioned defects.
[0064] The composite ink material of the present invention has excellent shear-thinning rheological properties, good printing ability, good dispersibility, and the printed thermal conductive parts have good thermal conductivity and flexibility; in addition, by adjusting the printing speed, the orientation degree of the thermal conductive particles in the composite material can be accurately adjusted, thereby adjusting the thermal conductivity of the obtained thermal conductive parts.
[0065] Based on the same inventive concept, the present invention also provides a method for preparing a thermal conductive member by ink direct writing 3D printing, comprising the following steps:
[0066] S1, loading the above composite ink material into the syringe of the ink direct writing 3D printing device;
[0067] S2. Setting printing process parameters and printing the thermal conductive part.
[0068] In some embodiments, the composite ink material prepared according to the technical solution of the present invention can generally adopt the same process parameters as the ink direct writing printing silicone rubber-based composite material in the prior art. In order to better illustrate the invention, the present invention provides a specific method for reference, and the composite ink material prepared by the technical solution of the present invention is used for ink direct writing, wherein the printing process parameters are: printing extrusion pressure of 0.5-3Mpa, printing needle diameter of 0.7-1.2mm, and printing speed of 1-10mm / s.
[0069] In some embodiments, during the printing process, a heating device is added to the printing substrate to quickly shape the composite ink material after extrusion to prevent the ink from collapsing. The resulting thermal conductive sample has good shape retention.
[0070] The present invention has the following beneficial effects:
[0071] 1. The composite ink material prepared by the present invention is used for ink direct writing printing. The obtained product is a composite material with low filling amount, high thermal conductivity and high elasticity, which is difficult to prepare by other printing methods, and has good tensile strength, which expands the selection range of thermal conductive composite materials with excellent performance for 3D printing;
[0072] 2. The composite ink material prepared by the present invention has moderate viscosity and good supporting force, making it suitable for ink direct writing printing processing, broadening the preparation method of composite material ink and expanding the molding method of silicone rubber-based composite materials;
[0073] 3. The composite material ink prepared by the present invention can adjust the thermal conductivity in different directions by controlling the printing speed and method;
[0074] 4. The preparation method of the present invention has mature process conditions, simple preparation process, low manufacturing cost and is suitable for large-scale production.
[0075] The following further illustrates the composite ink material of the present application, its preparation method and application, and the method for preparing a thermal conductor by direct ink writing 3D printing with specific examples. This section further illustrates the content of the present invention in conjunction with specific examples, but should not be construed as a limitation of the present invention. Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art. Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art.
[0076] The following examples mainly include experimental raw materials and reagents
[0077] Polydimethylsilicone rubber (PDMS) and curing agent are both SLYGARD 184 (PDMS is a two-component kit product composed of liquid components, including PDMS matrix and curing agent), density 1.04g / cm 3 , specific heat capacity 1.363 j / g·K, produced by Dow corning company in the United States;
[0078] Boron nitride (BN): density 2.29g / cm 3 , specific heat capacity 0.794 j / g·K, particle size 5-10 μm, hexagonal lamellar structure, produced by MacLean Company;
[0079] Magnesium oxide (MgO): density 3.58g / cm -3 , specific heat capacity 0.92j / g·K, particle size 1~5μm, spherical structure, produced by Bengbu Kexing Nano Technology Co., Ltd.
[0080] Testing and Characterization
[0081] Scanning electron microscopy analysis
[0082] The morphology of the thermal conductive sample was observed using a scanning electron microscope (SIGMA500, Beijing OPTON Optical Technology Co., Ltd.); the thermal conductive sample was quenched in liquid nitrogen, and the observation surface was vacuum-sprayed with gold.
[0083] Thermal conductivity test
[0084] The thermal conductivity coefficient of the heat conducting component is measured by a laser flash method thermal conductivity measuring instrument (unit: mm 2 / s) for testing. The thermal conductivity λ (W / m·K) is calculated by the following formula:
[0085] λ=α·ρ·C p
[0086] Where: The thermal diffusion coefficient α of the silicone rubber composite ink material is measured by a laser thermal conductivity meter, the test temperature is 25°C, and the density ρ of the silicone rubber composite ink material is calculated according to the formula:
[0087] ρ=f1ρ1+f2ρ2
[0088] Where: f1, f2 represent the volume fraction of the matrix (i.e. the cured silicone rubber resin) and the thermal conductive filler, respectively, ρ2, ρ2 represent the density of the matrix and the thermal conductive filler, respectively. p (Unit: J / g·K) Calculated according to the formula:
[0089] C p =ω1C p1 +ω2C p2
[0090] Where: ω1 and ω2 represent the mass fraction of the matrix (i.e. the cured silicone rubber resin) and the thermal conductive filler, respectively. p1 , C p1 represent the specific heat capacity of the matrix and thermal conductive filler respectively.
[0091] The thermal conductivity in the plane direction is tested by cutting and grinding the printed 20×20×1.5mm thermal conductive products into 10×10×1mm sheet samples. The thermal conductivity in the vertical direction is tested by cutting and grinding the printed 10×15×12mm thermal conductive products into 10×10×1mm sheet samples in the vertical direction. All samples must be sprayed with graphite coating before testing, and then placed in the corresponding fixture for testing after drying. Before testing, the graphite coating must be sprayed first, and then placed in the corresponding fixture for testing after drying.
[0092] Mechanical properties test
[0093] The mechanical properties of the thermal conductor were tested by an INSTRON68TM-10 tensile testing machine, and the tensile properties at break were tested at a tensile rate of 500 mm / min.
[0094] Thermal Weight Loss Test
[0095] A thermogravimetric analyzer (CLY01-TGA1, Wuhan Huinengzhi Technology Co., Ltd.) was used to carry out thermal weight loss test on the thermal conductive parts. The samples were first dried and placed in an alumina crucible for testing. The sample mass was about 5 mg, the test temperature range was 30°C to 800°C, the test rate was 10°C / min, and the test atmosphere was nitrogen.
[0096] Rheological test In this experiment, a strain-controlled rotational rheometer (DH-2) was used to test the ink rheology. A fixture with a diameter of 15 mm was used to test the ink rheology. The rheological characterization of the composite ink material was carried out in flow mode and oscillation mode. -3 -1000s -1 The change of apparent viscosity with shear rate in the range. Under the oscillation mode, with a fixed frequency of 1HZ, the oscillation strain varies in the range of 0.001 to 10%, which characterizes the change law of the linear viscoelastic region of the ink in this range as well as the storage modulus and loss modulus.
[0097] Example 1
[0098] This embodiment provides a composite ink material, including the following components in parts by weight:
[0099] 650 parts of silicone rubber resin, 300 parts of thermal conductive filler, 50 parts of curing agent;
[0100] Wherein, the silicone rubber resin is polydimethyl silicone rubber;
[0101] The thermal conductive filler includes magnesium oxide and boron nitride, with magnesium oxide accounting for 50 parts and boron nitride accounting for 250 parts.
[0102] This embodiment also provides a method for preparing the composite ink material, comprising the following steps:
[0103] S1, adding the thermal conductive filler into the silicone rubber resin and mixing at a speed of 300 r / min for 3 hours to obtain a silicone rubber mixed liquid;
[0104] S2, adding a curing agent to the silicone rubber mixture, mixing, ultrasonicating, and centrifuging to remove bubbles, and obtaining a composite ink material;
[0105] The ultrasonic time was 10 min, the ultrasonic temperature was controlled at 25°C, the centrifugal speed was 3000 r / min, and the centrifugal time was 5 min.
[0106] The composite ink material prepared in Example 1 was heated at a shear rate of 100 s at room temperature (25 °C). -1When the viscosity is 1000Pa·s.
[0107] Application Example 1
[0108] This application example provides a method for preparing a thermal conductive member by ink direct writing 3D printing, comprising the following steps:
[0109] S1. Loading the composite ink material prepared in Example 1 into the syringe of an ink direct writing 3D printing device;
[0110] S2, setting printing process parameters, and printing the heat conducting part;
[0111] Among them, the printing process parameters are: printing extrusion pressure is 1.5Mpa, the diameter of the printing needle is 0.7mm, and the printing speed is 2mm / s;
[0112] According to the method in the above-mentioned application example 1, rectangular heat-conducting parts with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively, thermally conductive parts with a length, width and height of 10 mm, 15 mm and 12 mm respectively, and rectangular heat-conducting parts with a length, width and height of 40 mm, 40 mm and 1 mm respectively were printed.
[0113] After testing, the thermal conductivity of the prepared rectangular heat-conducting parts with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively and the thermal conductivity of the heat-conducting parts with a length, width and height of 10 mm, 15 mm and 12 mm respectively are as follows: Figure 3 shown.
[0114] After testing, the prepared rectangular heat-conducting member with a length, width and height of 40 mm, 40 mm and 1 mm respectively was tested at a tensile rate of 500 mm / min. The elongation at break and the tensile strength were as shown in the attached figure. Figure 6 and Figure 7 shown.
[0115] Application Example 2
[0116] This application example provides a method for preparing a thermal conductive member by ink direct writing 3D printing, comprising the following steps:
[0117] S1. Loading the composite ink material prepared in Example 1 into the syringe of an ink direct writing 3D printing device;
[0118] S2, setting printing process parameters, and printing the heat conducting part;
[0119] Among them, the printing process parameters are: printing extrusion pressure is 1.5Mpa, the diameter of the printing needle is 0.7mm, and the printing speed is 2.5mm / s;
[0120] According to the method in the above-mentioned application example 1, rectangular heat-conducting parts with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively, thermally conductive parts with a length, width and height of 10 mm, 15 mm and 12 mm respectively, and rectangular heat-conducting parts with a length, width and height of 40 mm, 40 mm and 1 mm respectively were printed.
[0121] After testing, the thermal conductivity of the prepared rectangular heat-conducting parts with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively and the thermal conductivity of the heat-conducting parts with a length, width and height of 10 mm, 15 mm and 12 mm respectively are as follows: Figure 3 shown.
[0122] After testing, the prepared rectangular heat-conducting member with a length, width and height of 40 mm, 40 mm and 1 mm respectively has a breaking elongation and tensile strength as shown in the attached figure under a tensile rate of 500 mm / min. Figure 6 , Figure 7 shown.
[0123] Application Example 3
[0124] This application example provides a method for preparing a thermal conductive member by ink direct writing 3D printing, comprising the following steps:
[0125] S1. Loading the composite ink material prepared in Example 1 into the syringe of an ink direct writing 3D printing device;
[0126] S2, setting printing process parameters, and printing the heat conducting part;
[0127] Among them, the printing process parameters are: printing extrusion pressure is 1.5Mpa, the diameter of the printing needle is 0.7mm, and the printing speed is 3mm / s;
[0128] According to the method in the above-mentioned application example 1, rectangular heat-conducting parts with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively, thermally conductive parts with a length, width and height of 10 mm, 15 mm and 12 mm respectively, and rectangular heat-conducting parts with a length, width and height of 40 mm, 40 mm and 1 mm respectively were printed.
[0129] After testing, the thermal conductivity of the prepared rectangular heat-conducting parts with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively and the thermal conductivity of the heat-conducting parts with a length, width and height of 10 mm, 15 mm and 12 mm respectively are as follows: Figure 3 shown.
[0130] After testing, the prepared rectangular heat-conducting member with a length, width and height of 40 mm, 40 mm and 1 mm respectively has a breaking elongation and tensile strength as shown in the attached figure under a tensile rate of 500 mm / min. Figure 6 , Figure 7shown.
[0131] Application Example 4
[0132] This application example provides a method for preparing a thermal conductive member by ink direct writing 3D printing, comprising the following steps:
[0133] S1. Loading the composite ink material prepared in Example 1 into the syringe of an ink direct writing 3D printing device;
[0134] S2, setting printing process parameters, and printing the heat conducting part;
[0135] Among them, the printing process parameters are: printing extrusion pressure is 1.5Mpa, the diameter of the printing needle is 0.7mm, and the printing speed is 1.5mm / s;
[0136] According to the method in the above-mentioned application example 1, rectangular heat-conducting parts with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively, thermally conductive parts with a length, width and height of 10 mm, 15 mm and 12 mm respectively, and rectangular heat-conducting parts with a length, width and height of 40 mm, 40 mm and 1 mm respectively were printed.
[0137] After testing, the thermal conductivity of the prepared rectangular heat-conducting parts with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively and the thermal conductivity of the heat-conducting parts with a length, width and height of 10 mm, 15 mm and 12 mm respectively are as follows: Figure 3 shown.
[0138] After testing, the prepared rectangular heat-conducting member with a length, width and height of 40 mm, 40 mm and 1 mm respectively has a breaking elongation and tensile strength as shown in the attached figure under a tensile rate of 500 mm / min. Figure 6 , Figure 7 shown.
[0139] Example 2
[0140] This embodiment provides a composite ink material, including the following components in parts by weight:
[0141] 680 parts of silicone rubber resin, 250 parts of thermal conductive filler, 70 parts of curing agent;
[0142] Wherein, the silicone rubber resin is polydimethyl silicone rubber;
[0143] The thermal conductive filler includes magnesium oxide and boron nitride, wherein the magnesium oxide accounts for 50 parts and the boron nitride accounts for 200 parts.
[0144] This embodiment also provides a method for preparing the composite ink material, comprising the following steps:
[0145] S1, adding the thermal conductive filler into the silicone rubber resin and mixing at a speed of 300 r / min for 3 hours to obtain a silicone rubber mixed liquid;
[0146] S2, adding a curing agent to the silicone rubber mixture, mixing, ultrasonicating, and centrifuging to remove bubbles, and obtaining a composite ink material;
[0147] The ultrasonic time was 10 min, the ultrasonic temperature was controlled at 25°C, the centrifugal speed was 3000 r / min, and the centrifugal time was 5 min.
[0148] The composite ink material prepared in Example 2 has a shear rate of 100 s at room temperature. -1 When the viscosity is 200Pa·s.
[0149] Application Example 5
[0150] This application example provides a method for preparing a thermal conductive member by ink direct writing 3D printing, comprising the following steps:
[0151] S1. Loading the composite ink material prepared in Example 2 into the syringe of an ink direct writing 3D printing device;
[0152] S2, setting printing process parameters, and printing the heat conducting part;
[0153] Among them, the printing process parameters are: printing extrusion pressure is 1Mpa, the diameter of the printing needle is 0.7mm, and the printing speed is 2mm / s;
[0154] According to the method in the above-mentioned application example 1, a rectangular heat-conducting member with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively and a heat-conducting member with a length, width and height of 10 mm, 15 mm and 12 mm respectively were printed.
[0155] After testing, the thermal conductivity of the prepared rectangular heat-conducting parts with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively and the thermal conductivity of the heat-conducting parts with a length, width and height of 10 mm, 15 mm and 12 mm respectively are as follows: Figure 4 shown.
[0156] Example 3
[0157] This embodiment provides a composite ink material, including the following components in parts by weight:
[0158] 600 parts of silicone rubber resin, 350 parts of thermal conductive filler, 50 parts of curing agent;
[0159] Wherein, the silicone rubber resin is polydimethyl silicone rubber;
[0160] The thermal conductive filler includes magnesium oxide and boron nitride, wherein the magnesium oxide accounts for 50 parts and the boron nitride accounts for 300 parts.
[0161] This embodiment also provides a method for preparing the composite ink material, comprising the following steps:
[0162] S1, adding the thermal conductive filler into the silicone rubber resin and mixing at a speed of 300 r / min for 3 hours to obtain a silicone rubber mixed liquid;
[0163] S2, adding a curing agent to the silicone rubber mixture, mixing, ultrasonicating, and centrifuging to remove bubbles, and obtaining a composite ink material;
[0164] The ultrasonic time was 10 min, the ultrasonic temperature was controlled at 25°C, the centrifugal speed was 3000 r / min, and the centrifugal time was 5 min.
[0165] The composite ink material prepared in Example 1 has a shear rate of 100 s at room temperature. -1 When the viscosity is 2500Pa·s.
[0166] Application Example 6
[0167] This application example provides a method for preparing a thermal conductive member by ink direct writing 3D printing, comprising the following steps:
[0168] S1. Loading the composite ink material prepared in Example 3 into the syringe of an ink direct writing 3D printing device;
[0169] S2, setting printing process parameters, and printing the heat conducting part;
[0170] Among them, the printing process parameters are: printing extrusion pressure is 2Mpa, the diameter of the printing needle is 0.7mm, and the printing speed is 2mm / s;
[0171] According to the method in the above-mentioned application example 1, a rectangular heat-conducting member with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively and a heat-conducting member with a length, width and height of 10 mm, 15 mm and 12 mm respectively were printed.
[0172] After testing, the thermal conductivity of the prepared rectangular heat-conducting parts with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively and the thermal conductivity of the heat-conducting parts with a length, width and height of 10 mm, 15 mm and 12 mm respectively are as follows: Figure 4 shown.
[0173] Example 4
[0174] This embodiment provides a composite ink material, including the following components in parts by weight:
[0175] 650 parts of silicone rubber resin, 300 parts of thermal conductive filler, 50 parts of curing agent;
[0176] Wherein, the silicone rubber resin is methyl vinyl silicone rubber;
[0177] The thermal conductive filler includes aluminum oxide and boron nitride, wherein the aluminum oxide accounts for 50 parts and the boron nitride accounts for 300 parts.
[0178] This embodiment also provides a method for preparing the composite ink material, comprising the following steps:
[0179] S1, adding the thermal conductive filler into the silicone rubber resin and mixing at a speed of 300 r / min for 3 hours to obtain a silicone rubber mixed liquid;
[0180] S2, adding a curing agent to the silicone rubber mixture, mixing, ultrasonicating, and centrifuging to remove bubbles, and obtaining a composite ink material;
[0181] The ultrasonic time was 5 min, the ultrasonic temperature was controlled at 25°C, the centrifugal speed was 2000 r / min, and the centrifugal time was 10 min.
[0182] Application Example 7
[0183] This application example provides a method for preparing a thermal conductive member by ink direct writing 3D printing, comprising the following steps:
[0184] S1. Loading the composite ink material prepared in Example 4 into the syringe of an ink direct writing 3D printing device;
[0185] S2, setting printing process parameters, and printing the heat conducting part;
[0186] Among them, the printing process parameters are: printing extrusion pressure is 2Mpa, the diameter of the printing needle is 0.5mm, and the printing speed is 2mm / s;
[0187] According to the method in the above-mentioned application example 7, a rectangular heat-conducting member with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively is printed.
[0188] Example 5
[0189] This embodiment provides a composite ink material, including the following components in parts by weight:
[0190] 650 parts of silicone rubber resin, 300 parts of thermal conductive filler, 50 parts of curing agent;
[0191] Wherein, the silicone rubber resin is fluorosilicone rubber;
[0192] The thermally conductive filler is alumina.
[0193] This embodiment also provides a method for preparing the composite ink material, comprising the following steps:
[0194] S1, adding the thermal conductive filler into the silicone rubber resin and mixing at a speed of 300 r / min for 3 hours to obtain a silicone rubber mixed liquid;
[0195] S2, adding a curing agent to the silicone rubber mixture, mixing, ultrasonicating, and centrifuging to remove bubbles, and obtaining a composite ink material;
[0196] The ultrasonic time was 5 min, the ultrasonic temperature was controlled at 25°C, the centrifugal speed was 3000 r / min, and the centrifugal time was 10 min.
[0197] Application Example 8
[0198] This application example provides a method for preparing a thermal conductive member by ink direct writing 3D printing, comprising the following steps:
[0199] S1. Loading the composite ink material prepared in Example 5 into the syringe of an ink direct writing 3D printing device;
[0200] S2, setting printing process parameters, and printing the heat conducting part;
[0201] Among them, the printing process parameters are: printing extrusion pressure is 1Mpa, the diameter of the printing needle is 0.9mm, and the printing speed is 2mm / s;
[0202] According to the method in the above-mentioned application example 8, a rectangular heat-conducting member with a length, width and height of 20 mm, 20 mm and 1.5 mm respectively is printed.
[0203] Comparative Example 1
[0204] This comparative example provides a method for preparing pure silicone rubber, comprising the following steps:
[0205] S1, 650 parts by weight of silicone rubber resin and 50 parts by weight of curing agent are mixed and then cast, and then vacuum degassing is performed to obtain pure silicone rubber;
[0206] Wherein, the silicone rubber resin is polydimethyl silicone rubber.
[0207] Figure 1 The SEM images of the heat-conducting parts (specifically, rectangular heat-conducting parts with length, width and height of 20mm, 20mm and 1.5mm respectively) obtained in Application Example 1 are shown in Figure a, which shows that the boron nitride is shear-oriented along the extrusion direction. Figure b is an SEM image of the printed heat-conducting product after quenching, from which it can be clearly seen that the boron nitride is oriented along one direction. This shows that the shear orientation of the boron nitride is very effective during the extrusion process.
[0208] Specifically, refer to Figure 2As shown, it shows a schematic diagram of preparing a heat-conducting member by 3D printing of the present invention, wherein a composite ink material is loaded into a syringe 1 of an ink direct writing 3D printing device, and a heat-conducting member 2 is obtained by printing; the heat-conducting member 2 is a rectangular parallelepiped, wherein L represents the length of the heat-conducting member, W represents the width of the heat-conducting member, and H represents the height of the heat-conducting member; Figure 2 a represents the direction parallel to the length on the upper surface, which is the in-plane direction; Figure 3 In the middle, a represents the direction parallel to the width on the side, which is the vertical direction.
[0209] Figure 3 The thermal conductivity diagram of the thermal conductive member obtained in application examples 1 to 4 is as follows: the rectangular thermal conductive member sample with a length, width and height of 20 mm, 20 mm and 1.5 mm is the thermal conductivity in the plane, and the rectangular thermal conductive member sample with a length, width and height of 15 mm, 10 mm and 12 mm is the thermal conductivity diagram in the vertical direction; wherein, Figure 2 The printing speed of 1.5 mm / s represents the thermal conductive part prepared in Application Example 4, the printing speed of 2 mm / s represents the thermal conductive part prepared in Application Example 1, the printing speed of 2.5 mm / s represents the thermal conductive part prepared in Application Example 2, and the printing speed of 3 mm / s represents the thermal conductive part prepared in Application Example 3. The sample with a printing speed of 0 mm / s was prepared by casting the composite ink material prepared in Example 1 and then vacuum degassing.
[0210] from Figure 3 It can be seen that when the composite ink material is extruded and printed at different printing speeds, the shear force applied to the composite ink material will change with different extrusion speeds. Figure 3 In the process, the faster the printing speed, the greater the shear force applied to the boron nitride, the higher the degree of orientation of the boron nitride, and the higher its thermal conductivity along the printing direction (in-plane).
[0211] Figure 4 It is the thermal conductivity graph of the heat-conducting parts obtained in Example 2, Example 5, and Example 6 (specifically: rectangular heat-conducting parts with a length, width, and height of 20 mm, 20 mm, and 1.5 mm, and rectangular heat-conducting parts with a length, width, and height of 15 mm, 10 mm, and 12 mm, respectively). Among them, Figure 4250 parts represent the heat conductive member prepared in Application Example 5, 300 parts represent the heat conductive member prepared in Application Example 2, and 350 parts represent the heat conductive member prepared in Application Example 6. The amount of filler added is 0 parts, which is the pure silicone rubber prepared in Comparative Example 1; wherein vertical and in-plane represent: the thermal conductivity of the thermal conductive parts prepared in Application Example 5, Application Example 2, and Application Example 6 and the pure silicone rubber prepared in Comparative Example 1 are tested vertically and in-plane according to the above method respectively; 250 parts of the corresponding non-oriented representation: the composite ink material prepared in Example 2 is formed by tape casting, and the thermal conductivity of the sample is obtained after vacuum degassing; 300 parts of the corresponding non-oriented representation: the composite ink material prepared in Example 1 is formed by tape casting, and the thermal conductivity of the sample is obtained after vacuum degassing; 350 parts of the corresponding non-oriented representation: the composite ink material prepared in Example 3 is formed by tape casting, and the thermal conductivity of the sample is obtained after vacuum degassing; 0 parts of the corresponding non-oriented representation: according to the method in Comparative Example 1, 650 parts by weight of silicone rubber resin (PDMS) and 50 parts by weight of curing agent are mixed and then formed by tape casting, and then vacuum degassing is performed to obtain the sample, and its thermal conductivity is tested.
[0212] from Figure 4 It can be seen that for different mass fractions of thermally conductive fillers, under the same printing speed, as the mass fraction of the thermally conductive filler increases, the thermal conductivity oriented along the printing direction (in-plane) becomes higher.
[0213] Figure 5 This is a thermal weight loss test graph of the heat-conducting parts (specifically, rectangular heat-conducting parts with a length, width, and height of 20 mm, 20 mm, and 1.5 mm, respectively) obtained in Application Examples 2, 5, and 6. Figure 5 250 parts represent the heat conductive part prepared in Application Example 5, 300 parts represent the heat conductive part prepared in Application Example 2, 350 parts represent the heat conductive part prepared in Application Example 6, and the pure silicone rubber represents the pure silicone rubber prepared in Comparative Example 1.
[0214] from Figure 5 It can be seen that with the increase in the amount of thermal conductive filler, the remaining mass of the thermal conductive part at 800°C will also increase, and the thermal stability will also be improved.
[0215] Figure 6 and Figure 7 It is a tensile test diagram of the thermal conductive member samples obtained in Application Examples 1 to 3. Figures 6-7 2 mm / s represents the heat-conducting part prepared in Application Example 1, 2.5 mm / s represents the heat-conducting part prepared in Application Example 2, 3 mm / s represents the heat-conducting part prepared in Application Example 3, and pure silicone rubber represents the pure silicone rubber prepared in Comparative Example 1.
[0216] from Figures 6-7It can be seen that the addition of thermal conductive filler will lead to a decrease in the material's elongation at break and tensile strength. However, with the increase in printing speed, the degree of orientation of the filler in the matrix increases, thereby hindering the expansion of cracks in the matrix. The higher the degree of orientation, the more obvious the hindering effect, and the material's elongation at break and tensile strength will increase.
[0217] Figures 8-9 1 is a rheological test diagram of the composite ink material obtained in Examples 1, 2, and 3. Specifically, Figure 8 is a graph showing the change of viscosity of the composite ink material with shear rate; Fig. 9 This is a graph showing the storage modulus and loss modulus of the composite ink material changing with oscillation strain.
[0218] Figures 8-9 20% BN+5% MgO represents the composite ink material prepared in Example 2, 25% BN+5% MgO represents the composite ink material prepared in Example 1, and 30% BN+5% MgO represents the composite ink material prepared in Example 3. Figure 8 The medium-pure silicone rubber refers to the pure silicone rubber prepared in Comparative Example 1.
[0219] from Figures 8-9 It can be seen that with the increase of thermal conductive filler, the viscosity and modulus of the ink material will increase; when the mass fraction of thermal conductive filler is greater than 300, the storage modulus of the ink material is greater than the loss modulus, and the ink material is in a solidified state. At this time, the ink material has sufficient rheological properties to meet the printing needs.
[0220] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A composite ink material, characterized in that: It comprises the following components by weight: silicone rubber resin ≥ 600 parts, thermal conductive filler ≤ 400 parts, curing agent ≤ 70 parts; The total weight of the silicone rubber resin, the thermal conductive filler and the curing agent is 1000 parts.
2. The composite ink material according to claim 1, characterized in that: The silicone rubber resin includes at least one of methyl silicone rubber, methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, and fluorosilicone rubber.
3. The composite ink material according to claim 1, characterized in that: The thermally conductive filler includes at least one of boron nitride, magnesium oxide, and aluminum oxide.
4. The composite ink material according to any one of claims 1 to 3, characterized in that: The particle size of the thermally conductive filler is 1 to 10 μm; And / or, the composite ink material comprises the following components in parts by weight: 600-680 parts of silicone rubber resin, 250-350 parts of thermal conductive filler, and 50-70 parts of curing agent; The total weight of the silicone rubber resin, the thermal conductive filler and the curing agent is 1000 parts.
5. The method for preparing the composite ink material according to any one of claims 1 to 4, characterized in that: The following steps are involved: Adding thermal conductive filler to silicone rubber resin to obtain silicone rubber mixed liquid; A curing agent is added to the silicone rubber mixed liquid, and after mixing, ultrasonication and centrifugation are performed to remove bubbles, so as to obtain a composite ink material.
6. The method for preparing the composite ink material according to claim 5, characterized in that: The centrifugal speed is 1000-6000 r / min and the centrifugal time is 5-30 min.
7. The method for preparing the composite ink material according to claim 5, characterized in that: The ultrasonic time is 5 to 30 minutes.
8. Use of the composite ink material as claimed in any one of claims 1 to 4 or the composite ink material prepared by the preparation method as claimed in any one of claims 5 to 7 in preparing thermal conductive parts by ink direct writing 3D printing.
9. A method for preparing a thermally conductive component by ink direct writing 3D printing, characterized in that: The following steps are involved: The composite ink material according to any one of claims 1 to 4 or the composite ink material prepared by the preparation method according to any one of claims 5 to 7 is loaded into a syringe of an ink direct writing 3D printing device; Set the printing process parameters and print the thermal conductor.
10. The method for preparing a thermally conductive component by ink direct writing 3D printing according to claim 9, characterized in that: The printing process parameters are: printing extrusion pressure is 0.5-3Mpa, the diameter of the printing needle is 0.7-1.2mm, and the printing speed is 1-3mm / s.
Citation Information
Patent Citations
Preparing and cutting method of novel silicone rubber heat-conducting gasket
CN109354874A
Heat-conducting silica gel sheet and preparation method thereof
CN110358302A
Heat-conducting silicone rubber composite material as well as preparation method and application thereof
CN116285354A
Silicon dioxide composite functional material suitable for 3D printing silicone rubber as well as preparation method and application of silicon dioxide composite functional material
CN118027511A