Method for treating pollutants in process of leaching gold from refractory gold concentrate by biological oxidized carbon
Through filter press and washing of biological oxidation slurry, hydrogen peroxide oxidation treatment, carbon leaching cyanide with low cyanide agent and biological desulfurization cyanide treatment, the problem of pollutant treatment in difficult-to-treat gold ore has been solved, and the source reduction and reduction of pollutants have been achieved. Harmless treatment, recovery of valuable elements, and reduction of treatment costs and waste generation.
Patent Information
- Application Number
- CN202411063256.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Difficulties in treating the pollutants generated by the biooxidation-carbon gold leaching process of difficult-to-treat gold ores include the risk of storage of high-concentration oxidation liquid and cyanide tailings slurry, the inability to recover valuable elements, and high treatment costs.
Through pressure filtration and washing of biological oxidation slurry, hydrogen peroxide oxidation treatment of oxidized slag, low cyanide agent carbon leaching cyanidation, biological desulfurization cyanide treatment carbon leaching tailings washing liquid, and multi-stage neutralization treatment of flotation tailings are used to achieve the removal of pollutants. Source reduction and harmless treatment, and recovery of valuable elements.
It reduces the production of iron, arsenic, sulfide and other impurity ions, reduces cyanide consumption, reduces the production and processing costs of neutralization slag, realizes the collaborative treatment of pollutants and the recovery of valuable elements, and simplifies the process flow. , reducing investment and operating costs.
Smart Images

Figure CN118854071A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a method for treating pollutants in the field of environmental protection, and in particular to a method for treating pollutants in a process for leaching gold from a refractory gold concentrate using bio-oxidation carbon. Background Art
[0002] Refractory gold ore refers to gold ore that cannot be effectively leached by conventional cyanidation after fine grinding. The general definition standard is gold ore with a cyanidation leaching rate of less than 80% after fine grinding. At present, with the large-scale mining of gold resources, high-grade and easy-to-treat gold resources are decreasing, and refractory gold ore has gradually become the main raw material of the gold industry. According to incomplete statistics, about 30% of China's proven gold reserves are refractory gold ore, and this proportion will increase year by year. Because the gold particles in this type of ore are often wrapped by sulfides such as arsenopyrite and pyrite, and contain more impurity elements, such as non-metallic elements arsenic, sulfur, carbon and metallic elements copper, antimony, etc. Using the traditional direct cyanidation gold leaching process, the gold leaching rate is low and the consumption of cyanide is large. Therefore, refractory gold ore needs to be pretreated before leaching. The main pretreatment methods are oxidative roasting, pressure oxidation and bacterial oxidation. Among them, the bio-oxidation pretreatment process has the advantages of simple operation, low production cost and easy control compared with other difficult-to-metallurgical gold extraction technologies, and is increasingly favored by production companies.
[0003] Since difficult-to-treat ores often contain minerals with high sulfur, arsenic and iron content, they are easily oxidized during the biological oxidation process, producing oxidation liquid with high arsenic and iron concentrations and acidity, and high-sulfur, high-arsenic and high-iron oxidation slag. The oxidation slag containing impurity elements will consume a large amount of leaching reagents in the further cyanide leaching process, and at the same time produce secondary pollutants such as thiocyanate, ferrocyanate, arsenic compounds, etc. These pollutants need to be controlled and treated during the production process to reduce the adverse effects on production indicators.
[0004] At present, for the oxidation liquid and cyanide tailings produced in the process of bio-oxidation-carbon leaching of gold from difficult-to-treat gold concentrate, the oxidation liquid is generally used to treat the cyanide tailings slurry to achieve the purpose of treating waste with waste. Chinese patent application CN108117232A discloses a method for harmless treatment of cyanide-containing tailings slurry by bio-oxidation liquid in the gold extraction process of the gold industry. In this method, the bio-oxidation liquid is added to the cyanide-containing tailings slurry in a closed stirred reactor to remove the easily released cyanide and metal cyanide complex. The tailings slurry is stored in the tailings pond after filtration or filter pressing. However, there is a risk of cyanide and arsenic dissolution during the storage process, and the valuable elements such as gold and silver remaining in the tailings slurry cannot be recovered.
[0005] The oxidation liquid treatment generally adopts the alkali neutralization method such as lime and carbide slag, such as Chinese patent application CN106277360A, which discloses a method of neutralizing biological oxidation liquid with alkaline waste residue. This method uses the alkaline waste residue produced by the production of acetylene gas in a chemical plant to neutralize the acidic oxidation liquid produced by the biological oxidation operation of the biological oxidation gold extraction plant, which not only solves the pollution caused by the stacking of alkaline waste residues in the chemical plant to the environment, but also solves the pollution caused by the discharge of acidic oxidation liquid in the biological oxidation gold extraction plant to the surrounding environment, achieving zero pollution discharge and achieving the purpose of treating waste with waste. However, there is a large amount of slag produced by the neutralization slag, which increases the transportation and storage costs. The cyanide tailings slurry is generally treated separately by the Inco method or hydrogen peroxide oxidation method. Since copper sulfate needs to be added as a catalyst, too many copper ions are brought into the system, which has a certain adverse effect on production indicators. In addition, due to the large amount of reagents used, the processing cost is greatly increased.
[0006] Therefore, how to develop a method for treating pollutants in the bio-oxidation-carbon leaching process of difficult-to-treat gold concentrate, achieve harmless treatment of bio-oxidation liquid and cyanide tailings slurry, and realize the recovery or recycling of valuable elements is an environmental problem that urgently needs to be solved in the current bio-oxidation process. Summary of the invention
[0007] In view of the deficiencies in the prior art, the present invention aims to provide a method for treating pollutants in the process of bio-oxidation carbon leaching of gold from difficult-to-treat gold concentrate.
[0008] In order to achieve the above object, the present invention adopts the following technical solution:
[0009] A method for treating pollutants in a process for leaching gold from a refractory gold concentrate using bio-oxidation carbon comprises the following steps:
[0010] S1. After the bio-oxidized slurry produced by bio-oxidation of the refractory gold concentrate is thickened, the thick underflow is filtered and washed; the oxidized slag after washing is transferred to step S2, and the thickened overflow, the filter press filtrate and the washed liquid are combined to obtain the bio-oxidized liquid, a part of which is sent to step S4, and the other part is sent to step S5;
[0011] The reaction processes involved include:
[0012] S x S 2- +CN - →S x-1 S 2- +SCN - Reaction (1)
[0013] f 3+ +3CN - +3H 2 O→Fe(OH) 3 +3HCN Reaction (2)
[0014]
[0015] S2, add water to the oxidized slag to adjust the slurry to a slurry mass concentration of 30-40%, add hydrogen peroxide and stir to react for 1-2 hours, the reaction formula is shown in (4). Then add sodium polycyanamide or sodium carbonate cyanurate as an environmentally friendly gold extraction reagent to carry out carbon leaching for 24-30 hours. After the leaching is completed, the carbon leaching tail slurry is transferred to step S3 for harmless treatment;
[0016]
[0017] S3, the carbon leaching tailings obtained in step S2 are subjected to filter pressing and washing, and the carbon leaching tailings after washing meet the standards and are discharged into the tailings pond for safe storage, the filter press filtrate is returned to step S2 for slag slurry preparation, and the carbon leaching tailings washing liquid is transferred to step S4 for purification treatment;
[0018] S4. Add iron salt to the washing liquid of carbon leaching tailings, and react for 0.2-1h under stirring. The reaction process is shown in reaction formulas (5) and (6). Then, add the biological oxidation liquid in step S1 and continue to react for 0.2-1h. The reaction process is shown in reaction formula (7). Filter, the total cyanide concentration in the filtrate is less than 10mg / L, adjust the pH value to 6.5-8.5, use the microorganisms in the landfill leachate sludge or the coking plant sludge as the thiocyanate degrading bacteria, and add nutrients to adjust the carbon-nitrogen-phosphorus ratio. Under aeration conditions, the thiocyanate in the filtrate is subjected to biological desulfurization and cyanolysis. The reaction process is shown in reaction formula (8), so that the concentration of thiocyanate in the filtrate is reduced to below 50mg / L; the filtrate after biological desulfurization and cyanolysis is returned to step S3 and recycled for washing water of carbon leaching tailings;
[0019]
[0020]
[0021] S5. The bio-oxidation liquid is subjected to multi-stage neutralization treatment using flotation tailings, the neutralized slurry is thickened, the obtained dense underflow is filtered, and the filter residue is sent to the tailings pond for safe storage. The filter press liquid and the dense overflow obtained by thickening the neutralized slurry are combined and sent to step S1 for washing.
[0022] Furthermore, in step S1, the amount of water used for washing is 0.2-1 times the dry weight of the oxidized slag; in step S5, the level of neutralization of the oxidizing liquid is 3-6 levels.
[0023] Furthermore, in step S2, the mass concentration of hydrogen peroxide is 30%, the amount added is 0.1-0.5% of the volume of the slurry, and the amount of environmentally friendly gold extraction reagent added is 1-2 times the amount of sodium cyanide used in theoretical cyanide gold extraction.
[0024] Furthermore, in step S3, the amount of water used for washing the carbon-leached tailings is 0.4-3 times the dry weight of the carbon-leached tailings.
[0025] Furthermore, in step S4, the iron salt is ferrous sulfate heptahydrate, and the mass ratio of the added amount to the environmentally friendly gold extraction reagent in the carbon leaching tailings washing liquid is 5-10, and the iron content in the added biological oxidation liquid is 1-3 times the mass of the environmentally friendly gold extraction reagent in the carbon leaching tailings washing liquid; the biological desulfurization cyanide reaction conditions are water temperature 20-30°C, pH value 6.5-8.5, sludge concentration 3-10g / L, carbon nitrogen phosphorus mass ratio of 100:5:1, dissolved oxygen content 2-6mg / L, and aeration treatment for 24-72h.
[0026] Furthermore, the nutrients include one or more of glucose, ammonium salts, and phosphates.
[0027] Furthermore, in step S5, the flotation tailings are tailings produced by flotation of refractory gold ore before bio-oxidation.
[0028] The beneficial effects of the present invention are:
[0029] (1) The present invention uses bio-oxidation slurry filter pressing and washing to reduce the impurity ions such as iron, arsenic, polysulfide, etc. entering the carbon-leaching cyanidation process from the source, and reduces the generation of pollutants such as ferrocyanide, arsenic, and thiocyanate from the source; the bio-oxidation slag is oxidized with hydrogen peroxide before carbon-leaching cyanidation to oxidize low-valent sulfur to sulfate ions, thereby reducing the generation of thiocyanate from the source and reducing the amount of gold leaching agent used.
[0030] (2) The present invention adopts low-cyanide reagent for carbon leaching cyanidation to reduce the cyanide content in the carbon leaching tailings; the carbon leaching tailings are filtered and washed, and the filtrate is returned to the oxide slurry for slurry adjustment and re-enters the cyanidation leaching, thereby making full use of the gold leaching reagent remaining in the filtrate and recovering valuable elements such as gold and silver in the filtrate.
[0031] (3) The present invention uses biological oxidation liquid to treat carbon leaching tailings washing liquid, thereby reducing the cost of cyanide destruction treatment of the carbon leaching tailings washing liquid; the biological oxidation liquid also uses flotation tailings from difficult-to-treat gold ore for neutralization treatment, thereby reducing the amount of neutralization slag produced and the cost of neutralization treatment, thereby achieving waste treatment with waste.
[0032] (4) The present invention starts from the three aspects of source reduction, process control and terminal treatment, and realizes the reduction and harmless treatment of pollutants generated in the process of biological oxidation and cyanide carbon leaching of difficult-to-treat gold mines. Through the idea of "treating waste with waste", the synergy between pollutant treatment processes is achieved, the treatment cost and the amount of waste residue generated are reduced, and various valuable elements such as gold and silver are recovered at the same time. The treatment process of the present invention is simple, the investment and operation costs are low, and it has strong application value and prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is a flow chart of the method of Embodiment 1-2 of the present invention. DETAILED DESCRIPTION
[0034] The present invention will be further described below in conjunction with the accompanying drawings. It should be noted that this embodiment is based on the technical solution and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to this embodiment.
[0035] Example 1
[0036] This embodiment provides a method for treating pollutants in a process for leaching gold from a refractory gold concentrate using bio-oxidation carbon. Figure 1 As shown, the following steps are included:
[0037] S1. After the bio-oxidation slurry produced by the bio-oxidation of the difficult-to-treat gold concentrate is thickened, the thick underflow is filtered, and the oxidized slag obtained by the filtering is washed with water of 1 times the dry weight of the oxidized slag; the washed oxidized slag is transferred to step S2, and the thick overflow, the filter press filtrate and the washed liquid are combined to obtain the bio-oxidation liquid, a part of which is sent to step S4, and the other part is sent to step S5.
[0038] S2, add water to the oxidized slag to adjust the slurry to a slurry mass concentration of 30%, add 30% hydrogen peroxide at 0.5% of the slurry volume, stir and react for 1 hour, add carbonized sodium cyanurate as an environmentally friendly gold extraction reagent for carbon leaching for 24 hours, and after leaching, the carbon leaching tail slurry is transferred to step S3 for harmless treatment. The mass of the environmentally friendly gold extraction reagent added is 1.5 times the theoretical amount required for cyanide gold extraction using sodium cyanide.
[0039] S3, the carbon leaching tailings obtained in step S2 are filtered, and the carbon leaching tailings obtained by filtering are washed with water 0.4 times the dry weight of the carbon leaching tailings. After washing, the carbon leaching tailings meet the requirements for tailings pond disposal in the "Technical Specifications for Control of Cyanide Slag Pollution in the Gold Industry" (HJ943-2018), and are discharged into the tailings pond for safe storage. The filtrate obtained by filtering the carbon leaching tailings is returned to step S2 for slag slurry preparation, and the washing liquid of the carbon leaching tailings is transferred to step S4 for purification. The pollutant composition of the filtrate of the carbon leaching tailings is shown in Table 1.
[0040] S4, according to the addition amount of ferrous sulfate heptahydrate being 5 times the mass of the environmentally friendly gold extraction reagent in the carbon leaching tailings washing liquid, ferrous sulfate heptahydrate was added to the carbon leaching tailings washing liquid at 2g / L, and stirred for reaction for 0.5h, then, according to the iron content in the biological oxidation liquid being 1 times the mass of the gold extraction reagent in the carbon leaching tailings washing liquid, the biological oxidation liquid in step S1 was added to the carbon leaching tailings washing liquid, and the reaction was continued for 0.5h, filtered, and the total cyanide in the filtrate was 3.2mg / L, and the thiocyanate concentration was 965mg / L. After adjusting the pH value of the filtrate to 8.5, the microorganisms in the coking plant sludge are used as the thiocyanate degrading bacteria, and potassium dihydrogen phosphate is added to adjust the carbon, nitrogen and phosphorus ratio in the filtrate. The thiocyanate in the filtrate is subjected to biological desulfurization under aeration conditions. The conditions are water temperature of 30°C, pH value of 8.5, coking plant sludge concentration of 3g / L, dissolved oxygen content of 4.5mg / L, potassium dihydrogen phosphate addition of 0.1mg / L, carbon, nitrogen and phosphorus ratio in the filtrate of 100:5:1, aeration treatment time of 24h, and the thiocyanate concentration is reduced to 3.6mg / L. The filtrate after biological desulfurization is returned to step S3 for recycling of washing water for carbon leaching tailings;
[0041] S5. The bio-oxidation liquid is subjected to a three-stage neutralization treatment using the flotation tailings obtained by flotation of the difficult-to-treat gold ore before bio-oxidation. The neutralized slurry is thickened, and the obtained thick underflow is filtered. The filter press residue is sent to the tailings pond for safe storage. The filter press liquid and the thick overflow obtained by thickening the neutralized slurry are combined and sent to step S1 for washing the oxidation residue.
[0042] Table 1 Pollutant composition of the filtrate of carbon leaching tail slurry filter press mg / L
[0043] Cyanide Thiocyanate As Fe 376 1348 305 212
[0044] Example 2
[0045] This embodiment provides a method for treating pollutants in a process for leaching gold from a refractory gold concentrate using bio-oxidation carbon. Figure 1 As shown, the following steps are included:
[0046] S1. After the bio-oxidation slurry produced by the bio-oxidation of the difficult-to-treat gold concentrate is thickened, the thick underflow is filtered, and the oxidized slag obtained by the filtration is washed with water 0.4 times the dry weight of the oxidized slag; the washed oxidized slag is transferred to step S2, and the thick overflow, the filtrate from the filtration and the washed liquid are combined to obtain the bio-oxidation liquid, a part of which is sent to step S4, and the other part is sent to step S5.
[0047] S2, add water to the oxidized slag to adjust the slurry to a slurry mass concentration of 30%, add 30% hydrogen peroxide at 0.1% of the slurry volume, stir and react for 1 hour, add sodium polycyanamide as an environmentally friendly gold extraction reagent to carry out carbon leaching for 24 hours, and after the leaching is completed, the carbon leaching tail slurry is transferred to step S3 for harmless treatment. The amount of environmentally friendly gold extraction reagent added is 1.5 times the theoretical amount required for cyanide gold extraction using sodium cyanide.
[0048] S3. The carbon-leached tailings obtained in step S2 are filtered, and the carbon-leached tailings obtained by filtering are washed with water 2.5 times the dry weight of the carbon-leached tailings. After washing, the carbon-leached tailings meet the tailings pond disposal requirements in the "Technical Specifications for Cyanide Slag Pollution Control in the Gold Industry" (HJ943-2018), and are discharged into the tailings pond for safe storage. The filtrate obtained by filtering the carbon-leached tailings is returned to step S2 for slag slurrying, and the carbon-leached tailings washing liquid is transferred to step S4 for purification.
[0049] S4, according to the iron salt added amount of 10 times the mass of the gold extraction reagent in the carbon leaching tailings washing liquid, 4g / L of ferrous sulfate heptahydrate was added to the carbon leaching tailings washing liquid, and the reaction was stirred for 0.2h. Then, according to the iron content in the biological oxidation liquid of 3 times the mass of the gold extraction reagent in the carbon leaching tailings washing liquid, the biological oxidation liquid in step S1 was added to the carbon leaching tailings washing liquid and the reaction was continued for 0.2h. After filtering, the total cyanide in the filtrate was 4.5mg / L, and the thiocyanate concentration was 1274mg / L. After adjusting the pH value of the filtrate to 7, the microorganisms in the landfill leachate sludge are used as the thiocyanate degrading bacteria, and potassium dihydrogen phosphate is added to adjust the carbon-nitrogen-phosphorus ratio in the filtrate. The thiocyanate in the filtrate is subjected to biological desulfurization under aeration conditions. The conditions are water temperature 25°C, pH value 7, sludge concentration 6g / L, dissolved oxygen content 3mg / L, potassium dihydrogen phosphate addition amount 0.1mg / L, carbon-nitrogen-phosphorus ratio in the filtrate is 100:5:1, aeration treatment time is 72h, and the thiocyanate concentration is reduced to 7.5mg / L. The filtrate after biological desulfurization is returned to step S3 and recycled for washing water of carbon leaching tailings;
[0050] S5. The bio-oxidation liquid is subjected to a 6-stage neutralization treatment using the flotation tailings obtained by flotation of the difficult-to-treat gold ore before bio-oxidation. The neutralized slurry is thickened, and the obtained dense underflow is filtered. The filter press residue is sent to the tailings pond for safe storage. The filter press liquid and the dense overflow obtained by thickening the neutralized slurry are combined and sent to step S1 for washing.
[0051] Comparative experiment
[0052] The refractory gold concentrate obtained after flotation of a refractory gold ore of a gold mining enterprise was pretreated by a bio-oxidation pretreatment process. After the generated bio-oxidation slurry was concentrated, the concentrated underflow was filtered, and a part of the slag was washed with water 0.4 times the dry weight of the slag, while the other part of the slag was not washed. The composition of the washed slag and the unwashed slag is shown in Table 2.
[0053] Table 2 Oxidation slag pollutant composition g / kg
[0054] Components As Fe S Unwashed 146.3 584.6 550.8 After washing 7.4 123.5 131.2
[0055] The unwashed oxide slag was slurried with water to make the slurry mass concentration 30%, and divided into two groups, one of which was added with 30% hydrogen peroxide at 0.1% of the slurry volume and stirred for 1 hour, and the other group was not added with hydrogen peroxide. Then the two groups of slurries were cyanided and carbon-leached with sodium polycyanamide under the same conditions. The pollutant composition of the filter press filtrate of the carbon-leached tailings is shown in Table 3, and the gold content of the carbon-leached tailings obtained after the carbon-leached tailings were filtered and washed is shown in Table 4.
[0056] Table 3 Pollutant composition of filter press filtrate of carbon leaching tail slurry mg / L
[0057] Components Thiocyanate As Fe Not oxidized with hydrogen peroxide 3810 380 820 Hydrogen peroxide oxidation 2635 366 785
[0058] Table 4 Gold content in carbon leaching tailings
[0059] Components Au(g / t) Cost of ton of ore hydrogen peroxide (yuan) Hydrogen peroxide oxidation 3.16 2 Not oxidized with hydrogen peroxide 3.35 0
[0060] In addition, the ore pulp without hydrogen peroxide oxidation was divided into two groups, one group was added with sodium polycyanamide for carbon leaching for 24 hours, and the other group was added with sodium cyanide for carbon leaching. The amount of environmentally friendly gold extraction reagent added was 1.5 times the amount of sodium cyanide. The relevant indicators of carbon leaching tailings and filter press filtrate obtained after filter press washing of carbon leaching tailings are shown in Tables 5 and 6.
[0061] Table 5 Gold content in carbon leaching tailings and leaching cost per ton of ore
[0062] Components Au(g / t) Cost of leaching reagent per ton of ore (yuan) Sodium cyanide leaching 3.16 391 Environmentally friendly gold extraction reagent 3.54 399
[0063] Table 6 Pollutant composition of filter press filtrate of carbon leaching tail slurry mg / L
[0064] Components Total Cyanide Thiocyanate As Fe Sodium cyanide leaching 1092 3810 380 820 Environmentally friendly gold extraction reagent 305 2365 340 230
[0065] As shown in Table 2, after the biological oxidation slurry is filtered and washed, the contents of arsenic, iron and sulfur in the oxidation slag are significantly reduced. As shown in Tables 3 and 4, after oxidation with hydrogen peroxide, the content of thiocyanate in the filter press filtrate of the carbon-leached tailings produced by cyanidation of the oxidation slag is significantly reduced, and the content of gold in the carbon-leached tailings is also reduced. This shows that the biological oxidation slurry is filtered and washed and oxidized with hydrogen peroxide to remove impurities, which can not only reduce the content of pollutants entering the cyanidation link, but also reduce the ineffective consumption caused by the reaction of these impurities with the gold extraction reagent; As shown in Tables 5 and 6, at the same leaching agent cost, the leaching effect of sodium cyanide and environmentally friendly gold extraction reagent is equivalent. The gold content in the carbon-leached tailings of the environmentally friendly gold extraction reagent is slightly higher, but the contents of cyanide, thiocyanate, arsenic and iron in the carbon-leached tailings produced are reduced to varying degrees, reducing the pressure of subsequent tailings purification treatment.
[0066] For those skilled in the art, various corresponding changes and modifications can be made according to the above technical solutions and concepts, and all of these changes and modifications should be included in the protection scope of the claims of the present invention.
Claims
1. Treatment method of pollutants in the process of gold extraction from bio-oxidation carbon of difficult-to-treat gold concentrate, It is characterized in that The following steps are involved: S1. After the bio-oxidized slurry produced by bio-oxidation of the refractory gold concentrate is thickened, the thick underflow is filtered and washed; The washed oxidized slag is transferred to step S2, and the dense overflow, the filter press filtrate and the washed liquid are combined to obtain a biological oxidation liquid, a part of which is sent to step S4, and the other part is sent to step S5; S2, add water to the oxidized slag to adjust the slurry to a slurry mass concentration of 30-40%, add hydrogen peroxide and stir to react for 1-2 hours, then add sodium polycyanamide or sodium carbonate cyanurate as an environmentally friendly gold extraction reagent to carry out carbon leaching for 24-30 hours. After the leaching is completed, the carbon leaching tail slurry is transferred to step S3 for harmless treatment; S3, the carbon leaching tailings obtained in step S2 are subjected to filter pressing and washing, and the carbon leaching tailings after washing meet the standards and are discharged into the tailings pond for safe storage, the filter press filtrate is returned to step S2 for slag slurry preparation, and the carbon leaching tailings washing liquid is transferred to step S4 for purification treatment; S4, adding iron salt to the carbon leaching tailings washing liquid, reacting for 0.2-1h under stirring, then adding the biological oxidation liquid in step S1 to continue reacting for 0.2-1h, filtering, the total cyanide concentration in the filtrate is less than 10mg / L, adjusting the pH value to 6.5-8.5, using microorganisms in landfill leachate sludge or coking plant sludge as thiocyanate degrading bacteria, adding nutrients to adjust the carbon-nitrogen-phosphorus ratio, and biologically removing thiocyanate from the filtrate under aeration conditions to reduce the concentration of thiocyanate in the filtrate to less than 50mg / L; the filtrate after biologically removing thiocyanate is returned to step S3 for recycling water for washing carbon leaching tailings; S5. The bio-oxidation liquid is subjected to multi-stage neutralization treatment using flotation tailings, the neutralized slurry is thickened, the obtained dense underflow is filtered, and the filter residue is sent to the tailings pond for safe storage. The filter press liquid and the dense overflow obtained by thickening the neutralized slurry are combined and sent to step S1 for washing.
2. The processing method according to claim 1, It is characterized in that In step S1, the amount of water used for washing is 0.2-1 times the dry weight of the oxidation slag; in step S5, the level of neutralization of the oxidation liquid is 3-6 levels.
3. The processing method according to claim 1, It is characterized in that In step S2, the mass concentration of hydrogen peroxide is 30%, the amount added is 0.1-0.5% of the volume of the slurry, and the amount of environmentally friendly gold extraction reagent added is 1-2 times the mass of sodium cyanide used for theoretical cyanide gold extraction.
4. The processing method according to claim 1, It is characterized in that In step S3, the amount of water used for washing the carbon leaching tailings is 0.4-3 times the dry weight of the carbon leaching tailings.
5. The processing method according to claim 1, It is characterized in that In step S4, the iron salt is ferrous sulfate heptahydrate, and the added amount is 5-10 to the mass ratio of the environmentally friendly gold extraction reagent in the carbon leaching tailings washing liquid, and the iron content in the added biological oxidation liquid is 1-3 times the mass of the environmentally friendly gold extraction reagent in the carbon leaching tailings washing liquid; the biological desulfurization cyanide reaction conditions are water temperature 20-30°C, pH value 6.5-8.5, sludge concentration 3-10g / L, carbon nitrogen phosphorus mass ratio of 100:5:1, dissolved oxygen content 2-6mg / L, and aeration treatment for 24-72h.
6. The processing method according to claim 5, It is characterized in that The nutrients include one or more of glucose, ammonium salts, and phosphates.
7. The processing method according to claim 1, It is characterized in that In step S5, the flotation tailings are tailings produced by flotation of refractory gold ore before bio-oxidation.
Citation Information
Patent Citations
Refractory gold concentrate biological oxidizing slag cyaniding and gold-extracting method
CN102002587A
Secondary oxidation pretreatment process for arsenic, sulphur and carbon-containing difficultly treated gold concentrate
CN102011013A
Comprehensive recycling method for high-grade multi-element gold concentrate
CN115261635A
Gold ore dump leaching residue in-situ treatment method
CN115725851A
Method for processing refractory pyrrhotite-arsenopyrite-pyrite-berthierite-stibnite gold ores (options)
RU2807003C1
Cited By
Method for smelting and extracting gold from low-gold pyrite
CN121592871A