Method for extracting lithium by roasting spodumene flotation concentrate

Through direct powder ore roasting and high-temperature oxidation and acidification treatment, the problems of sintering and high energy consumption in traditional spodumene flotation concentrate roasting are solved, and efficient lithium metal extraction and energy consumption reduction are achieved.

CN118854079APending Publication Date: 2024-10-29SHANGHAI MILESTONE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410877791.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

During the roasting process of traditional spodumene flotation concentrate, excessive dust causes sintering problems, and the pelletizing process increases costs and operational risks, making it difficult to meet the market demand for lithium.

Method used

The powdered ore is roasted directly after filtering, and the moisture is evaporated through the roasting preheating system and heated to 200℃~350℃, and then in the heating system to 1100℃~1200℃ for gas-solid separation, and then transformed into β-type spodumene after oxidation The stone is reacted with industrial concentrated sulfuric acid in an acidizing kiln, eliminating the need for pelletizing and grinding processes, and improving heat recovery and energy consumption efficiency.

Benefits of technology

It achieves direct roasting without pelletizing, improves the lithium metal leaching rate and system heat recovery rate, reduces energy consumption and process flow, shortens process time, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854079A_ABST
    Figure CN118854079A_ABST
Patent Text Reader

Abstract

The invention discloses a method for extracting lithium from spodumene flotation concentrate through roasting transformation. The method comprises the following steps: S1, filter pressing: selecting ore and carrying out filter pressing to obtain a filter cake containing 8-14% of water; s2, preheating: feeding the filter cake into a roasting preheating system through forced feeding equipment, preheating, and discharging mineral powder at the temperature of 120-150 DEG C; s3, heating and separating: feeding the mineral powder discharged by roasting and preheating into a heating system, heating to 1100-1200 DEG C, separating by a gas-solid separation system, and feeding into a transformation reaction chamber; s4, oxidizing and acidifying: oxidizing in a reaction chamber for 30-60 minutes, cooling by a cooling system, directly feeding into an acid mixer, feeding into an acidifying kiln after acid mixing, and controlling the acidifying temperature of the acidifying kiln to be 250-300 DEG C; and S5, neutralizing and precipitating lithium: carrying out size mixing and water leaching, and adding sodium carbonate for replacement to produce lithium carbonate precipitate. The method is free of pelletizing, high in heat efficiency and low in energy consumption.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mineral processing, and in particular to a method for extracting lithium by roasting spodumene flotation concentrate. Background Art

[0002] Lithium is an active metal that can react with a variety of substances to form relatively stable compounds. It is widely used in the industrial and medical sectors. In recent years, with the development of new energy vehicles and electronic products, the demand for batteries has been increasing. Lithium carbonate is the main electrode material for preparing lithium batteries, and lithium hydroxide is an important raw material for preparing ternary batteries. Lithium carbonate is soluble in acid and slightly soluble in water. It is the most important lithium compound. The main raw materials for preparing lithium carbonate and lithium hydroxide are lithium ore and lithium extraction from salt lakes. As the market demand for lithium increases, the scale of lithium extraction from ore is also increasing.

[0003] Due to resource limitations, the market growth of lithium metal is mostly supplemented by lithium ore extraction. With the continuous expansion of lithium mining, the output of traditional processed gravity concentrate is difficult to meet market demand, and the new output is mostly supplied by spodumene flotation concentrate. In the process of preparing lithium carbonate or lithium hydroxide, spodumene concentrate first needs to transform α-type spodumene into β-type spodumene. The transformed spodumene concentrate is then subjected to sulfuric acid roasting and ion exchange to extract lithium. The spodumene transformation process requires high-temperature roasting.

[0004] The roasting of spodumene gravity concentrate is processed by rotary kiln. Because the particle size of spodumene gravity concentrate is coarse, the forward and obtained indicators are relatively stable.

[0005] When conducting spodumene flotation concentrate, because the ore particle size is relatively fine, the disadvantage of directly using a rotary kiln for roasting is: due to excessive dust, serious sintering problems will be caused, and there will be obstacles to the smooth operation of the rotary kiln processing equipment; and the disadvantages of using mineral powder to make balls and then roasting are: 1. Extra costs are incurred for ball making, and 2. After ball making, sintering problems will occur when running in a rotary kiln due to ball breakage. Summary of the invention

[0006] The purpose of the present invention is to provide a method for extracting lithium by roasting and transforming spodumene flotation concentrate, which eliminates the ball-making process, reduces sintering caused by excessive dust, and has low energy consumption, in view of the shortcomings of the prior art.

[0007] To achieve the above object, the technical solution adopted by the present invention is: a method for extracting lithium by roasting and transforming spodumene flotation concentrate, comprising the following steps:

[0008] S1. Filtration: Select spodumene flotation concentrate with a mass content of 50% to 90% of ore particle size -0.074 mm, a maximum ore particle size of 1 mm or more and a content of less than 2%, and a Li2O taste of 4% to 6.5%, and filter the spodumene flotation concentrate into a filter cake containing 8 to 14% water;

[0009] S2, preheating: the filter cake is fed into the roasting preheating system through the forced feeding equipment. The roasting preheating system evaporates the moisture of the filter cake to form mineral powder and heats the mineral powder to 200℃~350℃. The mineral powder in the roasting preheating system is directly fed into the heating system after preheating treatment. The temperature of the exhaust gas discharged by preheating is 100℃~150℃;

[0010] S3, heating and separation: the calcined preheated ore powder is fed into the heating system and heated to 1100°C to 1200°C. The heated ore powder is separated by the gas-solid separation system, and the ore powder after gas-solid separation is fed into the transformation reaction chamber;

[0011] S4, oxidation acidification: air is introduced into the bottom of the reaction chamber, and the mineral powder is oxidized in a fluidized state under the action of air. The oxidation time is controlled at 30-60min, and the spodumene in the mineral powder is transformed into β-type spodumene. The transformed mineral powder is cooled by a cooling system and directly fed into an acid mixer. At the same time, industrial concentrated sulfuric acid with a content of 90% to 98% is added to the acid mixer. The amount of industrial concentrated sulfuric acid used is 80% to 120% of the mass of the mineral powder after the transformation. The material stirred with the industrial concentrated sulfuric acid is fed into an acidification kiln, and the acidification temperature of the acidification kiln is controlled at 250°C to 300°C; the acidification reaction equation is: β-Li2O·Al2O3·4SiO2+H2SO4=Li2SO4+H2O·Al2O3·4SiO2;

[0012] S5. Neutralization and lithium precipitation: The material after acidification in the acidification kiln is slurried and soaked in water. After the material is soaked in water, it is filtered to separate the filtrate and the filter residue. The filtrate is sent to the sedimentation tank, alkali is added to the filtrate for neutralization and sodium carbonate is added for replacement reaction to produce lithium carbonate precipitate.

[0013] Preferably, the hot air from the gas-solid separation system is fed into a roasting preheating system to form hot air to preheat the filter cake.

[0014] Preferably, the waste gas in the roasting preheating system is discharged after passing through a dust collector, an exhaust fan and a chimney, and the dust collector feeds the collected ash into the transformation reaction chamber.

[0015] Preferably, the heating system provides heat through combustion in a fuel burner, and the fuel of the fuel burner is natural gas or pulverized coal.

[0016] Compared with the prior art, the present invention has the following advantages:

[0017] 1. The spodumene roasting flotation concentrate in the present invention does not need to be pelletized, and the powder ore can be directly fed in, eliminating the pelletizing process;

[0018] 2. The present invention not only fully recovers the heat in the flue gas, but also fully recovers the heat carried by the transformed spodumene ore, thereby improving the heat recovery rate of the whole system;

[0019] 3. The direct acidification of the spodumene concentrate after cooling in the present invention can meet the acidification temperature, eliminating the heating step in the traditional acidification process and reducing the energy consumption of the whole system;

[0020] 4. The present invention directly roasts the spodumene flotation concentrate, and the roasted ore powder does not need grinding. Compared with the traditional process of first roasting, cooling, then grinding, and heating and acidification, it not only has high energy utilization, but also saves the dry grinding process, shortens the process flow, and reduces costs;

[0021] 5. The present invention performs roasting transformation on the mineral powder. Due to the large contact area, the crystal conversion rate is higher than that of the traditional rotary kiln process, and the lithium metal leaching rate is higher. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a schematic diagram of the process of the present invention.

[0023] Figure 2 It is a structural schematic diagram of the present invention.

[0024] Among them, 11-forced feeding equipment, 12-roasting preheating system, 13-heating system, 14-gas-solid separation system, 15-transformation reaction chamber, 16-cooling system, 17-acid mixer, 18-acidification kiln, 19-sedimentation tank, 21-burner, 22-dust collector, 23-exhaust fan, 24-chimney. DETAILED DESCRIPTION

[0025] The present invention is further explained below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent forms of modifications to the present invention by those skilled in the art all fall within the scope defined by the claims attached to this application.

[0026] Example 1: Figure 1 The method for extracting lithium by roasting and transforming spodumene flotation concentrate shown in the figure comprises the following steps:

[0027] S1. Filtration: Select spodumene flotation concentrate with a mass content of 78.54% of ore particle size -0.074 mm, a content of less than 2% of the maximum ore particle size of 1 mm or more, and a Li2O content of 5.05%, and filter the spodumene flotation concentrate to obtain a filter cake with a water content of 9.56%;

[0028] S2, preheating: the filter cake is fed into the roasting preheating system 12 through the forced feeding device 11, the roasting preheating system 12 evaporates the moisture of the filter cake to form mineral powder and heats the mineral powder to 220°C, the mineral powder in the roasting preheating system 12 is directly fed into the heating system 13 after preheating treatment, the temperature of the exhaust gas discharged by preheating is 100°C to 150°C, the exhaust gas in the roasting preheating system 12 is discharged after passing through the dust collector 22, the exhaust fan 23 and the chimney 24, and the dust collector 22 feeds the collected mineral ash into the transformation reaction chamber 15;

[0029] S3, heating and separation: the calcined preheated ore powder is fed into the heating system 13 and heated to 1150°C, the heated ore powder is separated by the gas-solid separation system 14, the ore powder after gas-solid separation is fed into the transformation reaction chamber 15, the hot gas of the gas-solid separation system 14 is fed into the calcination preheating system 12 to form hot air to preheat the filter cake, the heating system 13 provides heat through combustion of the fuel burner, and the fuel of the fuel burner is natural gas or coal powder;

[0030] S4, oxidation acidification: air is introduced into the bottom of the reaction chamber, and the mineral powder is oxidized in a fluidized state under the action of air. The oxidation time is controlled at 30 minutes, and the spodumene in the mineral powder is transformed into β-type spodumene. The transformed mineral powder is cooled by the cooling system 16 and directly fed into the acid mixer 17. At the same time, industrial concentrated sulfuric acid with a content of 90% to 98% is added to the acid mixer 17. The amount of industrial concentrated sulfuric acid used is 95% of the mass of the mineral powder after the transformation. The material stirred with the industrial concentrated sulfuric acid is fed into the acidification kiln 18, and the acidification temperature of the acidification kiln 18 is controlled at 285°C;

[0031] S5, neutralization and lithium precipitation: the material after acidification in the acidification kiln 18 is slurried and soaked in water. After the material is soaked in water, it is filtered to separate the filtrate and the filter residue. The filtrate is led to the sedimentation tank 19, alkali is added to the filtrate for neutralization and sodium carbonate is added for replacement reaction to produce lithium carbonate precipitate. The Li2O grade of the filter residue after acidification, neutralization and filtration is 0.26%, and the leaching rate is 95.21%.

[0032] Example 2: Figure 1 The method for extracting lithium by roasting and transforming spodumene flotation concentrate shown in the figure comprises the following steps:

[0033] S1. Filtration: Select spodumene flotation concentrate with a mass content of 68.24% of ore particle size -0.074 mm, a content of less than 2% of ore with a maximum particle size of 1 mm or more, and a Li2O taste of 4.12%, and filter the spodumene flotation concentrate to obtain a filter cake with a water content of 7.88%;

[0034] S2, preheating: the filter cake is fed into the roasting preheating system 12 through the forced feeding device 11, the roasting preheating system 12 evaporates the moisture of the filter cake to form mineral powder and heats the mineral powder to 240°C, the mineral powder in the roasting preheating system 12 is directly fed into the heating system 13 after preheating treatment, the exhaust gas temperature in the roasting preheating system 12 is 100°C to 150°C, the exhaust gas in the roasting preheating system 12 is discharged after passing through the dust collector 22, the exhaust fan 23 and the chimney 24, and the dust collector 22 feeds the collected mineral ash into the transformation reaction chamber 15;

[0035] S3, heating and separation: the ore powder discharged from the roasting preheating is fed into the heating system 13 and heated to 1200°C, the heated ore powder is separated by the gas-solid separation system 14, the ore powder after gas-solid separation is fed into the transformation reaction chamber 15, the hot gas of the gas-solid separation system 14 is fed into the roasting preheating system 12 to form hot air to preheat the filter cake, the heating system 13 provides heat through combustion of the fuel burner, and the fuel of the fuel burner is natural gas or coal powder;

[0036] S4, oxidation acidification: air is introduced into the bottom of the reaction chamber, and the mineral powder is oxidized in a fluidized state under the action of air. The oxidation time is controlled at 45 minutes, and the spodumene in the mineral powder is transformed into β-type spodumene. The transformed mineral powder is cooled by the cooling system 16 and directly fed into the acid mixer 17. At the same time, industrial concentrated sulfuric acid with a content of 90% to 98% is added to the acid mixer 17. The amount of industrial concentrated sulfuric acid used is 85% of the mass of the mineral powder after the transformation. The material stirred with the industrial concentrated sulfuric acid is fed into the acidification kiln 18, and the acidification temperature of the acidification kiln 18 is controlled at 255°C;

[0037] S5, neutralization and lithium precipitation: the material after acidification in the acidification kiln 18 is slurried and soaked in water. After the material is soaked in water, it is filtered to separate the filtrate and the filter residue. The filtrate is led to the sedimentation tank 19, alkali is added to the filtrate for neutralization and sodium carbonate is added for replacement reaction to produce lithium carbonate precipitate. The Li2O grade of the filter residue after acidification, neutralization and filtration is 0.18%, and the leaching rate is 95.85%.

[0038] Example 3: Figure 1 The method for extracting lithium by roasting and transforming spodumene flotation concentrate shown in the figure comprises the following steps:

[0039] S1. Filtration: Select spodumene flotation concentrate with a mass content of 83.25% of ore particle size -0.074 mm, a content of less than 2% of ore with a maximum particle size of 1 mm or more, and a Li2O taste of 6.12%, and filter the spodumene flotation concentrate to obtain a filter cake with a water content of 10.54%;

[0040] S2, preheating: the filter cake is fed into the roasting preheating system 12 through the forced feeding device 11, the roasting preheating system 12 evaporates the moisture of the filter cake to form mineral powder and heats the mineral powder to 270°C, the mineral powder in the roasting preheating system 12 is directly fed into the heating system 13 after preheating treatment, the temperature of the exhaust gas discharged by preheating is 100°C to 150°C, the exhaust gas in the roasting preheating system 12 is discharged after passing through the dust collector 22, the exhaust fan 23 and the chimney 24, and the dust collector 22 feeds the collected mineral ash into the transformation reaction chamber 15;

[0041] S3, heating and separation: the ore powder discharged from the roasting preheating is fed into the heating system 13 and heated to 1150°C, the heated ore powder is separated by the gas-solid separation system 14, the ore powder after gas-solid separation is fed into the transformation reaction chamber 15, the hot gas of the gas-solid separation system 14 is fed into the roasting preheating system 12 to form hot air to preheat the filter cake, the heating system 13 provides heat through combustion of the fuel burner, and the fuel of the fuel burner is natural gas or coal powder;

[0042] S4, oxidation acidification: air is introduced into the bottom of the reaction chamber, and the mineral powder is oxidized in a fluidized state under the action of air. The oxidation time is controlled at 35 minutes, and the spodumene in the mineral powder is transformed into β-type spodumene. The transformed mineral powder is cooled by the cooling system 16 and directly fed into the acid mixer 17. At the same time, industrial concentrated sulfuric acid with a content of 90% to 98% is added to the acid mixer 17. The amount of industrial concentrated sulfuric acid used is 115% of the mass of the mineral powder after the transformation. The material stirred with the industrial concentrated sulfuric acid is fed into the acidification kiln 18, and the acidification temperature of the acidification kiln 18 is controlled at 245°C;

[0043] S5, neutralization and lithium precipitation: the material after acidification in the acidification kiln 18 is slurried and soaked in water. After the material is soaked in water, it is filtered to separate the filtrate and the filter residue. The filtrate is led to the sedimentation tank 19, alkali is added to the filtrate for neutralization and sodium carbonate is added for replacement reaction to produce lithium carbonate precipitate. The Li2O grade of the filter residue after acidification, neutralization and filtration is 0.17%, and the leaching rate is 97.42%.

[0044] Example 4: Figure 1 The method for extracting lithium by roasting and transforming spodumene flotation concentrate shown in the figure comprises the following steps:

[0045] S1. Filtration: Select spodumene flotation concentrate with a mass content of 50% of ore particle size -0.074 mm, a content of less than 2% of ore with a maximum particle size of 1 mm or more, and a Li2O content of 4%, and filter the spodumene flotation concentrate into a filter cake containing 8% water;

[0046] S2, preheating: the filter cake is fed into the roasting preheating system 12 through the forced feeding device 11, the roasting preheating system 12 evaporates the moisture of the filter cake to form mineral powder and heats the mineral powder to 200°C, the mineral powder in the roasting preheating system 12 is directly fed into the heating system 13 after preheating treatment, the exhaust gas temperature in the roasting preheating system 12 is 100°C to 150°C, the exhaust gas in the roasting preheating system 12 is discharged after passing through the dust collector 22, the exhaust fan 23 and the chimney 24, and the dust collector 22 feeds the collected mineral ash into the transformation reaction chamber 15;

[0047] S3, heating and separation: the ore powder discharged from the roasting preheating is fed into the heating system 13 and heated to 1100°C, the heated ore powder is separated by the gas-solid separation system 14, the ore powder after gas-solid separation is fed into the transformation reaction chamber 15, the hot gas of the gas-solid separation system 14 is fed into the roasting preheating system 12 to form hot air to preheat the filter cake, the heating system 13 provides heat through combustion of the fuel burner, and the fuel of the fuel burner is natural gas or coal powder;

[0048] S4, oxidation acidification: air is introduced into the bottom of the reaction chamber, and the mineral powder is oxidized in a fluidized state under the action of air. The oxidation time is controlled at 30 minutes, and the spodumene in the mineral powder is transformed into β-type spodumene. The transformed mineral powder is cooled by the cooling system 16 and directly fed into the acid mixer 17. At the same time, industrial concentrated sulfuric acid with a content of 90% to 98% is added to the acid mixer 17. The amount of industrial concentrated sulfuric acid used is 80% of the mass of the mineral powder after the transformation. The material stirred with the industrial concentrated sulfuric acid is fed into the acidification kiln 18, and the acidification temperature of the acidification kiln 18 is controlled at 250°C;

[0049] S5, neutralization and lithium precipitation: the material after acidification in the acidification kiln 18 is slurried and soaked in water. After the material is soaked in water, it is filtered to separate the filtrate and the filter residue. The filtrate is led to the sedimentation tank 19, alkali is added to the filtrate for neutralization and sodium carbonate is added for replacement reaction to produce lithium carbonate precipitate. The Li2O grade of the filter residue after acidification, neutralization and filtration is 0.28%, and the leaching rate is 93.64%.

[0050] Example 5: Figure 1 The method for extracting lithium by roasting and transforming spodumene flotation concentrate shown in the figure comprises the following steps:

[0051] S1. Filtration: Select spodumene flotation concentrate with a mass content of 90% of ore particle size -0.074 mm, a content of less than 2% of ore with a maximum particle size of 1 mm or more, and a Li2O taste of 6.5%, and filter the spodumene flotation concentrate into a filter cake containing 14% water;

[0052] S2, preheating: the filter cake is fed into the roasting preheating system 12 through the forced feeding device 11, the roasting preheating system 12 evaporates the moisture of the filter cake to form mineral powder and heats the mineral powder to 350°C, the mineral powder in the roasting preheating system 12 is directly fed into the heating system 13 after preheating treatment, the temperature of the exhaust gas discharged by preheating is 100°C to 150°C, the exhaust gas in the roasting preheating system 12 is discharged after passing through the dust collector 22, the exhaust fan 23 and the chimney 24, and the dust collector 22 feeds the collected mineral ash into the transformation reaction chamber 15;

[0053] S3, heating and separation: the ore powder discharged from the roasting preheating is fed into the heating system 13 and heated to 1200°C, the heated ore powder is separated by the gas-solid separation system 14, the ore powder after gas-solid separation is fed into the transformation reaction chamber 15, the hot gas of the gas-solid separation system 14 is fed into the roasting preheating system 12 to form hot air to preheat the filter cake, the heating system 13 provides heat through combustion of the fuel burner, and the fuel of the fuel burner is natural gas or coal powder;

[0054] S4, oxidation acidification: air is introduced into the bottom of the reaction chamber, and the mineral powder is oxidized in a fluidized state under the action of air. The oxidation time is controlled at 60 minutes, and the spodumene in the mineral powder is transformed into β-type spodumene. The transformed mineral powder is cooled by the cooling system 16 and directly fed into the acid mixer 17. At the same time, industrial concentrated sulfuric acid with a content of 90% to 98% is added to the acid mixer 17. The amount of industrial concentrated sulfuric acid used is 120% of the mass of the mineral powder after the transformation. The material stirred with the industrial concentrated sulfuric acid is fed into the acidification kiln 18, and the acidification temperature of the acidification kiln 18 is controlled at 300°C;

[0055] S5, neutralization and lithium precipitation: the material after acidification in the acidification kiln 18 is slurried and soaked in water. After the material is soaked in water, it is filtered to separate the filtrate and the filter residue. The filtrate is led to the sedimentation tank 19, alkali is added to the filtrate for neutralization and sodium carbonate is added for replacement reaction to produce lithium carbonate precipitate. The Li2O grade of the filter residue after acidification, neutralization and filtration is 0.22%, and the leaching rate is 98.52%.

[0056] The above description shows and describes the preferred embodiments of the present invention. As mentioned above, it should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the invention concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art do not depart from the spirit and scope of the present invention, and should be within the scope of protection of the claims attached to the present invention.

Claims

1. A method for extracting lithium by roasting and transforming spodumene flotation concentrate, characterized in that: The following steps are involved: S1. Filtration: Select spodumene flotation concentrate with a mass content of 50% to 90% of ore particle size -0.074 mm, a maximum ore particle size of 1 mm or more and a content of less than 2%, and a Li2O taste of 4% to 6.5%, and filter the spodumene flotation concentrate into a filter cake containing 8 to 14% water; S2, preheating: the filter cake is fed into the roasting preheating system through the forced feeding equipment. The roasting preheating system evaporates the moisture of the filter cake to form mineral powder and heats the mineral powder to 200℃~350℃. The mineral powder in the roasting preheating system is directly fed into the heating system after preheating treatment. The temperature of the exhaust gas discharged by preheating is 100℃~150℃; S3, heating and separation: the calcined preheated ore powder is fed into the heating system and heated to 1100°C to 1200°C. The heated ore powder is separated by the gas-solid separation system, and the ore powder after gas-solid separation is fed into the transformation reaction chamber; S4, oxidation acidification: air is introduced into the bottom of the reaction chamber, and the mineral powder is oxidized in a fluidized state under the action of air. The oxidation time is controlled at 30-60 minutes, and the spodumene in the mineral powder is transformed into β-type spodumene. The transformed mineral powder is cooled by a cooling system and directly fed into an acid mixer. At the same time, industrial concentrated sulfuric acid with a content of 90% to 98% is added to the acid mixer. The amount of industrial concentrated sulfuric acid used is 80% to 120% of the mass of the mineral powder after the transformation. The material stirred with industrial concentrated sulfuric acid is fed into an acidification kiln, and the acidification temperature of the acidification kiln is controlled at 250°C to 300°C; S5. Neutralization and lithium precipitation: The material after acidification in the acidification kiln is slurried and soaked in water. After the material is soaked in water, it is filtered to separate the filtrate and the filter residue. The filtrate is sent to the sedimentation tank, alkali is added to the filtrate for neutralization and sodium carbonate is added for replacement reaction to produce lithium carbonate precipitate.

2. The method for extracting lithium by roasting and transforming spodumene flotation concentrate according to claim 1, wherein: The hot air from the gas-solid separation system is fed into the roasting preheating system to form hot air to preheat the filter cake.

3. The method for extracting lithium by roasting and transforming spodumene flotation concentrate according to claim 1, characterized in that: The hot air in the roasting preheating system is discharged after passing through a dust collector, an exhaust fan and a chimney, and the dust collector feeds the collected ash into the transformation reaction chamber.

4. The method for extracting lithium by roasting and transforming spodumene flotation concentrate according to claim 1, characterized in that: The heating system provides heat through combustion of a fuel burner, and the fuel of the fuel burner is natural gas or pulverized coal.