High-specific-strength CrMoNbVTix refractory high-entropy alloy and preparation method thereof
By adding Ti element to CrMoNbVTix high-entropy alloy and using vacuum arc melting technology, a single body-centered cubic structure is formed, which solves the deficiencies in room temperature deformation ability and density of refractory high-entropy alloys and achieves low density, high strength and excellent properties. The plastic effect meets the application needs in the aerospace field.
Patent Information
- Application Number
- CN202410921578.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-10-29
AI Technical Summary
Existing refractory high-entropy alloys have insufficient room temperature deformation ability and high density, making it difficult to meet higher application requirements, especially in lightweight and high-strength materials in the aerospace field.
The preparation method of CrMoNbVTix refractory high-entropy alloy is adopted, and Ti element is added through vacuum arc melting to form a single body-centered cubic structure, which improves the room temperature plasticity and processability of the alloy, and is optimized through electromagnetic stirring and high-purity argon protective atmosphere. The chemical composition and density of the alloy.
The CrMoNbVTix high-strength alloy with low density, high strength and good room temperature plasticity has been realized, which improves the specific strength of the alloy and expands its application prospects in the aerospace field.
Smart Images

Figure CN118854136A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of refractory high entropy alloys, in particular to a high specific strength CrMoNbVTi x Refractory high entropy alloy and method for preparing the same. Background Art
[0002] The rapid development of the modern aerospace industry relies on high-performance alloy materials. High-entropy alloys have changed the traditional alloy design concept. They are usually composed of no less than 5 elements, and each element is mixed in an equimolar or nearly equimolar ratio. Refractory high-entropy alloys composed of refractory metal elements have excellent high-temperature strength, breaking through the service temperature limit of existing nickel-based high-temperature alloys. Therefore, they have broad application prospects in ultra-high temperature fields such as aviation, aerospace, metallurgy, and nuclear energy.
[0003] By adding different kinds of elements, refractory high entropy alloys can form a single-phase solid solution. Due to the difference in radius between different atoms, severe lattice distortion occurs, which in turn produces a strong solid solution strengthening effect. Therefore, compared with traditional alloys, refractory high entropy alloys can have higher strength.
[0004] Although refractory high entropy alloys have high strength, their room temperature deformation capacity is insufficient, which restricts the machinability of the alloys. For example, the room temperature yield strength of the NbMoTaW alloy prepared by arc melting is 1058MPa, and the compressive yield strength at 800℃ is 552MPa, but the room temperature compressive strain rate is only 2%. The room temperature compressive yield strength of the CrMoNbV alloy prepared by arc melting is about 1518MPa, and the yield strength at 800℃ can still be maintained at 1100MPa, but the room temperature compressive strain rate is only 5%. In addition, the density of refractory high entropy alloys is relatively high, and the specific strength of the comprehensive strength and density factor needs to be further improved. Therefore, the research and development of a refractory high entropy alloy with low density, high strength and good room temperature plasticity is a technical challenge and research hotspot in this field. Summary of the invention
[0005] The purpose of the present invention is to provide a high specific strength CrMoNbVTi x A refractory high-entropy alloy and a preparation method thereof are provided to solve the problem that the comprehensive strength and specific strength brought by the density of existing refractory high-entropy alloys are difficult to meet higher application requirements, and to obtain a new refractory high-entropy alloy with low density, high strength and good room temperature plasticity.
[0006] In order to achieve the above object, the present invention adopts the following technical solution:
[0007] The present invention provides a high specific strength CrMoNbVTi x A method for preparing a refractory high entropy alloy, wherein the chemical composition of the refractory high entropy alloy is: CrMoNbVTix , x represents the number of moles of atoms, and the value range of x is: 0 <x≤1;
[0008] The preparation method thereof comprises the following steps:
[0009] (1) Calculate the required mass of Cr, Mo, Nb, V, and Ti according to the amount of the designed components, and then weigh and proportion them to obtain a mixed material for later use;
[0010] (2) The mixed material obtained in step (1) is melted, and after the melting is completed, it is cooled to room temperature and sampled to obtain a high specific strength CrMoNbVTi x Refractory high entropy alloys.
[0011] Preferably, in the step (1), Cr metal blocks, Mo metal blocks, Nb metal blocks, V metal blocks and Ti metal blocks are weighed and proportioned; the purity of the Cr metal blocks, Mo metal blocks, Nb metal blocks, V metal blocks and Ti metal blocks are all ≥99.9%.
[0012] Preferably, in step (2), the smelting is carried out in a vacuum arc melting furnace; before smelting, the sample chamber of the vacuum arc melting furnace is evacuated and argon gas is introduced in sequence.
[0013] Preferably, in step (2), the purity of argon is ≥99.99%; and the internal pressure of the vacuum arc melting furnace when argon is introduced is -0.06 to -0.04 MPa.
[0014] Preferably, in step (2), the smelting is performed ≥ 8 times, and the duration of each smelting is 3 to 5 minutes; and electromagnetic stirring is performed during the smelting process.
[0015] The present invention also provides the high specific strength CrMoNbVTi x High specific strength CrMoNbVTi prepared by preparation method of refractory high entropy alloy x Refractory high entropy alloys.
[0016] It can be seen from the above technical solution that compared with the prior art, the present invention has the following beneficial effects:
[0017] (1) The Cr, Mo, Nb, V, and Ti metal elements added in the present invention are all high melting point elements. The prepared alloy has high high temperature strength and has potential application prospects under high temperature service conditions.
[0018] (2) The alloy of the present invention has a single body-centered cubic structure. The addition of Ti element enhances the room temperature plasticity of the alloy and improves the machinability of the alloy.
[0019] (3) The alloy of the present invention introduces the Ti element with a relatively low density, which can reduce the density of the alloy while maintaining a relatively high strength, thereby improving the specific strength of the alloy. As a type of lightweight and high-strength alloy, it has broad application prospects in the aerospace field.
[0020] (4) The preparation method of the present invention is formulated according to the nominal chemical composition, and the alloy is prepared by melting in a vacuum arc furnace. The method is simple, easy to implement, and has wide applicability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0022] Figure 1 CrMoNbVTi x XRD patterns of refractory high entropy alloys;
[0023] Figure 2 CrMoNbVTi x Room temperature compressive stress-strain curve of the alloy;
[0024] Figure 3 CrMoNbVTi 0.25 Microstructure and element distribution of alloy;
[0025] Figure 4 CrMoNbVTi 0.5 Microstructure and element distribution of alloy;
[0026] Figure 5 CrMoNbVTi 0.75 Microstructure and element distribution of alloy;
[0027] Figure 6 It is the 800℃ compressive stress-strain curve of CrMoNbVTi alloy;
[0028] Figure 7 The microstructure and element distribution diagram of CrMoNbVTi alloy;
[0029] Figure 8 CrMoNbVTi 0.25 CrMoNbVTi 0.5 、CrMoNbVTi 0.75 , CrMoNbVTi, other high entropy alloys and traditional alloys versus test temperature. DETAILED DESCRIPTION
[0030] The present invention provides a high specific strength CrMoNbVTi x A method for preparing a refractory high entropy alloy, wherein the chemical composition of the refractory high entropy alloy is: CrMoNbVTi x , x represents the number of moles of atoms, and the value range of x is: 0 <x≤1;
[0031] The preparation method thereof comprises the following steps:
[0032] (1) Calculate the required mass of Cr, Mo, Nb, V, and Ti according to the amount of the designed components, and then weigh and proportion them to obtain a mixed material for later use;
[0033] (2) The mixed material obtained in step (1) is melted, and after the melting is completed, it is cooled to room temperature and sampled to obtain a high specific strength CrMoNbVTi x Refractory high entropy alloys.
[0034] In step (1) of the present invention, Cr metal blocks, Mo metal blocks, Nb metal blocks, V metal blocks and Ti metal blocks are weighed and proportioned; the purity of the Cr metal blocks, Mo metal blocks, Nb metal blocks, V metal blocks and Ti metal blocks is independently preferably ≥99.9%, more preferably ≥99.95%, and even more preferably ≥99.99%.
[0035] In step (2) of the present invention, smelting is carried out in a vacuum arc melting furnace; before smelting, the sample chamber of the vacuum arc melting furnace is evacuated and argon gas is introduced in sequence.
[0036] In step (2) of the present invention, the purity of argon is preferably ≥99.99%, more preferably ≥99.992%, and more preferably ≥99.995%; the internal pressure of the vacuum arc melting furnace when argon is introduced is preferably -0.06 to -0.04 MPa, and more preferably -0.05 MPa.
[0037] In step (2) of the present invention, the number of smelting is preferably ≥8 times, more preferably ≥10 times, and more preferably ≥11 times; the duration of each smelting is preferably 3 to 5 minutes, and more preferably 4 minutes; and electromagnetic stirring is performed during the smelting process.
[0038] The present invention also provides the high specific strength CrMoNbVTi x High specific strength CrMoNbVTi prepared by preparation method of refractory high entropy alloy x Refractory high entropy alloys.
[0039] In the present invention, when x=0.25, the chemical formula of the alloy is CrMoNbVTi 0.25 , which is a single-phase body-centered cubic crystal structure, the room temperature compressive yield strength is 1509MPa, and the maximum compressive strain is 10.1%.
[0040] In the present invention, when x=0.5, the chemical formula of the alloy is CrMoNbVTi 0.5 , which is a single-phase body-centered cubic crystal structure, the room temperature compressive yield strength is 1402MPa, and the maximum compressive strain is 10.4%.
[0041] In the present invention, when x=0.75, the chemical formula of the alloy is CrMoNbVTi 0.75 It has a single-phase body-centered cubic structure, a room temperature compressive yield strength of 1586MPa, and a maximum compressive strain of 9.5%.
[0042] In the present invention, when x=1, the chemical formula of the alloy is CrMoNbVTi, it is a single-phase body-centered cubic structure, the room temperature compressive yield strength is 1414 MPa, and the maximum compressive strain is 11.0%.
[0043] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0044] Example 1
[0045] CrMoNbVTi 0.25 Alloy preparation and characterization:
[0046] (1) Raw material preparation: The refractory high entropy alloy developed by the present invention comprises Cr, Mo, Nb, V and Ti. A metal ingot with a purity of 99.9% is used as the raw material. The mass of Cr, Mo, Nb, V and Ti required for each alloy is calculated according to the amount of the designed components, and then weighed and proportioned for smelting and alloy preparation.
[0047] (2) Alloy smelting: The alloy of the present invention is prepared using a vacuum arc melting furnace, the sample chamber is evacuated, and high-purity argon gas with a purity of 99.99% is introduced until the furnace pressure is -0.05MPa. During the smelting process, the alloy ingot is reversed and smelted at least 8 times, each time for 3 minutes, and electromagnetic stirring is turned on. After the smelting is completed, it is cooled to room temperature and sampled to obtain an alloy ingot.
[0048] (3) Material mechanical property test and phase characterization: Wire cutting was used to cut cylindrical specimens with a diameter of 3.5 mm and a height of 5 mm from the smelted alloy ingots, and the room temperature mechanical properties of the alloy were tested using a universal mechanical testing machine. Small specimens were cut from the alloy ingots using wire cutting, and polished with 240#, 600#, 800#, 1000#, 2000#, 3000#, and 5000# sandpapers in turn, mechanically polished with 2.5μm diamond polishing paste, and ultrasonically cleaned with anhydrous ethanol and dried. The material was identified using an X-ray diffractometer (XRD). Figure 1 CrMoNbVTi 0.25 The XRD results of the alloy show that the alloy has a single-phase body-centered cubic structure. Figure 2 CrMoNbVTi 0.25 The room temperature stress-strain curve of the alloy shows that the room temperature compressive yield strength of the alloy is 1509 MPa and the maximum compressive strain is 10.1%. Figure 3 CrMoNbVTi 0.25 The microstructure and element distribution of the alloy show that Mo is mainly distributed in the dendrite region, Cr and Ti are mainly distributed between the dendrites, and Nb and V are evenly distributed. Figure 8 CrMoNbVTi 0.25 Relationship between alloy specific yield strength and test temperature. The room temperature specific yield strength of the alloy is about 191 MPa·g -1 cm 3 .
[0049] Example 2
[0050] CrMoNbVTi 0.5 Alloy preparation and characterization:
[0051] (1) Raw material preparation: The refractory high entropy alloy developed by the present invention comprises Cr, Mo, Nb, V and Ti. A metal ingot with a purity of 99.9% is used as the raw material. The mass of Cr, Mo, Nb, V and Ti required for each alloy is calculated according to the amount of the designed components, and then weighed and proportioned for smelting and alloy preparation.
[0052] (2) Alloy smelting: The alloy of the present invention is prepared using a vacuum arc melting furnace, the sample chamber is evacuated, and high-purity argon gas with a purity of 99.99% is introduced until the furnace pressure is -0.05MPa. During the smelting process, the alloy ingot is reversed and smelted at least 8 times, each time for 3 minutes, and electromagnetic stirring is turned on. After the smelting is completed, it is cooled to room temperature and sampled to obtain an alloy ingot.
[0053] (3) Material mechanical property testing and phase characterization: Cylindrical specimens with a diameter of 3.5 mm and a height of 5 mm were cut from the smelted alloy ingots by wire cutting, and the room temperature mechanical properties of the alloy were tested using a universal mechanical testing machine; small specimens were cut from the alloy ingots by wire cutting, and polished with 240#, 600#, 800#, 1000#, 2000#, 3000#, and 5000# sandpapers in sequence, mechanically polished with 2.5μm diamond polishing paste, and ultrasonically cleaned with anhydrous ethanol and dried. Figure 1 CrMoNbVTi 0.5 The XRD results of the alloy show that the alloy has a single-phase body-centered cubic structure. Figure 2 CrMoNbVTi 0.5 The room temperature compressive stress-strain curve of the alloy shows that the room temperature compressive yield strength of the alloy is about 1402 MPa, and the maximum compressive strain is about 10.4%. Figure 4 CrMoNbVTi 0.5 The microstructure and element distribution of the alloy show that Mo is mainly distributed in the dendrite region, Cr and Ti are mainly distributed between the dendrites, and Nb and V are evenly distributed. Figure 8 CrMoNbVTi 0.5 Relationship between alloy specific yield strength and test temperature. The room temperature specific yield strength of the alloy is about 182MPa·g -1 cm 3 .
[0054] Example 3
[0055] CrMoNbVTi 0.75 Alloy preparation and characterization:
[0056] (1) Raw material preparation: The refractory high entropy alloy developed by the present invention comprises Cr, Mo, Nb, V and Ti. A metal ingot with a purity of 99.9% is used as the raw material. The mass of Cr, Mo, Nb, V and Ti required for each alloy is calculated according to the amount of the designed components, and then weighed and proportioned for smelting and alloy preparation.
[0057] (2) Alloy smelting: The alloy of the present invention is prepared using a vacuum arc melting furnace, the sample chamber is evacuated, and high-purity argon gas with a purity of 99.99% is introduced until the furnace pressure is -0.05MPa. During the smelting process, the alloy ingot is reversed and smelted at least 8 times, each time for 3 minutes, and electromagnetic stirring is turned on. After the smelting is completed, it is cooled to room temperature and sampled to obtain an alloy ingot.
[0058] (3) Material mechanical property testing and phase characterization: Cylindrical specimens with a diameter of 3.5 mm and a height of 5 mm were cut from the smelted alloy ingots by wire cutting, and the room temperature mechanical properties of the alloy were tested using a universal mechanical testing machine; small specimens were cut from the alloy ingots by wire cutting, and polished with 240#, 600#, 800#, 1000#, 2000#, 3000#, and 5000# sandpapers in sequence, mechanically polished with 2.5μm diamond polishing paste, and ultrasonically cleaned with anhydrous ethanol and dried. Figure 1 CrMoNbVTi 0.75 The XRD results of the alloy show that the alloy has a single-phase body-centered cubic structure. Figure 2 CrMoNbVTi 0.75 The room temperature compressive stress-strain curve of the alloy shows that the room temperature compressive yield strength of the alloy is about 1586 MPa, and the maximum compressive strain is about 9.5%. Figure 5 CrMoNbVTi 0.75 The microstructure and element distribution of the alloy show that Mo segregation is more significant and is enriched in the dendrite area. Cr and Ti are mainly distributed between dendrites, while Nb and V are evenly distributed. Figure 8 CrMoNbVTi 0.75 Relationship between alloy specific yield strength and test temperature. The room temperature specific yield strength of the alloy is about 212MPa·g -1 cm 3 .
[0059] Example 4
[0060] Preparation and characterization of CrMoNbVTi alloy:
[0061] (1) Raw material preparation: The refractory high entropy alloy developed by the present invention is composed of Cr, Mo, Nb, V and Ti. A metal ingot with a purity of 99.9% is used as the raw material. The mass of Cr, Mo, Nb, V and Ti required for each alloy is calculated according to the amount of the designed components, and then weighed and proportioned for smelting and alloy preparation;
[0062] (2) Alloy smelting: The alloy of the present invention is prepared using a vacuum arc melting furnace, the sample chamber is evacuated, and high-purity argon gas with a purity of 99.99% is introduced until the furnace pressure is -0.05MPa. During the smelting process, the alloy ingot is reversed and smelted at least 8 times, each time for 3 minutes, and electromagnetic stirring is turned on. After the smelting is completed, it is cooled to room temperature and sampled to obtain an alloy ingot.
[0063] (3) Material mechanical property test and phase characterization: Wire cutting was used to cut cylindrical specimens with a diameter of 3.5 mm and a height of 5 mm from the smelted alloy ingot, and the room temperature mechanical properties of the alloy were tested using a universal mechanical testing machine. Wire cutting was used to cut cylindrical specimens with a diameter of 4 mm and a height of 6 mm from the smelted alloy ingot, and the high temperature mechanical properties of the alloy were tested using a universal mechanical testing machine. Small specimens were cut from the alloy ingot using wire cutting, and polished with 240#, 600#, 800#, 1000#, 2000#, 3000#, and 5000# sandpapers in turn, mechanically polished with 2.5μm diamond polishing paste, and cleaned with anhydrous ethanol and dried. Figure 1 The XRD results of CrMoNbTiV alloy show that the alloy has a single-phase body-centered cubic structure. Figure 2 The room temperature compressive stress-strain curve of the CrMoNbTiV alloy shows that the room temperature compressive yield strength of the alloy is about 1414 MPa, and the maximum compressive strain is about 11.0%. Figure 6 This is the compressive stress-strain curve of CrMoNbVTi alloy at 800℃, and the yield strength is about 1100MPa. Figure 7 Figure 3 is the microstructure and element distribution diagram of CrMoNbVTi alloy. Mo is enriched in the dendrite area, Cr and Ti are mainly distributed between the dendrites, and Nb and V are evenly distributed. Figure 8 The relationship between the specific yield strength and test temperature of the CrMoNbVTi alloy is shown in the figure. The specific yield strength of the alloy at room temperature is about 193 MPa·g -1 cm 3 . , 800℃ specific yield strength is about 150MPa·g -1 cm 3 .
[0064] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A high specific strength CrMoNbVTi x A method for preparing a refractory high entropy alloy, characterized in that: The chemical composition of the refractory high entropy alloy is: CrMoNbVTi x , x represents the number of moles of atoms, and the value range of x is: 0 <x≤1; The preparation method thereof comprises the following steps: (1) Calculate the required mass of Cr, Mo, Nb, V, and Ti according to the amount of the designed components, and then weigh and proportion them to obtain a mixed material for later use; (2) The mixed material obtained in step (1) is melted, and after the melting is completed, it is cooled to room temperature and sampled to obtain a high specific strength CrMoNbVTi x Refractory high entropy alloys.
2. The high specific strength CrMoNbVTi according to claim 1 x A method for preparing a refractory high entropy alloy, characterized in that: In the step (1), Cr metal blocks, Mo metal blocks, Nb metal blocks, V metal blocks and Ti metal blocks are weighed and proportioned; the purity of the Cr metal blocks, Mo metal blocks, Nb metal blocks, V metal blocks and Ti metal blocks are all ≥99.9%.
3. The high specific strength CrMoNbVTi according to claim 1 or 2. x A method for preparing a refractory high entropy alloy, characterized in that: In the step (2), the smelting is carried out in a vacuum arc melting furnace; before the smelting, the sample chamber of the vacuum arc melting furnace is evacuated and argon gas is introduced in sequence.
4. The high specific strength CrMoNbVTi according to claim 3 x A method for preparing a refractory high entropy alloy, characterized in that: In the step (2), the purity of argon is ≥ 99.99%; The gauge pressure inside the vacuum arc melting furnace when argon gas is introduced is -0.06 to -0.04 MPa.
5. The high specific strength CrMoNbVTi according to claim 4 x A method for preparing a refractory high entropy alloy, characterized in that: In the step (2), the smelting is performed ≥ 8 times, and the duration of each smelting is 3 to 5 minutes; and electromagnetic stirring is performed during the smelting process.
6. The high specific strength CrMoNbVTi according to any one of claims 1 to 5 x High specific strength CrMoNbVTi prepared by preparation method of refractory high entropy alloy x Refractory high entropy alloys.