Preparation method of TiAl-based composite material synergistically reinforced by Nb transition layer and B4C

By introducing Nb transition layer and B4C on the surface of TiAl alloy powder, TiAl matrix composite materials were prepared by powder metallurgy method, the problem of insufficient strength and oxidation resistance of TiAl alloy under high temperature conditions was solved, and the high-temperature performance improvement and industrialization of the material was achieved. applicability.

CN118639048BActive Publication Date: 2024-12-06XIAN RARE METAL MATERIALS RES INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411123842.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-12-06
Estimated Expiration
2044-08-16

AI Technical Summary

Technical Problem

The single TiAl alloy has problems such as poor room temperature plasticity, poor high-temperature oxidation resistance and low high-temperature strength above 800℃ under high temperature conditions, which limits its further development and application in aerospace and other fields.

Method used

A low-energy ball mill is used to introduce an Nb transition layer to make B4C uniformly coat the surface of TiAl alloy powder, and a TiAl matrix composite material is prepared by powder metallurgy method to form a structure that enhances the Nb transition layer and B4C together, improving high temperature strength and oxidation resistance.

Benefits of technology

The high-temperature strength of TiAl matrix composite material is achieved, the microstructure and thermal stability of the material are enhanced, and the problems of B4C powder agglomeration and low interface bonding rate are solved, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118639048B_ABST
    Figure CN118639048B_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a TiAl-based composite material synergistically reinforced by a Nb transition layer and B4C, the method comprising the following steps: 1. weighing raw material powder; 2. subjecting TiAl prealloy powder and Nb powder to primary low-energy ball milling to obtain a TiAl alloy powder having a Nb transition layer; 3. subjecting the TiAl alloy powder having a Nb transition layer to secondary low-energy ball milling with B4C powder to obtain a mixed powder in which a reinforcement is uniformly dispersed on the surface of the TiAl alloy powder; 4. screening treatment; 5. sintering the mixed powder to obtain a TiAl-based composite material. The invention introduces a Nb transition layer between the matrix powder and the B4C powder, so that the B4C powder is uniformly dispersed on the surface of the transition layer, effectively avoiding the ball milling agglomeration phenomenon of the B4C powder, obtaining a TiAl-based composite material synergistically reinforced by Nb and B4C, and improving the high temperature strength and oxidation resistance of the TiAl-based composite material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of TiAl alloys and composite materials thereof, and particularly relates to a method for preparing a TiAl-based composite material synergistically reinforced by a Nb transition layer and B4C. Background Art

[0002] The rapid development of the aerospace industry has put forward higher requirements for high-temperature structural materials. TiAl alloy is a low-density (3.9g / cm 3 –4.2g / cm 3 ), high specific strength and specific stiffness, and excellent creep resistance and high-temperature oxidation resistance. Compared with traditional titanium alloys, it has the great advantage of being used under high temperature conditions (800-900°C), and is widely used in aerospace, shipbuilding, automobiles and other fields. It is expected to replace some nickel-based high-temperature alloys in the near future. However, the shortcomings of single TiAl alloys, such as poor room temperature plasticity, poor high-temperature oxidation resistance and low high-temperature strength above 800°C, limit its further development and application. In recent years, TiAl-based alloys have been reinforced with continuous fiber reinforcement or discontinuous short fibers and particles, so that TiAl-based composites have the comprehensive excellent properties of both matrix and reinforcement.

[0003] Powder metallurgy has unique advantages in the preparation of TiAl-based alloys. It can refine grains and reduce casting defects such as segregation. At the same time, it can solve the problems of poor casting quality and difficulty in forming at room temperature of TiAl-based alloys by combining with high-temperature forming processes. In addition, the powder metallurgy method is used to prepare TiAl-based composite materials, and the reinforcing phase is generated in situ in the matrix, and the interface between the reinforcing phase and the matrix is ​​firmly bonded.

[0004] Therefore, a method for preparing a TiAl-based composite material synergistically reinforced with a Nb transition layer and B4C is needed. Summary of the invention

[0005] The technical problem to be solved by the present invention is to provide a method for preparing a TiAl-based composite material synergistically reinforced by a Nb transition layer and B4C in view of the deficiencies of the above-mentioned prior art. The method uses low-energy ball milling to introduce a Nb transition layer, so that B4C is evenly coated on the surface of the TiAl alloy powder, eliminating the agglomeration phenomenon of B4C during the ball milling process, and uses a powder metallurgy method to prepare the TiAl-based composite material, which can achieve near-net molding and ensure that the composition and microstructure of the material are controllable. B4C and the TiAl matrix in situ generate carbide or boride particles to limit the rapid growth of the matrix grains, thereby improving the high-temperature strength of the TiAl-based composite material.

[0006] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a TiAl-based composite material synergistically reinforced with a Nb transition layer and B4C, characterized in that the method comprises the following steps:

[0007] Step 1, weighing raw material powders: weighing TiAl pre-alloyed powder, Nb powder and B4C powder;

[0008] Step 2, initial low-energy ball milling: the TiAl pre-alloyed powder, Nb powder and grinding balls weighed in step 1 are placed in a ball mill, and then the ball mill is evacuated and argon gas is introduced into the ball mill, and then the ball mill is placed in a planetary ball mill for initial low-energy ball milling, so as to obtain TiAl alloy powder and grinding balls with a Nb transition layer on the surface in the ball mill;

[0009] Step 3, secondary low-energy ball milling: add the B4C powder weighed in step 1 to the ball milling jar containing the TiAl alloy powder with a Nb transition layer on the surface and the grinding balls obtained in step 2, then evacuate the ball milling jar and introduce argon gas, and then place it in a planetary ball mill for secondary low-energy ball milling to obtain a mixed powder and grinding balls with reinforcements uniformly dispersed on the surface of the TiAl alloy powder;

[0010] Step 4: Screening: Screening the mixed powder and grinding balls obtained in step 3 in which the reinforcement is evenly dispersed on the surface of the TiAl alloy powder;

[0011] Step 5, sintering: the mixed powder in which the reinforcement is evenly dispersed on the surface of the TiAl alloy powder after screening in step 4 is loaded into a graphite mold, and then the graphite mold is placed in a high-temperature sintering furnace, and then pressure sintered under vacuum to obtain a TiAl-based composite material with a Nb transition layer and B4C synergistically reinforced.

[0012] The invention uses primary low-energy ball milling to uniformly coat Nb powder on the surface of TiAl alloy powder to form a Nb transition layer, introduces the Nb transition layer to optimize the interface bonding between the reinforcement body and the matrix powder, and adds the Nb element to improve the room temperature plasticity and oxidation resistance of the TiAl alloy. Secondary low-energy ball milling is used to uniformly disperse B4C on the TiAl alloy powder with the Nb transition layer coated on the surface, removes the grinding balls by screening, and adopts powder metallurgy technology, that is, pressurized sintering molding to quickly densify the mixed powder to obtain a TiAl-based composite material with the Nb transition layer and B4C synergistically reinforced. Adding Nb and B4C is beneficial to significantly refine the grains of the TiAl composite material, reduces the size of the lamellar clusters, and optimizes the microstructure and thermal stability of the composite material. Secondly, B4C reacts with the matrix in situ to generate second phase particles, so that the strength and plasticity of the composite material are significantly enhanced. The Nb element is dissolved in the TiAl matrix, which can cause lattice distortion, increase the movement resistance of dislocations, and simultaneously improve the strength of the TiAl-based composite material.

[0013] After the initial low-energy ball milling in the present invention, there is no need to take out the product of the initial low-energy ball milling from the ball milling jar, and secondary low-energy ball milling can be performed after only adding B4C powder, thereby improving production efficiency and preventing the introduction of impurities.

[0014] The Nb powder used in the present invention is a constituent element of the TiAl alloy and can be well combined with the TiAl alloy powder matrix. The B4C powder used is in-situ self-generated to obtain carbide particles or boride particles, and the interface bonding is firm and pollution-free. The selected powder raw material has low cost and is suitable for industrial production.

[0015] The method for preparing a TiAl-based composite material synergistically reinforced by a Nb transition layer and B4C is characterized in that the mass ratio of the spherical TiAl pre-alloyed powder, Nb powder and B4C powder weighed in step 1 is 46~48.5:1.25~3.75:0.25. By limiting the mass ratio of the raw material powders, it is beneficial to ball milling and mixing the alloy powders, and the Nb powder is basically completely coated on the surface of the TiAl powder, avoiding the low coverage rate of the Nb powder on the surface of the TiAl powder or the dispersion of the Nb powder between the TiAl powders, ensuring the homogenization of the structure of the TiAl composite material after sintering, and the excessively high content of reinforcement is easy to cause particle agglomeration, and the content of the reinforcement phase of the sintered TiAl composite material is controlled, which is beneficial to exerting the excellent performance of the TiAl composite material.

[0016] The above-mentioned method for preparing a TiAl-based composite material synergistically reinforced with a Nb transition layer and B4C is characterized in that the TiAl pre-alloyed powder in step one is spherical, with a particle size of 45μm~150μm, and the material is Ti-47.7Al-7.8Nb, Ti-47Al-2W-0.5Si, Ti-45.5Al-4Nb or Ti4822, the Nb powder is spherical or irregularly flaky, with a particle size of 30μm~80μm, and the particle size of the B4C powder is 10μm~40μm. The TiAl pre-alloyed powder used in the present invention is prepared by a plasma rotating electrode method or a gas atomization method, has good fluidity and dispersibility, high sphericity, and a wide particle size distribution, which is conducive to the formation of a sintering neck and improves the compactness of the TiAl composite material. The present invention controls the morphology and powder particle size of the Nb powder, which is conducive to the Nb powder being continuously attached to the surface of the matrix particles during the collision, extrusion, deformation and the like of the grinding balls during the ball milling process to form a good interface bonding. By controlling the powder particle size of the B4C powder, it is conducive to the small-sized and high-hardness B4C powder being extruded and embedded in the large-sized matrix particles during ball milling, promoting the uniform dispersion of the reinforcing phase generated in situ in the matrix during sintering and forming, and further ensuring the improvement of the strength of the TiAl-based composite material.

[0017] The method for preparing the TiAl-based composite material synergistically reinforced with a Nb transition layer and B4C is characterized in that the rotation speed of the initial low-energy ball milling in step 2 is 50 r / min to 200 r / min, the time is 10 h to 15 h, and the ball-to-material ratio is 5 to 8: 1. The present invention controls the parameters of the initial low-energy ball milling to ensure that the Nb powder can be evenly coated on the surface of the TiAl alloy powder and form a uniform Nb transition layer, thereby avoiding the problem of uneven mixing of the Nb powder and the TiAl alloy powder, and further ensuring the improvement of the performance of the TiAl-based composite material.

[0018] The method for preparing the TiAl-based composite material synergistically reinforced by the Nb transition layer and B4C is characterized in that, in the TiAl alloy powder having the Nb transition layer on the surface in step 2, 60% to 90% of the surface area of ​​the TiAl alloy powder is coated with the Nb transition layer. The present invention controls the coating area of ​​the Nb transition layer so that most of the surface area of ​​the TiAl alloy powder is coated with the Nb transition layer. The uniform coating of most of the Nb transition layer is conducive to the uniform dispersion of the Nb element of the prepared TiAl-based composite material, and further ensures the improvement of the strength of the TiAl-based composite material.

[0019] The method for preparing the TiAl-based composite material synergistically reinforced by the Nb transition layer and B4C is characterized in that the rotation speed of the secondary low-energy ball milling treatment in step 3 is 50r / min~200r / min, the time is 2h~5h, and the ball-to-material ratio is 5~8: 1. The present invention controls the parameters of the secondary low-energy ball milling to uniformly disperse the B4C powder on the surface of the TiAl alloy powder coated with the Nb transition layer, prevents the B4C powder from agglomerating or seriously breaking the powder, and further ensures the improvement of the performance of the TiAl-based composite material.

[0020] The method for preparing the TiAl-based composite material synergistically reinforced with a Nb transition layer and B4C is characterized in that the sieving treatment in step 4 uses a sieve with a mesh size of 80 to 200. The present invention separates the grinding balls from the mixed powder simply and efficiently by controlling the mesh size of the sieve.

[0021] The above-mentioned method for preparing a TiAl-based composite material synergistically reinforced with a Nb transition layer and B4C is characterized in that the pressure of the pressure sintering in step five is 35MPa~45MPa, and the process of pressure sintering is: first heated to 800℃~900℃ at a heating rate of 100℃ / min~150℃ / min, then kept warm for 1min~2min, then heated to 1100℃~1300℃ at a heating rate of 40℃ / min~60℃ / min, then kept warm for 7min~8min, then cooled to 700℃~800℃ at a cooling rate of 150℃ / min~200℃ / min, and finally cooled to room temperature with the furnace. The present invention adopts staged sintering. First, the TiAl powder containing a Nb transition layer is combined with a reinforcement by controlling the heating rate, the holding temperature and the time. The powder diffuses to carry out a chemical reaction. Then, the temperature is controlled to carry out sintering in the α+γ two-phase region, which is conducive to the composite material obtaining a near-lamellar structure composed of a large number of γ / α2 lamellar clusters and a small number of γ grains distributed between the lamellar layers. Finally, the cooling rate is controlled in combination with furnace cooling to room temperature, which is conducive to more uniform grain size of the composite material. By controlling the short-time, high-temperature sintering process, the powder can be quickly densified, thereby improving the density and strength of the TiAl-based composite material.

[0022] Compared with the prior art, the present invention has the following advantages:

[0023] 1. The present invention adopts low-energy ball milling to introduce a Nb transition layer, so that the B4C powder is evenly coated on the surface of the TiAl alloy powder, eliminating the agglomeration phenomenon of the B4C powder during the ball milling process, and adopts a powder metallurgy method to prepare a TiAl-based composite material, which can not only achieve near-net molding, but also ensure that the composition and microstructure of the material are controllable. The B4C powder and the TiAl matrix generate carbide or boride particles in situ to limit the rapid growth of the matrix grains, thereby improving the high-temperature strength of the TiAl-based composite material.

[0024] 2. The present invention introduces a Nb transition layer through the initial low-energy ball milling, thereby solving the problems that after B4C powder is ball-milled alone with TiAl pre-alloyed powder, part of the B4C powder is dispersedly distributed between the matrix particles, the interface bonding rate between the two is low, and the B4C powder agglomerates during the ball milling process. The introduced Nb transition layer can modify the interface between the matrix particles and the B4C powder. After ball milling, the Nb powder is coated on the surface of the spherical TiAl powder to form a rough transition layer, so that the B4C powder is relatively evenly distributed after being added, and the bonding performance of the matrix powder and the B4C powder is optimized. In addition, the addition of Nb can refine the structure and improve the strength and oxidation resistance.

[0025] 3. The present invention adopts powder metallurgy sintering to form the reinforcement and the matrix in situ to generate carbide or boride reinforcement phase particles, so as to refine the microstructure of the TiAl alloy and improve the strength of the TiAl-based composite material. In addition, the short-time and high-temperature sintering process ensures the rapid densification of the TiAl-based composite material.

[0026] 4. The preparation process of the present invention is simple, requires less experimental equipment, is low in cost, is easy to implement, and is suitable for industrial mass production.

[0027] The technical solution of the present invention is further described in detail below through the accompanying drawings and embodiments. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 The SEM image of the mixed powder prepared in Example 4 of the present invention in which the reinforcement is uniformly dispersed on the surface of the TiAl alloy powder and the distribution diagram of each element.

[0029] Figure 2 This is a low-magnification microstructure image of the TiAl-based composite material prepared in Example 4 of the present invention.

[0030] Figure 3 This is a high-magnification microstructure image of the TiAl-based composite material prepared in Example 4 of the present invention.

[0031] Figure 4 Engineering stress-strain diagram of the TiAl-based composite material prepared in Example 4 of the present invention at 850°C and 900°C. DETAILED DESCRIPTION

[0032] Example 1

[0033] This embodiment includes the following steps:

[0034] Step 1, weighing raw material powder: weighing 48.5g of spherical TiAl pre-alloyed powder with a particle size of 45μm~100μm, 1.25g of spherical Nb powder with a particle size of 30μm~80μm, and 0.25g of B4C powder with a particle size of 10μm~40μm; the material of the TiAl pre-alloyed powder is Ti-47.7Al-7.8Nb;

[0035] Step 2, initial low-energy ball milling: the TiAl pre-alloyed powder and Nb powder weighed in step 1 are loaded into a ball milling jar with a ball-to-material ratio of 6:1, and then the ball milling jar is evacuated and argon gas is introduced, and then placed in a planetary ball mill, and the initial low-energy ball milling is performed at a speed of 100 r / min for 11 hours, and a TiAl alloy powder with a Nb transition layer on the surface and a grinding ball are obtained in the ball milling jar; in the TiAl alloy powder with a Nb transition layer on the surface, 80% of the area on the surface of the TiAl alloy powder is coated with the Nb transition layer;

[0036] Step 3, secondary low-energy ball milling: add the B4C powder weighed in step 1 to the ball mill jar containing the TiAl alloy powder with a Nb transition layer on the surface and the grinding balls obtained in step 2, with a ball-to-material ratio of 6:1, and then evacuate the ball mill jar and introduce argon gas, and then place it in a planetary ball mill and perform secondary low-energy ball milling at a speed of 100 r / min for 3 hours to obtain a mixed powder and grinding balls with reinforcements uniformly dispersed on the surface of the TiAl alloy powder;

[0037] Step 4: Screening: The mixed powder and grinding balls obtained in step 3, in which the reinforcement is evenly dispersed on the surface of the TiAl alloy powder, are screened using a 80-mesh screen;

[0038] Step 5, sintering: the mixed powder in which the reinforcement after screening in step 4 is evenly dispersed on the surface of the TiAl alloy powder is loaded into a graphite mold with a diameter of 50 mm, and then the graphite mold is placed in a high-temperature sintering furnace. Thereafter, under vacuum and a sintering pressure of 35 MPa, the furnace temperature is raised to 800°C at a rate of 100°C / min and kept warm for 1 min, the furnace temperature is raised to 1100°C at a rate of 50°C / min and kept warm for 8 min, the furnace temperature is lowered to 800°C at a rate of about 200°C / min, and the furnace is cooled to room temperature to obtain a TiAl-based composite material.

[0039] The results show that the TiAl alloy powder surface in the TiAl-based composite material prepared in this embodiment has Nb transition layer and B4C powder evenly distributed, the main structure is γ / α2 lamellar clusters and a small amount of equiaxed γ structure distributed between the lamellar clusters, and the lamellar clusters are small and uniform.

[0040] Example 2

[0041] This embodiment includes the following steps:

[0042] Step 1, weighing raw material powder: weighing 47.25g of spherical TiAl pre-alloyed powder with a particle size of 45μm~149μm, 2.5g of Nb powder with a particle size of 30μm~80μm, and 0.25g of B4C powder with a particle size of 10μm~40μm; the material of the TiAl pre-alloyed powder is Ti-47Al-2W-0.5Si;

[0043] Step 2, initial low-energy ball milling: the TiAl pre-alloyed powder and Nb powder weighed in step 1 are loaded into a ball milling jar with a ball-to-material ratio of 5:1, and then the ball milling jar is evacuated and argon gas is introduced, and then placed in a planetary ball mill, and the initial low-energy ball milling is performed at a speed of 50 r / min for 15 hours, and a TiAl alloy powder with a Nb transition layer on the surface and a grinding ball are obtained in the ball milling jar; in the TiAl alloy powder with a Nb transition layer on the surface, 70% of the surface area of ​​the TiAl alloy powder is coated with the Nb transition layer;

[0044] Step 3, secondary low-energy ball milling: add the B4C powder weighed in step 1 to the ball milling jar containing the TiAl alloy powder with a Nb transition layer on the surface and the grinding balls obtained in step 2, with a ball-to-material ratio of 5:1, and then evacuate the ball milling jar and introduce argon gas, and then place it in a planetary ball mill and perform secondary low-energy ball milling at a speed of 200 r / min for 2 hours to obtain a mixed powder and grinding balls with reinforcements uniformly dispersed on the surface of the TiAl alloy powder;

[0045] Step 4: Screening: The mixed powder and grinding balls obtained in step 3, in which the reinforcement is evenly dispersed on the surface of the TiAl alloy powder, are screened using a 100-mesh screen;

[0046] Step 5, sintering: the mixed powder in which the reinforcement after screening in step 4 is evenly dispersed on the surface of the TiAl alloy powder is loaded into a graphite mold with a diameter of 50 mm, and then the graphite mold is placed in a high-temperature sintering furnace. Thereafter, under vacuum and a sintering pressure of 35 MPa, the furnace temperature is raised to 900°C at a rate of 150°C / min and kept warm for 1 min, the furnace temperature is raised to 1200°C at a rate of 40°C / min and kept warm for 8 min, and the furnace temperature is lowered to 800°C at a rate of about 150°C / min, and cooled to room temperature with the furnace to obtain a TiAl-based composite material.

[0047] The results show that the TiAl alloy powder surface in the TiAl-based composite material prepared in this embodiment has Nb transition layer and B4C powder evenly distributed, the main structure is γ / α2 lamellar clusters and a small amount of equiaxed γ structure distributed between the lamellar clusters, and the lamellar clusters are small and uniform.

[0048] Example 3

[0049] This embodiment includes the following steps:

[0050] Step 1, weighing raw material powder: weighing 46g of spherical TiAl pre-alloyed powder with a particle size of 45μm~149μm, 3.75g of Nb powder with a particle size of 30μm~80μm, and 0.25g of B4C powder with a particle size of 10μm~40μm; the material of the TiAl pre-alloyed powder is Ti-45.5Al-4Nb;

[0051] Step 2, initial low-energy ball milling: the TiAl pre-alloyed powder and Nb powder weighed in step 1 are loaded into a ball milling jar with a ball-to-material ratio of 8:1, and then the ball milling jar is evacuated and argon gas is introduced, and then placed in a planetary ball mill, and the initial low-energy ball milling is performed at a speed of 200 r / min for 10 hours, and a TiAl alloy powder with a Nb transition layer on the surface and a grinding ball are obtained in the ball milling jar; in the TiAl alloy powder with a Nb transition layer on the surface, 60% of the surface area of ​​the TiAl alloy powder is coated with the Nb transition layer;

[0052] Step 3, secondary low-energy ball milling: add the B4C powder weighed in step 1 to the ball milling jar containing the TiAl alloy powder with a Nb transition layer on the surface and the grinding balls obtained in step 2, with a ball-to-material ratio of 8:1, then evacuate the ball milling jar and introduce argon gas, then place it in a planetary ball mill, and perform secondary low-energy ball milling at a speed of 50 r / min for 5 hours to obtain a mixed powder and grinding balls with reinforcements uniformly dispersed on the surface of the TiAl alloy powder;

[0053] Step 4: Screening: The mixed powder and grinding balls obtained in step 3, in which the reinforcement is evenly dispersed on the surface of the TiAl alloy powder, are screened using a 200-mesh screen;

[0054] Step 5, sintering: the mixed powder in which the reinforcement after screening in step 4 is evenly dispersed on the surface of the TiAl alloy powder is loaded into a graphite mold with a diameter of 50 mm, and then the graphite mold is placed in a high-temperature sintering furnace. Thereafter, under vacuum and a sintering pressure of 45 MPa, the furnace temperature is raised to 850°C at a rate of 120°C / min and kept warm for 2 min, the furnace temperature is raised to 1250°C at a rate of 60°C / min and kept warm for 7 min, and the furnace temperature is lowered to 750°C at a rate of about 180°C / min, and cooled to room temperature with the furnace to obtain a TiAl-based composite material.

[0055] The results show that the TiAl alloy powder surface in the TiAl-based composite material prepared in this embodiment has Nb transition layer and B4C powder evenly distributed, the main structure is γ / α2 lamellar clusters and a small amount of equiaxed γ structure distributed between the lamellar clusters, and the lamellar clusters are small and uniform.

[0056] Example 4

[0057] This embodiment includes the following steps:

[0058] Step 1, weighing raw material powder: weighing 48.5g of spherical TiAl pre-alloyed powder with a particle size of 53μm~150μm, 1.25g of Nb powder with a particle size of 30μm~80μm, and 0.25g of B4C powder with a particle size of 10μm~40μm; the material of the TiAl pre-alloyed powder is Ti4822;

[0059] Step 2, initial low-energy ball milling: the TiAl pre-alloyed powder and Nb powder weighed in step 1 are loaded into a ball milling jar with a ball-to-material ratio of 7:1, and then the ball milling jar is evacuated and argon gas is introduced, and then placed in a planetary ball mill, and the initial low-energy ball milling is performed at a speed of 150 r / min for 12 hours, and a TiAl alloy powder with a Nb transition layer on the surface and a grinding ball are obtained in the ball milling jar; in the TiAl alloy powder with a Nb transition layer on the surface, 90% of the surface area of ​​the TiAl alloy powder is coated with the Nb transition layer;

[0060] Step 3, secondary low-energy ball milling: add the B4C powder weighed in step 1 to the ball mill jar containing the TiAl alloy powder with a Nb transition layer on the surface and the grinding balls obtained in step 2, with a ball-to-material ratio of 7:1, then evacuate the ball mill jar and introduce argon gas, then place it in a planetary ball mill, and perform secondary low-energy ball milling at a speed of 150 r / min for 3 hours to obtain a mixed powder and grinding balls with reinforcements uniformly dispersed on the surface of the TiAl alloy powder;

[0061] Step 4: Screening: The mixed powder and grinding balls obtained in step 3, in which the reinforcement is evenly dispersed on the surface of the TiAl alloy powder, are screened using a 100-mesh screen;

[0062] Step 5, sintering: the mixed powder in which the reinforcement after screening in step 4 is evenly dispersed on the surface of the TiAl alloy powder is loaded into a graphite mold with a diameter of 50 mm, and then the graphite mold is placed in a high-temperature sintering furnace. Thereafter, under vacuum and a sintering pressure of 40 MPa, the furnace temperature is raised to 800°C at a rate of 100°C / min and kept warm for 1 min, the furnace temperature is raised to 1300°C at a rate of 50°C / min and kept warm for 7 min, the furnace temperature is lowered to 800°C at a rate of about 200°C / min, and the furnace is cooled to room temperature to obtain a TiAl-based composite material.

[0063] Figure 1 The SEM image of the mixed powder prepared in Example 4 of the present invention in which the reinforcement is uniformly dispersed on the surface of the TiAl alloy powder and the distribution diagram of each element are shown. Figure 1 The left side is the SEM image of the mixed powder with the reinforcement evenly dispersed on the surface of the TiAl alloy powder. Figure 1 The upper left corner on the right is Figure 1 The enlarged image of the dotted box on the left. Figure 1 The rest of the figures on the right are the distribution diagrams of the elements in the dotted box. Figure 1 It can be seen that in the mixed powder, the reinforcement is evenly dispersed on the surface of the TiAl alloy powder, and the Nb transition layer and B4C powder are evenly distributed on the surface of the TiAl alloy powder.

[0064] Figure 2 This is a low-magnification microstructure image of the TiAl-based composite material prepared in this embodiment. Figure 3 This is a high-magnification microstructure diagram of the TiAl-based composite material prepared in this embodiment. Figure 2 and Figure 3 It can be seen that the main structure of the TiAl-based composite material prepared in this embodiment is γ / α2 lamellar clusters and a small amount of equiaxed γ structure distributed between the lamellar clusters, and the lamellar clusters are fine and uniform.

[0065] Figure 4The engineering stress-strain diagram of the TiAl-based composite material prepared in this example at 850℃ and 900℃ is shown in Figure 2. Figure 4 It can be seen that the tensile strength of the TiAl-based composite material prepared in this example can reach 510 MPa at 850°C, and the elongation after fracture is 15%~25%. The tensile strength at 900°C can reach 450 MPa, and the elongation after fracture is 25%~35%.

[0066] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.

Claims

1. A method for preparing a TiAl-based composite material synergistically reinforced with a Nb transition layer and B4C, characterized in that: The method comprises the following steps: Step 1, weighing raw material powders: weighing TiAl pre-alloyed powder, Nb powder and B4C powder; the mass ratio of the weighed spherical TiAl pre-alloyed powder, Nb powder and B4C powder is 46-48.5:1.25-3.75:0.25; the particle size of the TiAl pre-alloyed powder is 45μm-150μm, the particle size of the Nb powder is 30μm-80μm, and the particle size of the B4C powder is 10μm-40μm; Step 2, initial low-energy ball milling: the TiAl pre-alloyed powder, Nb powder and grinding balls weighed in step 1 are placed in a ball mill, and then the ball mill is evacuated and argon gas is introduced into the ball mill, and then the ball mill is placed in a planetary ball mill for initial low-energy ball milling, so as to obtain TiAl alloy powder and grinding balls with a Nb transition layer on the surface in the ball mill; Step 3, secondary low-energy ball milling: add the B4C powder weighed in step 1 to the ball milling jar containing the TiAl alloy powder with a Nb transition layer on the surface and the grinding balls obtained in step 2, then evacuate the ball milling jar and introduce argon gas, and then place it in a planetary ball mill for secondary low-energy ball milling to obtain a mixed powder and grinding balls with reinforcements uniformly dispersed on the surface of the TiAl alloy powder; Step 4: Screening: Screening the mixed powder and grinding balls obtained in step 3 in which the reinforcement is evenly dispersed on the surface of the TiAl alloy powder; Step 5, sintering: the mixed powder in which the reinforcement after screening in step 4 is evenly dispersed on the surface of the TiAl alloy powder is loaded into a graphite mold, and then the graphite mold is placed in a high-temperature sintering furnace, and then pressure sintering is performed under vacuum to obtain a TiAl-based composite material synergistically reinforced with a Nb transition layer and B4C; the pressure of the pressure sintering is 35MPa~45MPa, and the process of pressure sintering is: first heated to 800℃~900℃ at a heating rate of 100℃ / min~150℃ / min, and then kept warm for 1min~2min, and then heated to 1100℃~1300℃ at a heating rate of 40℃ / min~60℃ / min, and then kept warm for 7min~8min, and then cooled to 700℃~800℃ at a cooling rate of 150℃ / min~200℃ / min, and finally cooled to room temperature with the furnace.

2. The method for preparing a TiAl-based composite material synergistically reinforced by a Nb transition layer and B4C according to claim 1, characterized in that: The TiAl pre-alloyed powder in step 1 is spherical and made of Ti-47.7Al-7.8Nb, Ti-47Al-2W-0.5Si, Ti-45.5Al-4Nb or Ti4822, and the Nb powder is spherical or irregularly flaky.

3. The method for preparing a TiAl-based composite material synergistically reinforced by a Nb transition layer and B4C according to claim 1, characterized in that: The rotation speed of the initial low-energy ball milling in step 2 is 50 r / min~200 r / min, the time is 10h~15h, and the ball-to-material ratio is 5~8:

1.

4. The method for preparing a TiAl-based composite material synergistically reinforced by a Nb transition layer and B4C according to claim 1, characterized in that: In the TiAl alloy powder having a Nb transition layer on the surface described in step 2, 60% to 90% of the surface of the TiAl alloy powder is coated with the Nb transition layer.

5. The method for preparing a TiAl-based composite material synergistically reinforced by a Nb transition layer and B4C according to claim 1, characterized in that: The rotation speed of the secondary low-energy ball milling treatment in step 3 is 50r / min~200r / min, the time is 2h~5h, and the ball-to-material ratio is 5~8:

1.