Outer part for timepiece or jewelry comprising coating of saturated intrinsic color and method for manufacturing said outer part

Through the chemical vapor deposition technology of tantalum (Ta)-based metal nitride or tantalum-based oxynitride, a Ta3N5 or AB(O, N) type composition coating with a thickness of 300nm to 10μm is formed, which solves the red coating problem in the existing technology. The problem of layer non-durability and viewing angle dependence of color perception is achieved, achieving a stable and durable red coating effect.

CN118854232APending Publication Date: 2024-10-29THE SWATCH GRP RES & DEVELONMENT LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410305766.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-03-18
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the field of watchmaking or jewelry, it is difficult to obtain bright and saturated red coatings on an industrial scale with existing technologies, and the color perception of the coating depends on viewing angle and thickness, and it is not resistant to mechanical stress.

Method used

Tantalum (Ta)-based metal nitride or tantalum-based oxynitride is used as the coating material, with a thickness between 300nm and 10μm. It is nitrided through chemical vapor deposition technology at a temperature of 600°C to 1200°C to form a bright red color. Characteristic Ta3N5 or AB(O, N) type composition coating.

Benefits of technology

A red coating with unchanged color under different viewing angles and high durability is achieved, which is suitable for use on external parts of watches or jewelry to maintain the integrity of the base structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854232A_ABST
    Figure CN118854232A_ABST
Patent Text Reader

Abstract

The invention relates to an outer part (10) of a watch or jewelry, comprising a substrate (11) on the surface of which there is extended a coating (12) comprising a tantalum-based nitride or a tantalum-based nitrogen oxide, having a thickness of 300 nm to 10 [mu] m, and having an inherent saturation color. The invention also relates to a method for manufacturing an outer part (10) for a watch or jewelry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of watchmaking or jewelry, and more particularly to an external part of a watch or jewelry comprising an intrinsically colored coating, and a method for manufacturing said external part.

[0002] In this context, the term "external part" refers to any decorative article in the field of watchmaking or jewellery consisting for example of a case, dial, dial appliques, hands, bezel, crown, links etc. and intended to be visible to the user.

[0003] Preferably, the invention relates to an outer part of a watch or jewellery comprising a coating whose intrinsic colour is a red hue. Background Art

[0004] In the field of watchmaking or jewellery and, more generally, in the field of decorated objects, the deposition methods of painting, lacquering or enamelling are not always suitable.

[0005] Indeed, on the one hand, the layer of material applied to the surface of the object to be decorated is too thick to reveal any surface structures such as brushed, sun-brushed, sandblasted or laser-structured surfaces, etc., and on the other hand, the lifetime of the layer and its color are not always satisfactory.

[0006] Therefore, thin layer vacuum deposition techniques such as physical vapor deposition (PVD), chemical vapor deposition (CVD) and atomic layer deposition (ALD) are preferred. In fact, these thin layer vacuum deposition techniques are able to deposit thin durable layers, which are generally suitable for coating small, easily rubbed parts and include, for example, fine surface structures.

[0007] However, although these deposition techniques allow coatings of a wide variety of intrinsic colors to be obtained, implementation of these methods does not allow certain specific intrinsic colors to be obtained on an industrial scale, such as red shades, and in particular bright and vivid reds.

[0008] It is also known to deposit stacks of thin layers to create an interference optical system for producing a given color. However, the perception of the color is likely to depend on the viewing angle. In addition, stacking of thin layers has significant manufacturing limitations, as the color produced is highly dependent on the thickness of the thin layers.

[0009] It is therefore necessary to obtain an external part having a bright and saturated color (for example red), which is obtained by one or more thin layers to maintain the structure of the substrate, whose appearance does not change with the user's viewing angle and which is suitable for withstanding mechanical stresses without degradation. Summary of the invention

[0010] To this end, the present invention relates to an outer part of a watch or jewelry, which includes a substrate having a coating extending on the surface thereof, the coating containing tantalum (Ta)-based metal nitride or tantalum-based oxynitride having a thickness of 300 nm to 10 μm to have a predetermined color.

[0011] In certain embodiments, the present invention may also include one or more of the following features alone or in any technically possible combination.

[0012] In a specific embodiment, the thickness of the coating is in the range of 1 μm to 3 μm, preferably 2 μm.

[0013] In certain embodiments, the red coating is composed of a stoichiometry substantially close to or equal to Ta 3 N 5 It is made of tantalum nitride Ta, which has a bright red color.

[0014] In a specific embodiment, the coating is produced with the addition of oxygen in the range of 0-5 atomic %.

[0015] In a particular embodiment, the coating has a red color characterized by coordinates a* and b* in the CieLAB color space measured in transmission mode of standard illuminant D65 being greater than 20, preferably greater than 50, even more preferably characterized by coordinates L*=[30; 50], a*=[50; 70] and b*=[60; 80], in particular L*=42, a*=58 and b*=72, wherein the observation angle / observer is at 10° and the measuring geometry is d:0°.

[0016] In a specific embodiment, the coating forms an AB (O, N) type composition, wherein B is tantalum Ta and A is a metal element.

[0017] In a specific embodiment, the metal element A is preferably selected from Ba, Ca, Nd, La, Sr, Eu and Yb. Then the coating comprises a metal element that is substantially close to or equal to BaTaO 2 N、CaTaO 2 N、NdTaO 2 N、LaTaO 2 N、SrTaO 2 N、EuTaO 2 N or Yb 2 Ta 2 O 5 N 2 The composition / composition of.

[0018] According to another object, the invention relates to a method for manufacturing a watch or jewellery external part, such as a watch or jewellery external part as described above, comprising the following steps:

[0019] - depositing a thin layer of a tantalum (Ta) based metal oxide on a substrate, said thin layer having a thickness in the range of 300 nm to 10 μm;

[0020] - Nitriding the thin layer to form a coating comprising at least one metal nitride or oxynitride.

[0021] In certain embodiments, the step of nitriding the deposited layer is not completed to produce an oxynitride of the coating material.

[0022] In a particular embodiment, during the deposition step, the deposited thin layer is composed of TaO x and a nitriding step is performed so that the coating is composed of a stoichiometric amount substantially close to or equal to orthorhombic Ta 3 N 5 The coating is made of tantalum nitride, which gives it a red color.

[0023] In a particular embodiment, during the deposition step, the deposited thin layer is composed of TaO x and is combined / bonded with at least one metal element selected from Ba, Ca, Nd, La, Sr, Eu or Yb.

[0024] In a specific embodiment, the nitridation step is performed in a suitable atmosphere at a temperature in the range of 600° C. to 1200° C. for a time of 10 to 60 hours, preferably at a temperature in the range of 700° C. to 1000° C. for a time of 20 to 50 hours.

[0025] In a specific embodiment, the nitridation step is performed at a temperature of 900° C. for 40 hours in a suitable atmosphere. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Other characteristics and advantages of the invention will become apparent from the following detailed description, given as a non-limiting example.

[0027] Figure 1 A cross-sectional view of an outer component according to a preferred embodiment of the present invention is schematically shown.

[0028] Note that for clarity, the drawings are not necessarily drawn to scale. DETAILED DESCRIPTION

[0029] The present invention relates to an outer part 10 of a watch or jewellery, such as Figure 1 As shown, the exterior component comprises a substrate 11 having extended on its visible surface a coating 12 comprising a metal nitride or metal oxynitride. The coating 12 has a predetermined color depending on the metal constituting the coating 12, as described later herein.

[0030] The coating 12 is thick enough so that its color is saturated, and thin enough so as not to smear any structure of the surface of the substrate 11, nor to affect the consistency of the external component 10. To this end, the thickness of the coating 12 is in the range of 300 nm to 10 μm, preferably in the range of 1 μm to 3 μm. Even more preferably, the thickness of the coating 12 is 2 μm.

[0031] The material constituting the substrate 11 is advantageously chosen so as to be able to withstand the conditions of deposition of the metal oxide layer and of nitridation of said layer, as described in more detail below.

[0032] For example, the substrate 11 may be made of a ceramic material such as zirconia or sapphire, or of a metal alloy such as stainless steel, or may also be made of silicon.

[0033] Advantageously, the outer part 10 may comprise a bonding layer 13 made of titanium, chromium or another suitable metal known to a person skilled in the art, between the substrate 11 and the coating 12. The thickness of the bonding layer 13 is in the range of 20 nm to 500 nm, preferably 100 nm.

[0034] In a preferred exemplary embodiment of the present invention, coating 12 is made of tantalum nitride, which is chemically and structurally substantially close to or equal to orthorhombic Ta. 3 N 5 This metal nitride has a bright red, that is to say saturated, color, which is defined by the following coordinates in the CieLAB color space measured in reflection mode with standard illuminant D65, with the observer at 10°, measured with specular reflection included (SCI, measuring geometry di: 8°) and with specular reflection excluded (SCE, measuring geometry de: 8°).

[0035] Table 1

[0036] Base material SCI / SCE L* a* b* sapphire SCI 63 2 0 sapphire SCE 21 9 0 White zircon SCI 58 14 -1 White zircon SCE 24 38 17

[0037] When the material constituting the substrate 11 is sapphire, the coating 12 can be directly observed, i.e., the coating 12 is located between the observer and the substrate 11, or indirectly observed, i.e., the substrate 11 is arranged between the observer and the coating 12, so that the coating 12 can be observed through the substrate 11. It should be noted that in the application case of the present invention, in which the coating 12 is indirectly observed, the external component 10 does not include the bonding layer 13, so that it does not reduce the color perception of the coating 12.

[0038] Table 1 above shows the color coordinates of coating 12 when viewed directly, and Table 2 below shows the color coordinates of coating 12 when viewed indirectly.

[0039] Table 2

[0040] Base material SCI / SCE L* a* b* sapphire SCI 49 11 -3 sapphire SCE 15 34 21

[0041] The bright red color of the coating 12 deposited on the sapphire substrate 11 can be characterized by the values ​​of L*=42, a*=58 and b*=72, which are obtained during the colorimetric measurement in transmission mode with the standard illuminant D65, with the observer at 10° and the measuring geometry d: 0°. Preferably, it is desirable to obtain a red color with coordinates a* and b* greater than 20, preferably greater than 50. More particularly, it is desirable to obtain a red color with coordinates L*=[30;50], a*=[50;70] and b*=[60;80].

[0042] In other exemplary embodiments of the present invention, the coating 12 may be formed of an AB (O, N) type composition having A metal element and B tantalum Ta. This feature allows selection of metal oxynitrides of different colors, so that the coating 12 may have a variety of different colors.

[0043] In various examples, the metal element A is selected from Ba, Ca, Nd, La, Sr, Eu, and Yb. Therefore, the coating 12 can be formed to have a color substantially close to or equal to BaTaO having a dark red or brown color. 2 N, CaTaO with green or yellow color 2 N, NdTaO with red or brown 2 N, SrTaO with orange color 2 N. LaTaO with red or orange 2 N. Brown EuTaO 2 N or Yb with green color 2 Ta 2 O 5 N 2 composition.

[0044] The invention also relates to a method for manufacturing an external part 10 for a watch or jewellery, for example as described above.

[0045] The method comprises a deposition step of depositing a thin layer comprising metal oxide on a substrate 11 such that the thickness of the thin layer is in the range of 300 nanometers to 10 micrometers, followed by a nitridation step of nitriding the thin layer to form a metal nitride or metal oxynitride coating 12 .

[0046] Preferably, the deposited thin layer consists of TaO x In particular, in this preferred example, by using a tantalum Ta target and O 2 The reaction gases composed are used to carry out the deposition step by means of a PVD deposition method. In particular, the thin layer can be deposited by cathode sputtering, vapor phase electron beam evaporation, arc or pulsed laser beam ablation.

[0047] At the end of the deposition step, the deposited thin layer thus consists of TaO x and a nitriding step is performed so that the coating 12 is made of red Ta 3 N 5 Made.

[0048] In particular, the nitriding step consists in exposing the thin layer to a suitable atmosphere, for example an atmosphere resulting from the thermal decomposition of ammonia, in the shell of a furnace heated to several hundred degrees Celsius for several hours. More specifically, the nitriding step is carried out at a temperature ranging from 600° C. to 1200° C. for 10 hours to 60 hours, preferably at a temperature ranging from 700° C. to 1000° C. for 20 hours to 50 hours. In the most preferred example, the nitriding step is carried out at a temperature of 900° C. for 40 hours. By way of example, the flow rate of the decomposed ammonia in the shell of the furnace during the nitriding step is 200 ml / min.

[0049] In a variant of the method, the nitridation of the deposited layer is incomplete in order to produce an oxynitride of the coating material 12 .

[0050] In the thin layer deposition step, it is also possible to deposit thin layers from several different metal sources or alloy metal sources so that at the end of the nitridation step, the coating 12 comprises an AB (O, N) type composition / composition / compound with A metal element and B tantalum Ta.

[0051] Before the step of depositing the coating 12, the manufacturing method may advantageously include a step of depositing a bonding layer 13 as described above, for example by CVD, ALD or PVD deposition. Advantageously, the bonding layer 13 deposition step and the coating 12 deposition step can be performed successively / continuously in the same deposition chamber, the pressure in the chamber being kept constant between the two depositions. These deposition steps require at least two different material sources, one of which is used to form the bonding layer 13 on the substrate 11 and the other is used to form the coating 12 on the bonding layer 13.

[0052] More generally, it should be noted that the above-described embodiments and examples have been described by way of non-limiting examples, and that other variations are possible.

[0053] In particular, before or after the nitridation step, a step of selectively structuring the thin layer over its entire thickness to form a specific decoration can be carried out. This step can be carried out using photolithography, laser ablation or the like.

[0054] For the same purpose, it is also possible to carry out a preliminary step of structuring the surface of the substrate 11 .

Claims

1. An outer part (10) of a watch or jewellery, It is characterized in that The external component comprises a substrate (11) on the surface of which a coating (12) extends, the coating comprising tantalum-based nitride or tantalum-based oxynitride and having a thickness in the range of 300 nm to 10 μm so as to have a predetermined color.

2. The outer part (10) according to claim 1, in, The thickness of the coating (12) is in the range of 1 μm to 3 μm.

3. The outer part (10) according to claim 2, in, The thickness of the coating (12) is equal to 2 μm.

4. The outer part (10) according to any one of claims 1 to 3, in, The coating (12) is made of tantalum nitride, which is substantially close to or equal to the stoichiometry of orthorhombic Ta. 3 N 5 .

5. The outer part (10) according to any one of claims 1 to 4, in, The coating is produced by adding oxygen in the range of 0-5 atomic %.

6. The outer part (10) according to any one of claims 1 to 5, in, The coating (12) has a red color characterized by its coordinates a* and b* in the CieLAB color space measured in transmission mode of standard illuminant D65, greater than 20, preferably greater than 50, with the observer at 10° and the measuring geometry d:0°.

7. The outer part (10) according to claim 6, in, The coating (12) has a red color characterized by its coordinates L*=[30;50], a*=[50;70] and b*=[60;80] in the CieLAB color space measured in transmission mode of standard illuminant D65, with the observer at 10° and the measuring geometry being d:0°.

8. The outer part (10) according to claim 7, in, The coating (12) has a red color characterized by its coordinates L*=42, a*=58 and b*=72 in the CieLAB color space measured in transmission mode of standard illuminant D65, with the observer at 10° and the measuring geometry d:0°.

9. The outer part (10) according to any one of claims 1 to 5, in, The coating layer (12) forms an AB (O, N) type composition, wherein B is tantalum and A is a metal element selected from Ba, Ca, Nd, La, Sr, Eu and Yb.

10. The outer part (10) according to claim 9, in, The coating (12) is made of BaTaO 2 N、CaTaO 2 N、NdTaO 2 N、LaTaO 2 N、SrTaO 2 N、EuTaO 2 N or Yb 2 Ta 2 O 5 N 2 Made.

11. A method for manufacturing an exterior part (10) for a watch or jewellery, the method The following steps are involved: - a deposition step: depositing a thin layer of tantalum-based metal oxide on a substrate (11), the thickness of the thin layer being in the range of 300 nm to 10 μm; - Nitriding step: nitriding the thin layer to form a coating (12) comprising at least one metal nitride or metal oxynitride.

12. The method according to claim 11, in, During the deposition step, the deposited thin layer consists of TaO x The nitriding step is performed so that the coating (12) is made of tantalum nitride, wherein the stoichiometry of the tantalum nitride is substantially close to or equal to that of orthorhombic Ta. 3 N 5 .

13. The method according to claim 11, in, During the deposition step, the deposited thin layer consists of TaO x The deposited thin layer is combined with at least one metal element selected from Ba, Sr, Ca, Nd, La, Eu or Yb.

14. The method according to any one of claims 11 to 13, in, The nitridation step is performed at a temperature ranging from 600° C. to 1200° C. for 10 hours to 60 hours. Preferably, the nitridation step is performed at a temperature ranging from 700° C. to 1000° C. for 20 hours to 50 hours.

15. The method according to claim 14, in, The nitridation step was performed at a temperature of 900° C. for 40 hours.