A method for preparing lignin-cellulose nanofibers through coupled steam explosion pretreatment
By combining steam explosion pretreatment and high-pressure homogenization to prepare LCNF, the problems of high energy consumption and low efficiency in the existing technology were solved, and high-performance and environmentally friendly LCNF materials were obtained.
Patent Information
- Application Number
- CN202411016749.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Existing technologies for preparing nanocellulose, especially lignin-containing cellulose nanofibers (LCNF), suffer from high energy consumption, incomplete lignin removal, and low efficiency, which affect material performance and environmental friendliness.
A coupled steam explosion pretreatment technique combined with high-pressure homogenization was adopted. The steam explosion pretreatment destroyed the fiber cell wall, reducing the use of chemicals. Subsequently, high-pressure homogenization was used to prepare LCNF, which reduced energy consumption and improved the degree of profibrillation.
It effectively reduces the energy consumption in preparing LCNF, improves the degree of fiber fibrillation, and obtains LCNF with smaller particle size and larger specific surface area. It has excellent mechanical properties, thermal stability, UV shielding and antibacterial properties, and is environmentally friendly and pollution-free.
Smart Images

Figure CN118854705B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of nanocellulose preparation technology, and in particular to a method for preparing lignin-containing cellulose nanofibers by coupled steam explosion pretreatment. Background Technology
[0002] Crop straw and forestry branches, as byproducts of agricultural and forestry production, have low utilization rates and have not been rationally developed. Therefore, the rational utilization of crop straw and forestry branches is of great significance for promoting ecological balance, improving resource utilization efficiency, and driving the circular economy.
[0003] Crop straw is typically burned, but this causes environmental pollution. Current research suggests that returning straw to the field can increase soil organic matter and improve soil structure; it can also be used as animal feed or fermented to produce biofuel. The energy utilization of straw provides a new energy solution for rural areas. Forestry branches also have multiple uses, from traditional timber processing to modern biomass energy production, all representing effective utilization of these resources. However, these utilization methods face challenges in implementation, including technological, economic, and policy issues, resulting in low utilization rates.
[0004] Cellulose nanofibers (CNFs) have wide applications in constructing advanced materials and have received considerable attention from researchers in recent years. The main methods for preparing cellulose nanofibers include: using a high-pressure homogenizer, where raw materials are passed through a tiny high-pressure homogenizing chamber under high pressure. During this process, the sudden pressure change causes the material to undergo shearing, compression, and expansion, resulting in fibrillation in the S2 layer of the fiber cells, thus reducing particle size and increasing specific surface area. Ultrasonic methods are also used, where high-frequency vibrations, assisted by an energy field, are employed to prepare cellulose nanofibers; these are all physical methods. Chemical methods for preparing cellulose nanofibers include the TEMPO oxidation method, which selectively oxidizes fibers and then dissociates them to obtain cellulose nanofibers. Biological methods are often used to produce bacterial cellulose, which is essentially an insoluble polysaccharide produced and metabolized by microorganisms.
[0005] Nanocellulose that retains lignin before preparation is called lignin-containing cellulose nanofibril (LCNF). Recent studies have shown that LCNF exhibits some properties superior to CNF. For example, Yao Lu prepared nanopaper using LCNF with varying lignin contents, and its tensile strength and Young's modulus were significantly better than nanopaper prepared with CNF. This demonstrates that an appropriate amount of lignin is beneficial for stress transmission in materials, improving their mechanical properties. Furthermore, lignin can provide CNF with UV shielding, antibacterial, and water-resistant properties. Xiao et al. utilized this principle to prepare films with UV shielding and higher thermal stability, and lignin, acting as a binder, provided the films with superior mechanical properties and a higher water contact angle.
[0006] The preparation method of LCNF is the same as that of CNF, although the lignin removal ratio is lower. However, if no lignin is removed at all, it will lead to excessively high energy consumption in subsequent homogenization or ultrasonic mechanical operations. This patent utilizes coupled steam explosion pretreatment technology to destroy the fiber cell wall, eliminating the need for large amounts of chemicals to remove the lignin barrier. The chemicals used in this technology are water vapor and air, which are then combined with high-pressure homogenization, making this method efficient and environmentally friendly. Summary of the Invention
[0007] To address the aforementioned problems, this invention provides a method for preparing lignin-cellulose nanofibers through steam explosion pretreatment. This method effectively improves preparation efficiency, reduces energy consumption, and yields LCNFs with excellent performance by coupling steam explosion pretreatment with high-pressure homogenization.
[0008] A method for preparing lignin-cellulose nanofibers by steam explosion pretreatment includes the following steps:
[0009] S1 Pre-soaking: Cut the raw material into small pieces of 1-5cm, soak them in NaOH or aqueous solution, use 0-8% alkali, and soak for 2-24 hours. The solution must just submerge the surface of the raw material. After pre-soaking, it is ready for use. Preferably, the raw material is agricultural crop straw, forestry branches and other waste materials.
[0010] S2 Steam Explosion Pretreatment: The tobacco stalk fragments soaked in S1 are placed into the steam explosion storage tank. The pressure and holding time are set, and the pressure relief program is started. The pressure is released for 0.005 to 3.0 seconds to obtain the steam-exploded material A1. The steam explosion in S2 is a coupled steam explosion. The steam pressure is set to 0.4-0.8 MPa, and then air is used to pressurize the total pressure to 1.0-1.8 MPa. The holding time is 2-15 minutes.
[0011] Preferably, the steam explosion technology is instantaneous ejection steam explosion technology (ICSE), and the pressure release time is less than 0.01s.
[0012] S3 Washing: A1 is washed to remove impurities, and the concentration of material A1 is adjusted to 0.5%wt to obtain material A2;
[0013] S4 High-Pressure Homogenization: Material A2 is processed using a high-pressure homogenizer at a pressure of 700 bar until the fiber suspension of material A2 exhibits a gel-like texture. The degree of fibrillation is controlled by measuring the viscosity of the suspension, resulting in LCNF material A3. The number of homogenization cycles in this step can be adjusted based on the viscometer measurement results. The minimum number of homogenization cycles can be reduced to 5 to achieve a qualified LCNF product.
[0014] S5 Concentration: Material A3 is concentrated using a vacuum rotary evaporator to obtain a product of the target concentration.
[0015] Beneficial effects
[0016] Compared with existing technologies, the method of this invention has the following advantages: This invention effectively reduces the number of high-pressure homogenization cycles through steam explosion pretreatment, saving energy consumption. Direct homogenization of crop straw is impossible; using 0.8 MPa saturated steam explosion pretreatment requires 20 homogenization cycles to prepare LCNF that meets the requirements. However, using coupled steam explosion treatment with the same amount of steam, the number of homogenization cycles can be reduced to 5, reducing the energy consumption for LCNF preparation by 75%. Even using 0.6 MPa steam, the number of homogenization cycles can be reduced to 6, fully demonstrating the energy-saving effect of coupled steam pretreatment.
[0017] This invention improves the fibrillation degree of fibers by coupling steam pretreatment, resulting in LCNF with smaller particle size and larger specific surface area.
[0018] The LCNF prepared by this invention has excellent mechanical properties and thermal stability, as well as good UV shielding and antibacterial properties.
[0019] This invention uses very few chemicals, and even pre-soaking can be done without the use of alkaline solution, resulting in no pollution or even pollution, making it environmentally friendly, economical, and efficient. Attached Figure Description
[0020] Figure 1 SEM (ac) and AFM (df) microstructure images of LCNF obtained in Example 9;
[0021] Figure 2 Water contact angle (a) and soybean oil contact angle (b) of LCNF obtained in Examples 1-9;
[0022] Figure 3The zeta potential of LCNF obtained in Examples 1-9
[0023] Figure 4 The Pickering emulsion stability of LCNF obtained in Example 9 is shown in the left figure after 1 day of natural settling and the right figure after 30 days of natural settling. Detailed Implementation
[0024] This invention provides a technical solution: a method for preparing lignin-cellulose nanofibers through steam explosion pretreatment. The method involves soaking chopped straw or branch fragments in water or NaOH solutions with varying alkali concentrations for 2-24 hours, then placing them into the storage tank of an ICSE (Integrated Chloride Separation) device. Saturated steam at a pressure of 0.4-0.8 MPa is injected, and simultaneously, air is used to pressurize the device to a set total pressure and maintain this pressure for a certain period. Then, a pressure relief procedure is initiated, instantly releasing the steam / air from the device. The steam-exploded straw material A1 is then sprayed under pressure into a spray pan to separate the material from residual steam. Material A1 is conveyed from the bottom of the spray pan into a washing device via a belt, where a large amount of clean water is injected for thorough washing. Then, it is concentrated using an inclined screw press. The concentrated material is sent to a thickening tank, where clean water is injected to achieve a concentration of approximately 0.5% required by the homogenizer. Then, homogenization is performed using a homogenizer at a pressure of 700 bar until the fiber suspension exhibits a gel-like texture. During the process, the degree of fibrillation of each sample was controlled by measuring the viscosity of LCNF. When the viscosity reached the set value, the homogenization endpoint was determined, and qualified LCNF material A2 was obtained.
[0025] The present invention will be further described in detail below with reference to implementation examples, but the implementation of the present invention is not limited thereto.
[0026] Example 1
[0027] First, the tobacco stalks are chopped into 1-5cm pieces using a shredder, completing the material preparation. Then, the processed material is conveyed to a pre-soaking tank via a belt conveyor. NaOH (5% of the raw material's weight) and water are added to the pre-soaking tank, and the mixture is stirred until the material is completely submerged in the solution. After soaking for 24 hours, the liquid has fully penetrated the cell walls. Then, under the action of an inclined screw conveyor, the material is discharged from the top. It is then conveyed to a steam explosion tank via a horizontal screw conveyor. Saturated steam at a pressure of 0.8MPa is introduced into the explosion tank, and after maintaining the pressure for 15 minutes, the pressure is released through the spray nozzle. The steam-exploded straw material A1 is sprayed under pressure into a spray pan to separate the material from the residual steam. Material A1 is conveyed from the bottom of the spray pan to a washing device via a belt conveyor, where a large amount of clean water is injected for thorough washing. Then, it is concentrated using an inclined screw press. The concentrated material is sent to a thickening tank, where clean water is injected to achieve a concentration of approximately 0.5% required by the homogenizer. Then, homogenization was performed using a homogenizer at a pressure of 700 bar until the fiber suspension developed a gel-like texture. During this process, the degree of fibrillation of each sample was controlled by measuring the viscosity of the LCNF. The homogenization endpoint was reached when the viscosity reached that of commercial CNF, yielding qualified LCNF material A2. This embodiment requires 20 homogenization cycles to reach the endpoint.
[0028] The AFM and SEM images of LCNF obtained in Example 1 are shown in the appendix. Figure 1 (a) and (d) No fibrillation of the fibers was found.
[0029] Example 2
[0030] First, the tobacco stalks are chopped into 1-5cm pieces using a shredder, completing the material preparation. Then, the processed material is conveyed to a pre-soaking tank via a belt conveyor. NaOH (5% of the raw material's weight) and water are added to the pre-soaking tank, and the mixture is stirred until the material is completely submerged in the solution. After soaking for 24 hours, the liquid has fully penetrated the cell walls. Then, the material is discharged from the top by an inclined screw conveyor. It is then conveyed to a steam explosion tank using a horizontal screw conveyor. Saturated steam at 0.4MPa is introduced into the explosion tank, followed by air to reach a total pressure of 1.0MPa. This pressure is maintained for 15 minutes, then released through a spray nozzle. The steam-exploded straw material A1 is sprayed under pressure into a spray pan to separate the material from the residual steam. Material A1 is conveyed from the bottom of the spray pan to a washing device via a belt conveyor, where a large amount of clean water is injected for thorough washing. Then, it is concentrated using an inclined screw press. The concentrated material is sent to a thickening tank, where clean water is injected to achieve a concentration of approximately 0.5% required by the homogenizer. Then, homogenization was performed using a homogenizer at a pressure of 700 bar until the fiber suspension developed a gel-like texture. During this process, the degree of fibrillation of each sample was controlled by measuring the viscosity of the LCNF. The homogenization endpoint was reached when the viscosity reached that of commercial CNF, yielding qualified LCNF material A2. This embodiment requires 16 homogenization cycles to reach the endpoint.
[0031] Example 3
[0032] First, the wheat straw raw material is chopped into 1-5cm pieces using a shredder, completing the material preparation. Then, the processed raw material is conveyed into a pre-soaking tank via a belt conveyor. Sufficient water is added to the pre-soaking tank, and the mixture is stirred evenly to ensure the raw material is completely immersed in the solution. After soaking for 2 hours, the liquid has fully penetrated the cell walls. Then, under the action of an inclined screw conveyor, the raw material is discharged from the top. Next, a horizontal screw conveyor transports it into a steam explosion tank. Saturated steam at a pressure of 0.4MPa is introduced into the explosion tank, followed by air to bring the total pressure to 1.4MPa. After maintaining this pressure for 10 minutes, the pressure is released through the spray nozzle, and the steam-exploded straw material A1 is sprayed under pressure into a spray pan to separate the material from the residual steam. Material A1 is conveyed from the bottom of the spray pan into a washing device via a belt conveyor, where a large amount of water is injected for thorough washing. Then, it is concentrated using an inclined screw press. The concentrated material is sent to a thickening tank, where water is injected to achieve a concentration of approximately 0.5% required by the homogenizer. Then, homogenization was performed using a homogenizer at a pressure of 700 bar until the fiber suspension developed a gel-like texture. During this process, the degree of fibrillation of each sample was controlled by measuring the viscosity of the LCNF. The homogenization endpoint was reached when the viscosity reached the level of commercial CNF, yielding qualified LCNF material A2. This embodiment requires 11 homogenization cycles to reach the endpoint.
[0033] Example 4
[0034] First, the forestry branches and timber are shredded into 1-5cm pieces using a crusher to prepare the raw materials. Then, the processed materials are conveyed to a pre-soaking tank via a belt conveyor. NaOH (8% of the raw material's weight) and water are added to the pre-soaking tank, and the mixture is stirred until the raw materials are completely submerged in the solution. After soaking for 24 hours, the liquid has fully penetrated the cell walls. The raw materials are then discharged from the top by an inclined screw conveyor. A horizontal screw conveyor then transports the material into a steam explosion tank. Saturated steam at 0.6MPa is introduced into the explosion tank, followed by air to reach a total pressure of 1.2MPa. This pressure is maintained for 8 minutes before being released through a spray nozzle. The steam-exploded straw material A1 is then sprayed under pressure into a spray pan to separate the material from the residual steam. Material A1 is conveyed from the bottom of the spray pan to a washing device via a belt conveyor, where a large amount of clean water is injected for thorough washing. Then, it is concentrated using an inclined screw press. The concentrated material is sent to a thickening tank, where clean water is injected to achieve a concentration of approximately 0.5% required by the homogenizer. Then, homogenization was performed using a homogenizer at a pressure of 700 bar until the fiber suspension developed a gel-like texture. During this process, the degree of fibrillation of each sample was controlled by measuring the viscosity of the LCNF. The homogenization endpoint was reached when the viscosity reached the level of commercial CNF, yielding qualified LCNF material A2. This embodiment required 13 homogenization cycles to reach the endpoint.
[0035] Example 5
[0036] First, the tobacco stalks are chopped into 1-5cm pieces using a shredder, completing the material preparation. Then, the processed material is conveyed to a pre-soaking tank via a belt conveyor. NaOH (5% of the raw material's weight) and water are added to the pre-soaking tank, and the mixture is stirred until the material is completely submerged in the solution. After soaking for 12 hours, the liquid has fully penetrated the cell walls. Then, under the action of an inclined screw conveyor, the material is discharged from the top. It is then conveyed to a steam explosion tank via a horizontal screw conveyor. Saturated steam at a pressure of 0.6MPa is introduced into the explosion tank, followed by air to bring the total pressure to 1.4MPa. This pressure is maintained for 5 minutes, then released through a spray nozzle. The steam-exploded straw material A1 is sprayed under pressure into a spray pan to separate the material from the residual steam. Material A1 is conveyed from the bottom of the spray pan to a washing device via a belt conveyor, where a large amount of clean water is injected for thorough washing. Then, it is concentrated using an inclined screw press. The concentrated material is sent to a thickening tank, where clean water is injected to achieve a concentration of approximately 0.5% required by the homogenizer. Then, homogenization was performed using a homogenizer at a pressure of 700 bar until the fiber suspension developed a gel-like texture. During this process, the degree of fibrillation of each sample was controlled by measuring the viscosity of the LCNF. The homogenization endpoint was reached when the viscosity reached the level of commercial CNF, yielding qualified LCNF material A2. In this embodiment, 10 homogenization cycles were required to reach the endpoint.
[0037] The AFM and SEM images of LCNF obtained in Example 5 are shown in the appendix. Figure 1 (b) and (e) indicate that the degree of fibrillation of the fiber is relatively low.
[0038] Example 6
[0039] First, the cotton stalks are chopped into 1-5cm pieces using a shredder to prepare the raw material. Then, the processed material is conveyed to a pre-soaking tank via a belt conveyor. In the pre-soaking tank, 2.5% NaOH (based on the amount of raw material) and water are added and stirred until the material is completely submerged in the solution. After soaking for 24 hours, the liquid has fully penetrated the cell walls. Then, the material is discharged from the top by an inclined screw conveyor. Next, a horizontal screw conveyor transports the material into a steam explosion tank. Saturated steam at 0.6MPa is introduced into the explosion tank, followed by air to reach a total pressure of 1.4MPa. This pressure is maintained for 5 minutes, then released through a spray nozzle. The steam-exploded straw material A1 is sprayed under pressure into a spray pan to separate the material from the residual steam. Material A1 is conveyed from the bottom of the spray pan to a washing device via a belt conveyor, where a large amount of clean water is injected for thorough washing. Then, it is concentrated using an inclined screw press. The concentrated material is sent to a thickening tank, where clean water is injected to achieve a concentration of approximately 0.5% required by the homogenizer. Then, homogenization was performed using a homogenizer at a pressure of 700 bar until the fiber suspension developed a gel-like texture. During this process, the degree of fibrillation of each sample was controlled by measuring the viscosity of the LCNF. The homogenization endpoint was reached when the viscosity reached the level of commercial CNF, yielding qualified LCNF material A2. This embodiment requires six homogenization cycles to reach the endpoint.
[0040] Example 7
[0041] First, the tobacco stalks are chopped into 1-5cm pieces using a shredder, completing the preparation. Then, the processed stalks are conveyed to a pre-soaking tank via a belt conveyor. NaOH (5% of the stalk weight) and water are added to the pre-soaking tank, and the mixture is stirred until the stalks are completely submerged in the solution. After soaking for 24 hours, the liquid has fully penetrated the cell walls. The stalks are then discharged from the top by an inclined screw conveyor. A horizontal screw conveyor then transports the stalks into a steam explosion tank. Saturated steam at 0.8MPa is introduced into the explosion tank, followed by air to reach a total pressure of 1.4MPa. This pressure is maintained for 4 minutes before being released through a spray nozzle. The steam-exploded straw material A1 is then sprayed under pressure into a spray pan to separate the material from the residual steam. Material A1 is conveyed from the bottom of the spray pan to a washing device via a belt conveyor, where a large amount of clean water is injected for thorough washing. Then, it is concentrated using an inclined screw press. The concentrated material is then sent to a thickening tank, where clean water is injected to achieve a concentration of approximately 0.5% required by the homogenizer. Then, homogenization was performed using a homogenizer at a pressure of 700 bar until the fiber suspension developed a gel-like texture. During this process, the degree of fibrillation of each sample was controlled by measuring the viscosity of the LCNF. The homogenization endpoint was reached when the viscosity reached the level of commercial CNF, yielding qualified LCNF material A2. In this embodiment, 10 homogenization cycles were required to reach the endpoint.
[0042] Example 8
[0043] First, the tobacco stalks are chopped into 1-5cm pieces using a shredder, completing the material preparation. Then, the processed material is conveyed to a pre-soaking tank via a belt conveyor. In the pre-soaking tank, 2.5% NaOH (based on the amount of material) and water are added, and the mixture is stirred until the material is completely submerged in the solution. After soaking for 24 hours, the liquid has fully penetrated the cell walls. Then, under the action of an inclined screw conveyor, the material is discharged from the top. Next, a horizontal screw conveyor transports the material into a steam explosion tank. Saturated steam at a pressure of 0.8MPa is introduced into the explosion tank, followed by air to bring the total pressure to 1.6MPa. After maintaining this pressure for 3 minutes, the pressure is released through a spray nozzle, and the steam-exploded straw material A1 is sprayed under pressure into a spray pan to separate the material from the residual steam. Material A1 is conveyed from the bottom of the spray pan to a washing device via a belt conveyor, where a large amount of clean water is injected for thorough washing. Then, it is concentrated using an inclined screw press. The concentrated material is sent to a thickening tank, where clean water is injected to bring the concentration to approximately 0.5% required by the homogenizer. Then, homogenization was performed using a homogenizer at a pressure of 700 bar until the fiber suspension developed a gel-like texture. During this process, the degree of fibrillation of each sample was controlled by measuring the viscosity of the LCNF. The homogenization endpoint was reached when the viscosity reached the level of commercial CNF, yielding qualified LCNF material A2. This embodiment requires six homogenization cycles to reach the endpoint.
[0044] Example 9
[0045] First, the tobacco stalks are chopped into 1-5cm pieces using a shredder, completing the material preparation. Then, the processed material is conveyed to a pre-soaking tank via a belt conveyor. Water is added to the pre-soaking tank and stirred thoroughly, ensuring the material is completely immersed in the solution for 24 hours, allowing the liquid to fully penetrate the cell walls. The material is then discharged from the top by an inclined screw conveyor. A horizontal screw conveyor then transports the material into a steam explosion tank. Saturated steam at 0.8MPa is introduced into the explosion tank, followed by air to reach a total pressure of 1.8MPa. This pressure is maintained for 2 minutes before being released through a spray nozzle. The steam-exploded straw material A1 is then sprayed under pressure into a spray pan to separate the material from the residual steam. Material A1 is conveyed from the bottom of the spray pan to a washing device via a belt conveyor, where a large amount of water is injected for thorough washing. Then, it is concentrated using an inclined screw press. The concentrated material is sent to a thickening tank, where water is injected to achieve a concentration of approximately 0.5% required by the homogenizer. Then, homogenization was performed using a homogenizer at a pressure of 700 bar until the fiber suspension developed a gel-like texture. During this process, the degree of fibrillation of each sample was controlled by measuring the viscosity of the LCNF. The homogenization endpoint was reached when the viscosity reached the level of commercial CNF, yielding qualified LCNF material A2. This embodiment requires five homogenization cycles to reach the endpoint.
[0046] The AFM and SEM images of LCNF obtained in Example 9 are shown in the appendix. Figure 1 (c) and (f) indicate that the fiber fibrillation is relatively high.
[0047] Performance characterization of LCNF
[0048] The contact angles of the LCNFs (LCNF1 to LCNF9) obtained in Examples 1-9 are shown in the appendix. Figure 2 Its water contact angle is between 68.2° and 87.5°, indicating it is not very hydrophilic. In comparison, the highest water contact angle of LCNF (lignin content 11%-17%) prepared by Guo Shasha is 34.5°. The reason for the high water contact angle of LCNF prepared by this patented method is that ICSE redistributes lignin, and the more uniformly distributed lignin hinders the formation of hydrogen bonds between hydroxyl groups on the fiber and water molecules. Furthermore, the P-layer and S1-layer of the fiber cells, which are not effectively destroyed, hinder fiber swelling, resulting in a higher water contact angle for the sample. Simultaneously, this patented method does not remove lignin, and its lignin content is much higher than that of LCNF reported in the literature. According to the formula for the change of water-oil surface free energy reported by other researchers, under the same conditions, the closer the water contact angle of the pickering stabilized particles is to 90°, the better the stability of the prepared pickering emulsion. This fully demonstrates that the LCNF prepared by this patented method, due to its high lignin content and redistributed lignin, possesses excellent pickering emulsion stabilization properties.
[0049] The Zeta potentials of the LCNFs (LCNF1 to LCNF9) obtained in Examples 1-9 are shown below. Figure 3 Sergio et al. prepared LCNF using laccase-catalyzed lignin oxidation and a high-pressure homogenizer, achieving a zeta potential of -21.7 mV to 26.7 mV. Liu et al. prepared LCNF using a mechanochemical method, with a zeta potential range of -16 mV to 40.8 mV. In contrast, the LCNF prepared by the steam explosion combined with high-pressure homogenization method of this patented technology generally exhibits a lower zeta potential. It is generally believed that fiber suspensions are prone to flocculation when the absolute value of the zeta potential is below 25 mV. Due to the low zeta potential of the suspension, there is insufficient charge repulsion between LCNFs to maintain the suspension's stability. Sedimentation was observed in the LCNF suspension at lower concentrations (less than 1%) during storage. After vacuum rotary evaporation concentration, sedimentation no longer occurred in the fiber suspension at higher concentrations (greater than 1%). Analysis of variance showed no significant correlation between the zeta potential and the ICSE process parameters.
[0050] The Pickering emulsion stability of the LCNF (LCNF9) obtained in Example 9 is shown in the appendix. Figure 4 Soybean oil was used as the oil phase, and LCNF was used as the solid stabilizing particles in the Pickering emulsion. The Pickering emulsion was prepared using ultrasonic emulsification with a cell disruptor at an oil-to-water ratio of 1:4 (mL:g). Ultrasonic emulsification was performed at a power of 300W with a switching frequency of "3s-3s" for a total emulsification time of 2 minutes, resulting in an oil-in-water Pickering emulsion with LCNF as the stabilizing particles. At an addition of 1 mg / mL, the emulsion separated rapidly, and the volume fraction of the emulsion phase decreased to 29% and tended to stabilize with increasing time. Increasing the amount of LCNF9 resulted in more LCNF9 adsorbing at the water-oil interface, strengthening the emulsion's stabilizing ability; therefore, a rapid increase in emulsion stability was observed with increasing LCNF9 addition. The samples with 2 mg / mL and 5 mg / mL showed almost no emulsion stratification during the 30-day natural sedimentation process, and the volume fraction of the emulsion phase was similar, both maintaining at about 95%. This is close to the volume fraction of the emulsion phase during natural sedimentation of LCNF prepared by Guo Shasha using acid-hydrolyzed eucalyptus mechanical pulp.
[0051] The foregoing has shown and described the basic principles, main features, and advantages of the present invention. It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered illustrative and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the scope of the invention. No reference numerals in the claims should be construed as limiting the scope of the claims.
[0052] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.
Claims
1. A method for preparing lignin-cellulose nanofibers through coupled steam explosion pretreatment, characterized in that, Includes the following steps: S1 Pre-soaking: Cut the raw material into small pieces of 1-5cm, soak them in NaOH or aqueous solution, and set aside after pre-soaking; S2 Coupled Steam Explosion Pretreatment: The tobacco stalk fragments soaked in S1 are placed into a steam explosion storage tank. Coupled steam explosion is used, and the steam pressure is set to 0.4-0.8MPa. Then, air is used to pressurize the total pressure to 1.0-1.8MPa, and the pressure holding time is 2-15min. The pressure relief program is started, and the pressure is released in 0.005-3.0s to obtain the steam-exploded material A1. S3 Washing: A1 is washed to remove impurities, and the concentration of material A1 is adjusted to 0.5%wt to obtain material A2; S4 High-Pressure Homogenization: Material A2 is processed using a high-pressure homogenizer at a pressure of 700 bar until the fiber suspension of material A2 exhibits a gel-like texture. The degree of fibrillation is controlled by measuring the viscosity of the suspension to obtain LCNF material A3. S5 Concentration: Material A3 is concentrated using a vacuum rotary evaporator to obtain a product of the target concentration.
2. The method according to claim 1, characterized in that, The raw materials in S1 are crop straw and forestry branch waste.
Citation Information
Patent Citations
Beet pulp cellulose nanofibril and preparation method thereof
CN106087507A
Tobacco waste comprehensive utilization method
CN111945452A