Coarse aggregate elasticity modulus testing method and device based on point load
Through the test method based on point load, combined with Hertz contact theory and elasticity theory, the elastic modulus of coarse aggregate is directly calculated, which solves the problem of distortion of test results in the existing technology and achieves accurate evaluation of the elastic modulus of coarse aggregate. , providing a new theoretical basis for concrete design.
Patent Information
- Application Number
- CN202411046972.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-10-29
AI Technical Summary
The existing technology has multiple defects when testing the elastic modulus of coarse aggregate, including inhomogeneity of the cement, changes in the shape of the specimen, bond damage and the inability to directly characterize the deformation ability of the coarse aggregate, resulting in distortion of the test results, and different rock types. The particle size and shape of elastic rocks vary greatly during the crushing process, and there is a lack of accurate elastic modulus calculation methods.
Using a test method based on point load, by obtaining the load-displacement curve of the contact surface point during the compression process, combined with Hertz contact theory and elastic theory, the equivalent elastic modulus of the coarse aggregate is calculated, and the elasticity of the fixture contact head is calculated The modulus and Poisson's ratio are calculated simultaneously to directly obtain the elastic modulus of coarse aggregate.
It achieves accurate and direct testing of the elastic modulus of coarse aggregate and has a wide range of applications. It can evaluate coarse aggregates of different lithological rocks and shapes, provides a high-precision concrete design basis, reduces human operation errors, and improves efficiency. Validity of test results.
Smart Images

Figure CN118857960A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of the construction industry, and more specifically to a method and a device for testing the elastic modulus of coarse aggregate based on point load. Background Art
[0002] Concrete is the most important building material in today's society. The elastic modulus of concrete is an important parameter used to evaluate the relationship between the stiffness and deflection of its components. It is also a representation of the ability of concrete components to resist elastic deformation. In actual projects, although the concrete strength meets the requirements, the elastic modulus is low, which will lead to a large stress loss in the prestressed concrete structure, and then cause the structure to fail.
[0003] Coarse aggregate is the largest component of concrete by volume, so the performance of coarse aggregate has a crucial impact on the performance of concrete. More and more studies have shown that under certain conditions, the higher the elastic modulus of coarse aggregate, the greater the elastic modulus of concrete. However, in the actual design, production and application of concrete, there is a lack of accurate parameters related to the elastic modulus of coarse aggregate, and there is still a lack of corresponding testing methods in the specifications. Therefore, coarse aggregate is often regarded as an inert component and does not participate in accurate calculations. Even when coarse aggregate is considered, the parameters corresponding to the parent rock are directly used as the elastic parameters of coarse aggregate for analysis.
[0004] Due to geographical differences, even rocks of the same lithology will have large performance differences due to different mineral compositions. In response to the "low-carbon" policy, more and more projects are beginning to try to use recycled coarse aggregate to replace natural coarse aggregate. When designing concrete, it is more necessary to consider the performance of coarse aggregate itself. Based on this, how to determine the elastic parameters of coarse aggregate has become an urgent problem to be solved, which will also have far-reaching significance for concrete performance prediction and high elastic modulus concrete design. With the continuous maturity of ultrasonic detection technology, ultrasonic coarse aggregate detection technology has begun to be applied. The patent with publication number CN111239253A discloses a method for analyzing the elastic modulus of coarse aggregate based on ultrasonic velocity. The method first calculates the elastic modulus of the specimen prepared by the binder and the coarse aggregate, and then calculates the elastic modulus of the coarse aggregate according to the elastic parameters of the epoxy resin; the Chinese patent with publication number CN116558953A discloses a method for analyzing the performance of coarse aggregate by the control variable method, controlling the coarse aggregate to be different and other factors to be the same, and using the compressive strength ratio of concrete reaching the curing age as an indicator of the performance of coarse aggregate.
[0005] However, there are still many defects in the calculation of elastic modulus of coarse aggregate, which are mainly reflected in the following aspects:
[0006] (1) The current test of the elastic modulus of coarse aggregate does not test the coarse aggregate itself. When analyzing the specimens prepared with binder and coarse aggregate, the binder is manually stirred, the prepared specimens are thick, bubbles are difficult to avoid during the pouring process, and the uniformity of the binder in the specimens cannot be guaranteed.
[0007] (2) When ultrasonic testing is performed on specimens made of binder and coarse aggregate, the epoxy resin and other components in the binder will shrink in the natural environment, and the shape of the specimen will change. In addition, since the coarse aggregate has a small deformation, the bond between the binder and the coarse aggregate may be damaged. Bond damage, internal bubbles and deformation of the specimen will affect the ultrasonic testing process, causing distortion of the test results.
[0008] (3) When testing concrete prepared with different coarse aggregates, the performance of coarse aggregate can only be characterized in terms of strength. In actual engineering, the deformation capacity of concrete will have a more profound impact on the service performance of concrete;
[0009] (4) In the process of coarse aggregate production, rocks of different lithology will have different particle sizes and shapes even if the same crushing method is used.
[0010] Therefore, in order to better characterize the elastic modulus of coarse aggregate, a method for directly testing the elastic modulus of coarse aggregate is urgently needed. After obtaining the elastic modulus of coarse aggregate, it can promote a better analysis of the relationship between the elastic modulus of coarse aggregate and the elastic modulus of concrete, which has far-reaching significance for establishing a concrete elastic modulus prediction model based on coarse aggregate. Summary of the invention
[0011] In view of this, the present invention proposes a method and device for testing the elastic modulus of coarse aggregate based on point load, which can directly test the elastic modulus of coarse aggregate particles.
[0012] In order to achieve the above object, the present invention adopts the following technical solution:
[0013] The present invention provides a method for testing the elastic modulus of coarse aggregate based on point load, comprising the following steps:
[0014] S1. Based on the point load test, the load-displacement curve of the contact surface particle when elastic deformation occurs during compression is obtained;
[0015] S2. Based on Hertz contact theory, the equivalent elastic modulus of the contact surface is calculated through the load-displacement curve;
[0016] S3. Based on the elastic theory, the equivalent elastic modulus of the contact surface is obtained through the elastic modulus and Poisson's ratio of the fixture contact head and the elastic modulus and Poisson's ratio of the coarse aggregate;
[0017] S4. The equivalent elastic modulus obtained by the two different calculation methods of S2 and S3 are combined to calculate the elastic modulus of coarse aggregate.
[0018] Preferably, the method further comprises step S5: repeating steps S1 to S4 and taking the average value of the multiple times as the elastic modulus of the coarse aggregate.
[0019] Preferably, 6 specimens are designed for each test group. If the difference between the final test result and the average value is less than 15%, the average value is recorded as the effective coarse aggregate elastic modulus. If the difference is greater than 15%, the average value is recalculated after removing the maximum error value and then analyzed until the difference between all test results and the average value is less than 15%. The newly calculated average value is recorded as the effective value, but the number of final effective test results in each group should not be less than 3 values.
[0020] The present invention also provides a device for testing a load-displacement curve based on a point load, comprising a fixture shell, an upper pressure plate is provided on the upper side of the inner cavity of the fixture shell, and a lower pressure plate is provided on the lower side of the inner cavity, and loading blocks serving as pressure heads are provided at the axial centers of the opposing surfaces of the upper pressure plate and the lower pressure plate; a bearing plate is provided on the upper outer portion of the fixture shell, and the bearing plate and the upper pressure plate are connected by a connecting rod vertically penetrating the fixture shell, and a spring is sleeved on the outer ring of the connecting rod between the bearing plate and the upper surface of the fixture shell; displacement sensors are installed on both sides of the inner cavity of the fixture shell through a fixing frame, and the two displacement sensors are respectively connected to a displacement collection box through a wire, and the displacement sensor is used to analyze the displacement curve between the upper and lower pressure plates of the fixture over time during loading.
[0021] Preferably, the steps of using the fixture to obtain a load-displacement curve when a particle on the contact surface undergoes elastic deformation during compression are as follows:
[0022] (1) Install the fixture at the axis of the lower platen of the strength testing instrument, and fix the coarse aggregate sample to the center of the upper surface of the lower platen;
[0023] (2) Turn on the strength testing instrument to load, and adopt displacement loading to obtain a curve of load variation with time during the loading process; obtain the load-displacement curve during the entire loading process through the displacement-time curve obtained by the displacement sensor and the load-time curve obtained by the strength testing instrument.
[0024] Preferably, based on the Hertz contact theory, the calculation steps of the equivalent elastic modulus of the contact surface through the load-displacement curve are as follows: the obtained load-displacement curve is subjected to secondary processing, a new load-displacement curve is drawn with 3 times the load as the ordinate and the 3 / 2 power of the displacement as the abscissa, and the equivalent elastic modulus at the point load contact surface is calculated by regression analysis;
[0025] The load-displacement relationship of coarse aggregate during point loading is:
[0026]
[0027] in,
[0028] F con is the load corresponding to the contact surface;
[0029] E con is the equivalent elastic modulus at the contact surface;
[0030] d is the diameter of the hemispherical loading block on the upper and lower plates of the fixture;
[0031] ξ is the change in elastic displacement of the contact surface during loading.
[0032] Preferably, based on elastic theory, the method for obtaining the equivalent elastic modulus of the contact surface through the elastic modulus and Poisson's ratio of the fixture contact head and the elastic modulus and Poisson's ratio of the coarse aggregate is:
[0033] The micromechanical formula of coarse aggregate based on elastic theory is as follows:
[0034]
[0035] in,
[0036] ν st is the Poisson’s ratio of the clamp pressure head;
[0037] E st is the elastic modulus of the clamp indenter;
[0038] ν ca is the Poisson’s ratio of coarse aggregate, obtained during the parent rock property test;
[0039] E ca is the elastic modulus of coarse aggregate.
[0040] Preferably, the equivalent elastic moduli obtained by two different calculation methods are combined to calculate the elastic modulus of the coarse aggregate, and the calculation formula is as follows:
[0041]
[0042] Preferably, the loading block is a hemispherical tungsten carbide loading block, and the Poisson's ratio and elastic modulus of the loading block pressure head are 0.30 and 650 GPa respectively.
[0043] Preferably, the strength testing instrument is an electro-hydraulic servo pressure testing machine with an accuracy of 0.01N and a loading speed of 0.01mm / s to 0.03mm / s; and / or, a sponge for fixing coarse aggregate is installed on the lower pressure plate, and a hole is opened in the middle of the sponge.
[0044] Compared with the prior art, the method and device for testing the elastic modulus of coarse aggregate based on point load of the present invention have the following beneficial effects:
[0045] 1. The invention has strong applicability, high accuracy and wide application range. It can directly test the elastic modulus of coarse aggregates or other granular building materials of different shapes and sizes prepared from different lithology rocks, realize the direct evaluation of the elastic modulus of granular building materials such as coarse aggregates, and provide a new theoretical basis for the design of high elastic modulus concrete.
[0046] 2. The test result processing method designed in the present invention fully guarantees the validity of the test results. The results obtained during the test are continuous and free from human operation errors and subjective judgments. The quantitative effect is good. The difference in elastic properties of coarse aggregates of different lithologies can be more intuitively obtained through comparative analysis of load-displacement curves. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0048] Figure 1 A flow chart of a method for testing the elastic modulus of coarse aggregate based on point load provided by the present invention;
[0049] Figure 2 The structure diagram of the device for load-displacement curve test based on point load;
[0050] Figure 3 It is a front view of a sponge for fixing coarse aggregate;
[0051] Figure 4 It is a top view of the sponge used for fixing the coarse aggregate;
[0052] Figure 5 This is a diagram showing the failure state of coarse aggregate after point load test is completed;
[0053] Figure 6 is the load-displacement curve of coarse aggregate based on point loading;
[0054] Figure 7 This is the load-displacement curve of granite in Example 1.
[0055] Figure 8 For the granite in Example 1 Solve the curve.
[0056] Fig. 9 This is the load-displacement curve of basalt in Example 2.
[0057] Fig.10 The basalt in Example 2 Solve the curve.
[0058] In the figure: 1- fixture housing, 2- upper pressure plate, 3- lower pressure plate, 4- loading block, 5- bearing plate, 6- connecting rod, 7- spring, 8- fixing frame, 9- displacement sensor, 10- displacement collection box, 11- sponge. DETAILED DESCRIPTION
[0059] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are intended to be used to explain the present invention, and should not be construed as limiting the present invention.
[0060] In the description of the present invention, it is necessary to understand that the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0061] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is two or more, unless otherwise clearly and specifically defined.
[0062] like Figure 1 As shown, the present invention provides a method for testing the elastic modulus of coarse aggregate based on point load, comprising the following steps:
[0063] S1. Based on the point load test, the load-displacement curve of the contact surface particle when elastic deformation occurs during compression is obtained;
[0064] S2. Based on Hertz contact theory, the equivalent elastic modulus of the contact surface is calculated through the load-displacement curve;
[0065] S3. Based on the elastic theory, the equivalent elastic modulus of the contact surface is obtained through the elastic modulus and Poisson's ratio of the fixture contact head and the elastic modulus and Poisson's ratio of the coarse aggregate;
[0066] S4. The equivalent elastic modulus obtained by the two different calculation methods of S2 and S3 are combined to calculate the elastic modulus of coarse aggregate.
[0067] Furthermore, the method of the present invention further comprises step S5: repeating steps S1 to S4, and taking the average value of the multiple times as the elastic modulus of the coarse aggregate.
[0068] like Figure 2 As shown, the present invention also provides a load-displacement curve testing device based on point load, including a fixture shell 1, an upper pressure plate 2 is provided on the upper side of the inner cavity of the fixture shell 1, a lower pressure plate 3 is provided on the lower side of the inner cavity, and loading blocks 4 as pressure heads are provided at the axial centers of the opposing surfaces of the upper pressure plate 2 and the lower pressure plate 3; a bearing plate 5 is provided on the upper outer part of the fixture shell 1, the bearing plate 5 and the upper pressure plate 2 are connected by a connecting rod 6 vertically penetrating the fixture shell 1, and a spring 7 is sleeved on the outer ring of the connecting rod between the bearing plate 5 and the upper surface of the fixture shell 1; displacement sensors 9 are installed on both sides of the inner cavity of the fixture shell 1 through a fixing frame 8, and the two displacement sensors 9 are respectively connected to a displacement acquisition box 10 through a wire, and the displacement sensor 9 is used to analyze the displacement change curve between the upper and lower pressure plates of the fixture during loading.
[0069] In the present invention, the loading block 4 is a hemispherical tungsten carbide loading block with a diameter of 5 mm, and the Poisson's ratio and elastic modulus of the loading block pressure head are 0.30 and 650 GPa respectively.
[0070] In the present invention, the load plate 5 is pressed down by a strength testing instrument to load the fixture. The strength testing instrument is an electro-hydraulic servo pressure testing machine with an accuracy of 0.01N and a loading speed of 0.01mm / s to 0.03mm / s.
[0071] The present invention installs an LVDT displacement sensor on the inner side of the fixture housing 1 through a fixed knob, which is used to analyze the displacement curve between the upper and lower pressure plates of the fixture during loading. In addition, the loading block 4 is bolted to the upper and lower pressure plates to replace hemispherical loading blocks with different radii. At the same time, the installation of the spring 7 can ensure that after loading is completed, the upper pressure plate 2 of the fixture rebounds to the initial position as the electro-hydraulic servo pressure testing machine rises.
[0072] In the present invention, a sponge 11 for fixing the coarse aggregate is installed on the lower pressing plate 3. Figure 3 , Figure 4 As shown, a hole is opened in the middle of the sponge 11. When the sponge 11 is installed, the hole in the middle of the sponge 11 needs to be just at the center of the hemisphere of the lower pressing plate of the clamp.
[0073] In S1, the steps of using the fixture to obtain the load-displacement curve when the contact surface particles undergo elastic deformation during compression are as follows:
[0074] (1) Install the fixture of the present invention equipped with the LVDT displacement sensor at the center of the pressure platform of the electro-hydraulic servo pressure testing machine, and fix the coarse aggregate sample to the center of the upper surface of the lower pressure plate, specifically, fix the coarse aggregate in the middle opening of the sponge pad;
[0075] When sampling coarse aggregates, the present invention generally takes 10 particles of each coarse aggregate to be tested, of which 4 are used as spares. In order to ensure the accuracy of the test results, the fracture surface of the crushed coarse aggregate particles should be generated by the development of the point load loading point. At the same time, in order to obtain a complete load-displacement curve, needle-shaped particles should be avoided when sampling coarse aggregates. The coarse aggregate to be tested is placed at the center of the hemisphere above the lower pressure plate of the fixture, and slightly adjusted so that the coarse aggregate to be tested is effectively fixed on the sponge and does not fall from above the hemisphere.
[0076] (2) Turn on the electro-hydraulic servo pressure testing machine for loading. The loading method is displacement loading. The loading rate is 0.01 mm / s to 0.03 mm / s. The load-time curve during the loading process can be obtained. The load-displacement curve during the entire loading process can be obtained by the displacement-time curve obtained by the LVDT displacement sensor and the load-time curve obtained by the electro-hydraulic servo pressure testing machine;
[0077] After each coarse aggregate is loaded, remove the sponge pad under the coarse aggregate, use a brush to clean the sponge pad and the space between the upper and lower pressure plates of the fixture, and replace the sponge pad after ensuring that there are no broken coarse aggregate particles. After placing it, place another coarse aggregate to be tested on the hemisphere of the lower pressure plate of the fixture, and start the testing machine to test again;
[0078] After all 6 particles have been tested, the load-displacement curve is drawn based on the time correspondence. To determine whether the coarse aggregate destruction process is effective, refer to Figure 5 ( Figure 5 A in the figure refers to the point load loading point). When the coarse aggregate is damaged, if the damaged section is developed at the point load loading position, the damage process is considered to be effective. During the continuous test, if the fracture surface of a particle is cracked at a non-point load loading position, it is considered invalid. At this time, other spare particles should be used for retesting to obtain a supplementary load-displacement curve.
[0079] In S2, based on the Hertz contact theory, the equivalent elastic modulus of the contact surface is calculated through the load-displacement curve, which is specifically carried out in the following steps:
[0080] Firstly, the load-displacement curves obtained for different coarse aggregate particles were analyzed, such as Figure 6 As shown, it is determined that there are no noise points in the entire loading process and the entire process is complete. After confirming that the load-displacement curve meets the requirements of the next step of analysis, the load-displacement curve is processed for further analysis.
[0081] Considering the uneven shape of the coarse aggregate surface, if a flat indenter is used for loading, the contact surface between the coarse aggregate surface and the fulcrums on the upper and lower pressing plates may be unstable, which will make it difficult to determine the size of the contact surface area between the two. Therefore, in the fixture provided by the present invention, the fulcrums set on the upper and lower pressing plates are selected to be hemispherical. According to the Hertz theory, when a circular indenter contacts a plane, the relationship between load and displacement satisfies the equation 1:
[0082]
[0083] In the formula, F con is the load corresponding to the contact surface; E con is the equivalent elastic modulus at the contact surface; D is the diameter of the hemispherical loading block on the upper and lower plates of the fixture; ξ is the elastic displacement change of the contact surface during the loading process.
[0084] The fixture provided by the present invention is provided with two upper and lower pressing plates, and both pressing plates are provided with hemispherical fulcrums, so that during the load loading process, the same deformation will occur on the contact surface of the loading points on both sides of the coarse aggregate, and the total deformation ξ actually occurring in the load-displacement curve obtained by the test Tol =2ξ, so formula 1 can be simplified
[0085] Formula 2:
[0086]
[0087] Where d is the radius of the upper and lower hemispherical loading blocks.
[0088] From formula 2, we can know that the equivalent elastic modulus E at the contact surface is con The relationship shown in formula 3 will be satisfied:
[0089]
[0090] From formula 3, we can see that by converting the horizontal axis into the 3 / 2 power of displacement and setting the vertical axis to 3 times the load, the equivalent elastic modulus E at the contact surface position can be obtained by regression analysis: con .
[0091] In S3, based on elastic theory, the equivalent elastic modulus at the contact surface can be calculated by the elastic modulus and Poisson's ratio of two different materials, as shown in Equation 4;
[0092]
[0093] Where, ν st 、E st are the Poisson's ratio and elastic modulus of the fixture pressure head, respectively. Since the loading block is made of tungsten carbide, ν st 、E st Take 0.30 and 650 GPa respectively; ν ca 、E ca are the Poisson’s ratio and elastic modulus of the coarse aggregate, respectively, where ν ca It is obtained when testing the parent rock performance. When testing the parent rock elastic modulus, empirical parameters can be used for analysis. The statistical Poisson's ratio of common rocks is shown in Table 1.
[0094] Table 1 Poisson's ratio of common rocks
[0095]
[0096] In S4, by combining equations 3 and 4, we can obtain the equation for directly calculating the elastic modulus of coarse aggregate, as shown in equation 5;
[0097]
[0098] In order to ensure the accuracy of the measurement results, the present invention also designs a test result processing method. Each group is designed with 6 test pieces. If the difference between the final test result and the average value is less than 15%, the average value is recorded as the effective coarse aggregate elastic modulus.
[0099] Specifically, the six groups of load-displacement curves were analyzed, and the elastic moduli of the six coarse aggregates were calculated by equations 1 to 5. The average value of the elastic moduli of the six coarse aggregates was taken. When the elastic modulus E calculated for each coarse aggregate cai If formula 6 is satisfied, the result is considered valid;
[0100]
[0101] In the formula, E cai is the elastic modulus of each coarse aggregate, i = 1, 2, 3…
[0102] If the difference is greater than 15%, remove the maximum error value and recalculate the average value, and substitute it into Formula 6 for calculation again until the relationship in Formula 6 is satisfied. The newly calculated average value is recorded as the valid value. When screening out the maximum error value for processing, it should be ensured that the final number of valid test results should not be less than 3 to be valid.
[0103] Embodiment 1:
[0104] Granite coarse aggregate with a particle size range of 10mm to 20mm was sampled, and a total of 10 pieces were selected. The Poisson's ratio obtained from the granite parent rock test was 0.30. In the subsequent calculation, the Poisson's ratio of the coarse aggregate was taken as 0.30, and the elastic modulus and Poisson's ratio of the hemispherical loading block were taken as 650GPa and 0.30 respectively. The fixture with the LVDT displacement sensor installed was placed at the axis of the lower load platform of the electro-hydraulic servo pressure testing machine; a fixed sponge was installed above the hemispherical loading block of the lower pressure plate of the fixture, and the testing machine was turned on after slight adjustments. The loading mode was set to displacement loading, and the loading speed was 0.02mm / s. After the loading was completed, the fixed sponge plane was cleaned until 6 sets of effective coarse aggregate load-time curves and displacement-time curves were obtained. The elastic modulus of the coarse aggregate calculated from the 6 sets of data was averaged as the final value. Here, one of the load-displacement curves is used for illustration. The final load-displacement curve obtained is shown as follows: Figure 7 shown.
[0105] Set the ordinate to 3 times the load value and the abscissa to the 3 / 2 power of the displacement, and get the new load-displacement curve as follows: Figure 8 As shown in formula 3, the slope of the curve after secondary processing is Depend on Figure 8 The fitting results show that the equivalent elastic modulus E of granite coarse aggregate is con satisfy And because d = 2.5 mm, then E con =67.92GPa. The equivalent elastic modulus E of granite coarse aggregate con Substitute into equation 4 and equation 5, where ν st =0.30, E st =650GPa, ν ca = 0.30, the elastic modulus of granite coarse aggregate is E ca =68.30GPa.
[0106] By analyzing the other five groups of data, the elastic moduli of the coarse aggregate obtained are 62.50 GPa, 60.83 GPa, 72.02 GPa, 67.56 GPa and 65.33 GPa, respectively, which meet the requirements of Formula 6. Therefore, the elastic modulus of the granite coarse aggregate to be tested is 66.090 GPa.
[0107] Embodiment 2:
[0108] Basalt coarse aggregate with a particle size of 10 mm to 20 mm was sampled, and 10 pieces were also selected. The Poisson's ratio of the basalt parent rock test was 0.23. In the subsequent calculation, the Poisson's ratio of the basalt coarse aggregate was 0.23. The specific test process was the same as that in Example 1 until 6 groups of load-time curves and displacement-time curves of effective coarse aggregate were obtained. The elastic modulus of the coarse aggregate calculated from the 6 groups of data was averaged as the final value. Here, one of the load-displacement curves is also used for illustration. The final load-displacement curve obtained is as follows: Fig. 9 As shown:
[0109] Set the ordinate to 3 times the load value and the abscissa to the 3 / 2 power of the displacement, and get the new load-displacement curve as follows: Fig.10 As shown in the figure, regression analysis shows that the equivalent elastic modulus E of basalt coarse aggregate is con satisfy And because d = 2.5 mm, then E con =75.15GPa. The equivalent elastic modulus E of granite coarse aggregate con Substitute into equation 4 and equation 5, where ν st =0.30, E st =650GPa, ν ca = 0.23, the elastic modulus of basalt coarse aggregate is E ca =79.93GPa.
[0110] By analyzing the other five groups of data, the elastic moduli of the coarse aggregate obtained are 84.65 GPa, 70.66 GPa, 75.91 GPa, 77.63 GPa and 85.36 GPa, respectively, which meet the requirements of Formula 6. Therefore, the elastic modulus of the basalt coarse aggregate to be tested is 79.02 GPa.
[0111] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0112] The above description of the disclosed embodiments enables one skilled in the art to implement or use the present invention. Various modifications to these embodiments will be apparent to one skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features disclosed herein.
Claims
1. A method for testing the elastic modulus of coarse aggregate based on point load, characterized in that: The following steps are involved: S1. Based on the point load test, the load-displacement curve of the contact surface particle when elastic deformation occurs during compression is obtained; S2. Based on Hertz contact theory, the equivalent elastic modulus of the contact surface is calculated through the load-displacement curve; S3. Based on the elastic theory, the equivalent elastic modulus of the contact surface is obtained through the elastic modulus and Poisson's ratio of the fixture contact head and the elastic modulus and Poisson's ratio of the coarse aggregate; S4. The equivalent elastic modulus obtained by the two different calculation methods of S2 and S3 are combined to calculate the elastic modulus of coarse aggregate.
2. A method for testing the elastic modulus of coarse aggregate based on point load according to claim 1, characterized in that: The method further comprises step S5: repeating steps S1 to S4 and taking an average value of the multiple times as the elastic modulus of the coarse aggregate.
3. A method for testing the elastic modulus of coarse aggregate based on point load according to claim 2, characterized in that: Six specimens are designed for each test group. If the difference between the final test result and the average value is less than 15%, the average value is recorded as the effective coarse aggregate elastic modulus. If the difference is greater than 15%, the average value is recalculated after removing the maximum error value and then analyzed until the difference between all test results and the average value is less than 15%. The newly calculated average value is recorded as the effective value, but the number of final effective test results in each group should not be less than 3 values.
4. A device for testing a load-displacement curve based on a point load, characterized in that: It includes a fixture shell, an upper pressure plate is provided on the upper side of the inner cavity of the fixture shell, and a lower pressure plate is provided on the lower side of the inner cavity, and loading blocks serving as pressure heads are provided at the axial centers of the opposing surfaces of the upper pressure plate and the lower pressure plate; a bearing plate is provided on the upper outer part of the fixture shell, and the bearing plate and the upper pressure plate are connected by a connecting rod vertically penetrating the fixture shell, and a spring is sleeved on the outer ring of the connecting rod between the bearing plate and the upper surface of the fixture shell; displacement sensors are installed on both sides of the inner cavity of the fixture shell through a fixing frame, and the two displacement sensors are respectively connected to a displacement acquisition box through a wire, and the displacement sensor is used to analyze the displacement curve between the upper and lower pressure plates of the fixture during loading.
5. The device for testing a load-displacement curve based on a point load according to claim 4, characterized in that: The steps of using the fixture to obtain the load-displacement curve when the contact surface particle undergoes elastic deformation during compression are as follows: (1) Install the fixture at the axis of the lower platen of the strength testing instrument, and fix the coarse aggregate sample to the center of the upper surface of the lower platen; (2) Turn on the strength testing instrument to load, and adopt displacement loading to obtain a curve of load variation with time during the loading process; obtain the load-displacement curve during the entire loading process through the displacement-time curve obtained by the displacement sensor and the load-time curve obtained by the strength testing instrument.
6. The device for testing a load-displacement curve based on a point load according to claim 5, characterized in that: Based on the Hertz contact theory, the calculation steps of the equivalent elastic modulus of the contact surface through the load-displacement curve are as follows: the obtained load-displacement curve is processed twice, a new load-displacement curve is drawn with 3 times the load as the ordinate and the 3 / 2 power of the displacement as the abscissa, and the equivalent elastic modulus at the point load contact surface is calculated by regression analysis; The load-displacement relationship of coarse aggregate during point loading is: in, F con is the load corresponding to the contact surface; E con is the equivalent elastic modulus at the contact surface; d is the diameter of the hemispherical loading block on the upper and lower plates of the fixture; ξ is the change in elastic displacement of the contact surface during loading.
7. The device for testing a load-displacement curve based on a point load according to claim 6, characterized in that: Based on the elastic theory, the method for obtaining the equivalent elastic modulus of the contact surface is as follows through the elastic modulus and Poisson's ratio of the fixture contact head and the elastic modulus and Poisson's ratio of the coarse aggregate: The micromechanical formula of coarse aggregate based on elastic theory is as follows: in, ν st is the Poisson’s ratio of the clamp pressure head; E st is the elastic modulus of the clamp indenter; ν ca is the Poisson’s ratio of coarse aggregate, obtained during the parent rock property test; E ca is the elastic modulus of coarse aggregate.
8. The device for testing a load-displacement curve based on a point load according to claim 7, characterized in that: The equivalent elastic modulus obtained by two different calculation methods is combined to calculate the elastic modulus of coarse aggregate. The calculation formula is as follows: 。 9. The device for testing a load-displacement curve based on a point load according to claim 4, characterized in that: The loading block is a hemispherical tungsten carbide loading block, and the Poisson's ratio and elastic modulus of the loading block pressure head are 0.30 and 650 GPa respectively.
10. The device for testing a load-displacement curve based on a point load according to claim 4, characterized in that: The strength testing instrument is an electro-hydraulic servo pressure testing machine with an accuracy of 0.01N and a loading speed of 0.01mm / s to 0.03mm / s; and / or, a sponge for fixing coarse aggregate is installed on the lower pressure plate, and a hole is opened in the middle of the sponge.