A method, device, equipment and medium for evaluating the anti-ablation performance of ultra-high temperature ceramics
By obtaining the component allocation ratio information of ceramics and the porosity of oxide films, judging the depletion layer, building an ablation calculation model, and evaluating the ablation resistance of ceramic materials, it solves the complicated and time-consuming evaluation of the ablation resistance of ceramic materials in the prior art. Problems, improving assessment accuracy and efficiency.
Patent Information
- Application Number
- CN202411320379.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-09-23
AI Technical Summary
The existing ceramic materials have complex and time-consuming methods for evaluating anti-ablative performance in the design of thermal protection structures of high-speed aircraft, making it difficult to directly measure the ablative resistance of ceramic materials under service conditions.
By obtaining the group allocation ratio information of C-SiC-ZrB2 ceramics, determining its oxide film porosity in high-temperature aerobic environment, and determining whether there is a silicon carbide depletion layer, ablation calculation model is constructed to evaluate the ablation resistance of ceramics. Performance, including oxide layer thickness, ceramic retraction and ceramic weight gain.
It improves the accuracy and efficiency of performance evaluation of ceramic materials, saves people, finances and material resources, and improves the analysis efficiency of thermal protection structure design of high-speed aircraft.
Smart Images

Figure CN118862518B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of high-speed aircraft thermal protection, and in particular to a method, device, equipment and medium for evaluating the anti-ablation performance of ultra-high temperature ceramics. Background Art
[0002] At present, C-SiC-ZrB 2 (Carbon-Silicon Carbide-Zirconium Diboride) ultra-high temperature ceramic materials have been favored by aerospace designers in recent years and are widely used in thermal protection of key parts of the new generation of high-speed aircraft.
[0003] When designing the thermal protection structure of high-speed aircraft, it is necessary to consider the C-SiC-ZrB 2 The current performance evaluation methods for ceramic materials are usually experimental assessment and theoretical calculation. Experimental testing is the basis of analysis. However, for various application scenarios such as different component ratios, temperatures and oxygen partial pressures, the test is very complicated and time-consuming. Summary of the invention
[0004] In view of this, the purpose of the present invention is to provide a method, device, equipment and medium for evaluating the anti-ablation performance of ultra-high temperature ceramics, which effectively solves the current problem of determining the anti-ablation performance of ceramic materials under service conditions by direct measurement, and improves the accuracy and efficiency of performance evaluation, thereby improving the efficiency of high-speed aircraft thermal protection structure design and analysis, and greatly saving manpower, financial and material resources. The specific scheme is as follows:
[0005] In a first aspect, the present application provides a method for evaluating the ablation resistance of ultra-high temperature ceramics, comprising:
[0006] Get C-SiC-ZrB 2 The component ratio information corresponding to the ceramic; wherein the component ratio information is C component, SiC component and ZrB 2 The ratio information of the components;
[0007] Determine the composition ratio of the C-SiC-ZrB after oxidation in a preset high temperature oxygen environment based on the composition ratio information 2 The porosity of the surface oxide film of the ceramic;
[0008] The C-SiC-ZrB after oxidation is determined based on the porosity and the preset depletion layer judgment rule. 2 Whether there is a silicon carbide depletion layer between the ceramic and the oxide to obtain the corresponding judgment result;
[0009] Constructing a corresponding mathematical model according to the judgment result and the corresponding environmental conditions to obtain a corresponding ablation calculation model;
[0010] Based on the ablation calculation model, the C-SiC-ZrB 2 The ablation characteristic parameters corresponding to the ceramic are used to complete the corresponding ceramic anti-ablation performance evaluation operation; wherein the ablation characteristic parameters include the corresponding oxide layer thickness, ceramic retreat amount and ceramic weight gain.
[0011] Optionally, the C-SiC-ZrB after oxidation is judged based on the porosity and a preset depletion layer judgment rule. 2 Whether there is a silicon carbide depletion layer between the ceramic and the oxide, in order to obtain the corresponding judgment results, including:
[0012] Based on the porosity, the C-SiC-ZrB 2 The mole fraction of SiC in the ceramic is calculated using a preset judgment formula to obtain a corresponding target threshold;
[0013] Determine the C-SiC-ZrB 2 Whether the first volume fraction of C / SiC in the ceramic is greater than the target threshold value, so as to obtain a corresponding judgment result.
[0014] Optionally, constructing a corresponding mathematical model according to the judgment result and corresponding environmental conditions to obtain a corresponding ablation calculation model includes:
[0015] When the judgment result shows that the first volume fraction is not greater than the target threshold, it is determined that a silicon carbide depletion layer exists, and a high-temperature solid-state hybrid layer model or a low-temperature surface glass layer model is constructed under corresponding conditions by selecting corresponding environmental conditions;
[0016] When the judgment result indicates that the first volume fraction is greater than the target threshold, it is determined that the silicon carbide depletion layer does not exist, and the corresponding environmental conditions are selected to perform a high-temperature solid-state mixed layer model or a low-temperature surface glass layer model under corresponding conditions to obtain a corresponding ablation calculation model.
[0017] Optionally, the step of selecting corresponding environmental conditions to construct a high-temperature solid-state mixed layer model or a low-temperature surface glass layer model under corresponding conditions includes:
[0018] In the construction of mathematical models, the corresponding thermochemical reaction analysis, internal depletion layer flow rate relationship analysis, solid oxide layer evolution analysis, high temperature liquid-solid oxide layer evolution analysis or low temperature surface SiO 2 -B 2 O 3 The glass layer evolution is analyzed, and a formula is derived based on the first volume fraction, the porosity, and the mole fraction corresponding to the SiC to obtain the corresponding ablation calculation model.
[0019] Optionally, the ablation calculation model is used to determine the C-SiC-ZrB 2 The corresponding ablation characteristic parameters of ceramics are used to complete the corresponding ceramic anti-ablation performance evaluation operation, including:
[0020] The oxidized C-SiC-ZrB is calculated based on the porosity, the mole fraction corresponding to the SiC, and the first volume fraction. 2 Borosilicate and ZrO in the oxide layer of ceramics 2 , to obtain the corresponding second volume fraction and third volume fraction;
[0021] Determine the ablation calculation model, the second volume fraction, and the third volume fraction based on the C-SiC-ZrB 2 The corresponding oxide layer thickness, ceramic retreat amount and ceramic weight gain of the ceramic are used to complete the corresponding ceramic anti-ablation performance evaluation operation.
[0022] Optionally, the ablation calculation model, the second volume fraction and the third volume fraction are used to determine the C-SiC-ZrB 2 The thickness of the oxide layer corresponding to the ceramic includes:
[0023] When the ablation calculation model is a high-temperature solid mixed layer model, the corresponding solid oxide thickness calculation and surface glassy material thickness calculation are performed through the ablation calculation model, the second volume fraction, and the third volume fraction to obtain the corresponding first thickness and second thickness;
[0024] The first thickness and the second thickness are combined to obtain the corresponding oxide layer thickness.
[0025] In a second aspect, the present application provides an ultra-high temperature ceramic ablation resistance evaluation device, comprising:
[0026] Ratio information acquisition module, used to obtain C-SiC-ZrB 2 The component ratio information corresponding to the ceramic; wherein the component ratio information is C component, SiC component and ZrB 2 The ratio information of the components;
[0027] The porosity acquisition module is used to determine the porosity of the C-SiC-ZrB after oxidation in a preset high temperature oxygen environment based on the component ratio information. 2 The porosity of the surface oxide film of the ceramic;
[0028] A depletion layer judgment module is used to judge the depletion layer of the oxidized C-SiC-ZrB based on the porosity and the preset depletion layer judgment rule. 2Whether there is a silicon carbide depletion layer between the ceramic and the oxide to obtain the corresponding judgment result;
[0029] A mathematical model building module, used to build a corresponding mathematical model according to the judgment result and corresponding environmental conditions to obtain a corresponding ablation calculation model;
[0030] A parameter calculation module is used to determine the C-SiC-ZrB 2 The ablation characteristic parameters corresponding to the ceramic are used to complete the corresponding ceramic anti-ablation performance evaluation operation; wherein the ablation characteristic parameters include the corresponding oxide layer thickness, ceramic retreat amount and ceramic weight gain.
[0031] Optionally, the depletion layer determination module includes:
[0032] A threshold value acquisition unit is used for obtaining a threshold value based on the porosity and the C-SiC-ZrB 2 The mole fraction of SiC in the ceramic is calculated using a preset judgment formula to obtain a corresponding target threshold;
[0033] A judgment result acquisition unit is used to judge the C-SiC-ZrB 2 Whether the first volume fraction of C / SiC in the ceramic is greater than the target threshold value, so as to obtain a corresponding judgment result.
[0034] In a third aspect, the present application provides an electronic device, including:
[0035] Memory, used to store computer programs;
[0036] The processor is used to execute the computer program to implement the steps of the aforementioned method for evaluating the anti-ablation performance of ultra-high temperature ceramics.
[0037] In a fourth aspect, the present application provides a computer-readable storage medium for storing a computer program, which, when executed by a processor, implements the steps of the aforementioned method for evaluating the ablation resistance of ultra-high temperature ceramics.
[0038] It can be seen that in this application, the C-SiC-ZrB 2 The component ratio information corresponding to the ceramic; wherein the component ratio information is C component, SiC component and ZrB 2 component ratio information; based on the component ratio information, determining the C-SiC-ZrB after oxidation in a preset high temperature oxygen environment 2 The porosity of the surface oxide film of the ceramic is determined based on the porosity and the preset depletion layer judgment rule. 2Whether there is a silicon carbide depletion layer between the ceramic and the oxide, so as to obtain a corresponding judgment result; construct a corresponding mathematical model according to the judgment result and the corresponding environmental conditions to obtain a corresponding ablation calculation model; determine the C-SiC-ZrB 2 The ablation characteristic parameters corresponding to the ceramic are used to complete the corresponding ceramic anti-ablation performance evaluation operation; wherein the ablation characteristic parameters include the corresponding oxide layer thickness, ceramic retreat amount and ceramic weight gain. That is, in this application, firstly based on C-SiC-ZrB 2 The porosity of the oxide layer is determined based on the composition ratio information of the ceramic, and then the presence or absence of a silicon carbide depletion layer is determined. Then, the corresponding ablation calculation model is determined based on the judgment result and environmental conditions, and the ablation calculation model is used to obtain the C-SiC-ZrB 2 The corresponding oxide layer thickness, ceramic retreat and ceramic weight gain of the ceramic are used to complete the corresponding anti-ablation performance evaluation operation. In this way, the current problem of determining the anti-ablation performance of ceramic materials under service conditions by direct measurement is effectively solved, and the accuracy and efficiency of performance evaluation are improved, thereby improving the efficiency of high-speed aircraft thermal protection structure design and analysis, and greatly saving manpower, financial and material resources. BRIEF DESCRIPTION OF THE DRAWINGS
[0039] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the provided drawings without paying creative work.
[0040] Figure 1 A flow chart of a method for evaluating the anti-ablation performance of ultra-high temperature ceramics provided in this application;
[0041] Figure 2 A schematic diagram of a specific process flow of an ultra-high temperature ceramic ablation resistance evaluation method provided in this application;
[0042] Figure 3 A C-SiC-ZrB provided in this application 2 Schematic diagram of low temperature oxidation of ceramics with a depletion layer;
[0043] Figure 4 A C-SiC-ZrB provided in this application 2 Schematic diagram of high temperature oxidation of ceramics with a depletion layer;
[0044] Figure 5 A C-SiC-ZrB provided in this application 2 Schematic diagram of low-temperature oxidation of ceramics without depletion layer;
[0045] Figure 6 A SiC-ZrB with different compositions and temperatures provided in this application 2 Schematic diagram of oxidation weight gain;
[0046] Figure 7 A schematic diagram of the structure of an ultra-high temperature ceramic ablation resistance evaluation device provided in this application;
[0047] Figure 8 A structural diagram of an electronic device provided for this application. DETAILED DESCRIPTION
[0048] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0049] When designing the thermal protection structure of high-speed aircraft, it is necessary to consider the C-SiC-ZrB 2 The anti-ablation performance of ceramic materials, and the current performance evaluation methods usually include two methods: experimental assessment and theoretical calculation. Experimental testing is the basis of analysis. However, for various application scenarios such as different component ratios, temperatures and oxygen partial pressures, the test is very complicated and time-consuming. To this end, this application provides an ultra-high temperature ceramic anti-ablation performance evaluation scheme, which can effectively solve the current problem of determining the anti-ablation performance of ceramic materials under service conditions by direct measurement, and improve the accuracy and efficiency of performance evaluation. See Figure 1 As shown, the embodiment of the present invention discloses a method for evaluating the anti-ablation performance of ultra-high temperature ceramics, comprising:
[0050] Step S11, obtain C-SiC-ZrB 2 The component ratio information corresponding to the ceramic; wherein the component ratio information is C component, SiC component and ZrB 2 The ratio information of the components.
[0051] Step S12: Determine the composition ratio of the C-SiC-ZrB after oxidation in a preset high temperature oxygen environment based on the composition ratio information. 2 The porosity of the surface oxide film of ceramics.
[0052] Step S13: judging the oxidized C-SiC-ZrB based on the porosity and the preset depletion layer judgment rule. 2 Whether there is a silicon carbide depletion layer between the ceramic and the oxide, in order to obtain the corresponding judgment result.
[0053] Combination Figure 2 As shown, in this embodiment, it is determined that the C-SiC-ZrB 2 Ceramics (the C-SiC-ZrB 2 Ceramics Figure 2 The surface oxide film (i.e. ZrO 2 The porosity f pore (That is, Figure 2 After the 'porosity of oxide layer' in the equation, it is necessary to judge the C-SiC-ZrB after oxidation based on the corresponding criterion of the presence or absence of depletion layer. 2 Whether there is a silicon carbide (SiC) depletion layer between the ceramic and the oxide. Specifically, the criterion for whether there is a depletion layer is as follows:
[0054] (1);
[0055] Among them, f cs The substrate (i.e., the C-SiC-ZrB 2 The volume fraction of C / SiC in the ceramic (which can be determined based on the component ratio information); m 2 is the molar fraction of SiC component; M C is the molar mass of C; is the density of C; M SiC is the molar mass of SiC; is the density of SiC; ZrB 2 The molar mass of ZrB 2 density; ZrB 2 With O 2 The reaction rate of the reaction; C-SiC and O 2 The reaction rate of the reaction. It can be seen that f cs There is a maximum value, beyond which no SiC depletion layer is formed, which is related to the component composition and the respective reaction rate constants. 2 The reaction rates in ceramics are basically the same, i.e. , and the obtained f cs ≈0.55. That is, the porosity and the preset depletion layer judgment rule are used to judge the oxidation of the C-SiC-ZrB 2 Whether there is a silicon carbide depletion layer between the ceramic and the oxide, so as to obtain a corresponding judgment result, including: based on the porosity, the C-SiC-ZrB2 The mole fraction of SiC in the ceramic (i.e. m 2 ) and the preset judgment formula are calculated to obtain the corresponding target threshold; determine the C-SiC-ZrB 2 The first volume fraction of C / SiC in ceramics (i.e., f cs ) is greater than the target threshold to obtain the corresponding judgment result.
[0056] Step S14: construct a corresponding mathematical model according to the judgment result and the corresponding environmental conditions to obtain a corresponding ablation calculation model.
[0057] Combination Figure 2 As shown, in this embodiment, after obtaining the judgment result, a corresponding high-temperature or low-temperature mathematical model is constructed based on the corresponding environmental conditions (temperature), that is, the corresponding mathematical model is constructed according to the judgment result and the corresponding environmental conditions to obtain the corresponding ablation calculation model, including: when the judgment result shows that the first volume fraction is not greater than the target threshold, it is determined that there is a silicon carbide depletion layer, and the high-temperature solid-state hybrid layer model or the low-temperature surface glass layer model is constructed under the corresponding conditions by selecting the corresponding environmental conditions; when the judgment result shows that the first volume fraction is greater than the target threshold, it is determined that there is no silicon carbide depletion layer, and the high-temperature solid-state hybrid layer model or the low-temperature surface glass layer model is constructed under the corresponding conditions by selecting the corresponding environmental conditions to obtain the corresponding ablation calculation model.
[0058] Further, in this embodiment, the construction of a high-temperature solid mixed layer model or a low-temperature surface glass layer model under corresponding conditions by selecting corresponding environmental conditions includes: in the construction of the mathematical model, by performing corresponding thermochemical reaction analysis, internal depletion layer flow rate relationship analysis, solid oxide layer evolution analysis and high-temperature liquid-solid oxide layer evolution analysis or low-temperature surface SiO 2 -B 2 O 3 The glass layer evolution is analyzed, and a formula is derived based on the first volume fraction, the porosity, and the mole fraction corresponding to the SiC to obtain the corresponding ablation calculation model.
[0059] Step S15: Determine the C-SiC-ZrB 2 The ablation characteristic parameters corresponding to the ceramic are used to complete the corresponding ceramic anti-ablation performance evaluation operation; wherein the ablation characteristic parameters include the corresponding oxide layer thickness, ceramic retreat amount and ceramic weight gain.
[0060] It should be understood that in this embodiment, the ablation calculation model is used to determine the C-SiC-ZrB2 ablation characteristic parameters corresponding to the ceramic to complete the corresponding ceramic ablation resistance evaluation operation, including: calculating the C-SiC-ZrB after oxidation based on the porosity, the mole fraction corresponding to the SiC, and the first volume fraction; 2 Borosilicate (B 2 O 3 -SiO 2 ) and ZrO 2 The volume fraction of the C-SiC-ZrB is determined based on the ablation calculation model, the second volume fraction and the third volume fraction to obtain the corresponding second volume fraction and third volume fraction; 2 The corresponding oxide layer thickness, ceramic retreat and ceramic weight gain (i.e. Figure 2 material mass loss in the process) to complete the corresponding ceramic ablation resistance evaluation operation.
[0061] It is further understood that, in this embodiment, the ablation calculation model, the second volume fraction and the third volume fraction are used to determine the C-SiC-ZrB 2 The oxide layer thickness corresponding to the ceramic includes: when the ablation calculation model is a high-temperature solid mixed layer model, the corresponding solid oxide thickness calculation and surface glassy material thickness calculation are performed through the ablation calculation model, the second volume fraction and the third volume fraction to obtain the corresponding first thickness and second thickness; the first thickness and the second thickness are combined to obtain the corresponding oxide layer thickness. That is to say, when the ablation calculation model is a high-temperature solid mixed layer model, the oxide layer thickness is the sum of the solid oxide thickness and the surface glassy material thickness. At the same time, it can be understood that when the ablation calculation model is a low-temperature surface glass layer model, the oxide layer thickness is the surface glassy material thickness.
[0062] Regarding the low temperature surface glass layer model, combined with Figure 3 As shown, there is SiO on the low temperature surface 2 -B 2 O 3 Under glass layer conditions, the thickness of the surface glassy material (l 3a )、Thickness of solid oxide layer(l 23 )、Ceramic retreat( + )、Ceramic weight gain W gain The expressions are as follows:
[0063] (2);
[0064] (3);
[0065] (4);
[0066] (5);
[0067] And about the depletion layer size l 12 ,exist:
[0068] (6);
[0069] Where, t is the oxidation time; ZrO in the oxide layer 2 Volume fraction; f glass Borosilicate (B 2 O 3 -SiO 2 ) volume fraction; m 1 is the mole fraction of component C; for ZrO 2 density; for ZrO 2 The molar mass of SiO 2 Evaporation flow rate; For B 2 O 3 Evaporation flow rate, the subscript "vap" means evaporation; For B 2 O 3 The molar mass of is the flow rate of SiO in area 12; SiO 2 The molar mass of SiO 2 density; for Figure 3 The oxygen flow rate in the region 23 between the interfaces i2 and i3; ZrB 2 The amount of setback of the component; is the retreat amount of SiC component; l 23 for Figure 3 The thickness of the region 23 between the interfaces i2 and i3; 3a is the thickness of the region a3 between i3 and a.
[0070] Regarding the high temperature solid mixed layer model, there is no SiO on the surface 2 -B 2 O 3 Under the glass layer condition, the ratio of the thickness of the glassy substance to the thickness of the solid oxide layer and the weight gain of the ceramic are:
[0071] (7);
[0072] (8).
[0073] It can be seen that in the embodiment of the present application, the C-SiC-ZrB 2 The component ratio information corresponding to the ceramic; wherein the component ratio information is C component, SiC component and ZrB 2 component ratio information; based on the component ratio information, determining the C-SiC-ZrB after oxidation in a preset high temperature oxygen environment 2 The porosity of the surface oxide film of the ceramic is determined based on the porosity and the preset depletion layer judgment rule. 2 Whether there is a silicon carbide depletion layer between the ceramic and the oxide, so as to obtain a corresponding judgment result; construct a corresponding mathematical model according to the judgment result and the corresponding environmental conditions to obtain a corresponding ablation calculation model; determine the C-SiC-ZrB 2 The ablation characteristic parameters corresponding to the ceramic are used to complete the corresponding ceramic anti-ablation performance evaluation operation; wherein the ablation characteristic parameters include the corresponding oxide layer thickness, ceramic retreat amount and ceramic weight gain. That is, in this application, firstly based on C-SiC-ZrB 2 The porosity of the oxide layer is determined based on the composition ratio information of the ceramic, and then the presence or absence of a silicon carbide depletion layer is determined. Then, the corresponding ablation calculation model is determined based on the judgment result and environmental conditions, and the ablation calculation model is used to obtain the C-SiC-ZrB 2 The corresponding oxide layer thickness, ceramic retreat and ceramic weight gain of the ceramic are used to complete the corresponding anti-ablation performance evaluation operation. In this way, the current problem of determining the anti-ablation performance of ceramic materials under service conditions by direct measurement is effectively solved, and the accuracy and efficiency of performance evaluation are improved, thereby improving the efficiency of high-speed aircraft thermal protection structure design and analysis, and greatly saving manpower, financial and material resources.
[0074] Combine the following Figure 2-Figure 6 The schematic diagram disclosed in the figure specifically illustrates the technical solution of the embodiment of the present application.
[0075] Regarding the analysis of thermochemical reactions, it is considered that the oxidation rate of ceramics is controlled by the dissolution and penetration of oxygen in the glassy substance, that is, the diffusion rate into the material, rather than the reaction to form carbon gaseous products (CO or CO 2 ) outward diffusion control. Therefore, for the presence or absence of SiC depletion layer, it is assumed that there is an extremely small SiC depletion layer at the beginning of oxidation, and the CO / CO 2Convection diffusion transport mechanism. If after a certain oxidation time, the SiC depletion layer void area has no significant change relative to the initial thickness and solid oxide layer, it is considered that there is no depletion layer, otherwise the calculated value is used as the depletion layer thickness. Therefore, a depletion layer model is first established, combined with Figure 3 and Figure 4 shown.
[0076] Assuming that C and SiC share an oxidation surface, the molar ratio of the two is , and let m 1 +m 2 =1. At the beginning, the oxidation reaction formula of C / SiC when encountering oxygen is:
[0077] (9);
[0078] The generated CO and SiO gas products diffuse outward and encounter oxygen at the top of the depletion layer (void) for further oxidation.
[0079] 2m 2 SiO(g)+m 2 O 2 (g)→2m 2 SiO 2 (l)(10);
[0080] 2CO(g)+O 2 (g)→2CO 2 (g)(11);
[0081] Among them, 'l' means liquid, i.e. liquid state; 'g' means gas, i.e. gas state. The generated CO 2 Diffuses inward and reacts with C / SiC as an oxidant.
[0082] (12);
[0083] From this point on, the generated CO and SiO are further oxidized, and the amount of the products is different from the initial stage:
[0084] m 2 SiO(g)+(m 2 / 2)*O2(g)→m 2 SiO 2 (c)(13);
[0085] (2+m 2 )CO(g)+(1+m 2 / 2)O 2 (g)→(2+m 2 )CO 2 (g)(14);
[0086] In the formula (9), (13) and (14), the 'c' in '(c)' represents concentration. 2 As O 2 The carrier consumes the same amount as the initial stage (1+m 2 )Unit O 2 , extra m 2 Units of CO (or CO 2 ) escapes outward, the C element in the raw material is consumed, and similarly, m 2 Unit of condensed phase oxidation product SiO 2 , the Si element in the raw material is consumed. Combining equation (11) and equation (13), we can get:
[0087] (15);
[0088] ZrB as the main component of raw materials 2 The oxidation reaction is:
[0089] (16);
[0090] Solid ZrO 2 As the skeleton of the oxide layer, it is tightly bonded to the substrate, and because the products are not all of this kind, there must be some pores. 2 O 3 With SiO 2 Together they form borosilicate (a glassy substance) that fills the pores and covers the outermost surface. ZrB 2 The equilibrium constant for the oxidation reaction is:
[0091] (17);
[0092] Among them, the activity of solid matter is 1; is the dimensionless oxygen partial pressure, the first subscript identifies the component and the second subscript indicates the interface location where the reaction occurs.
[0093] ZrO 2 The porosity of the region f pore with ZrO 2 The phase transition point is closely related to the volume relationship of the oxide in the oxide layer, so the volume relationship of the oxide in the oxide layer is shown in the following expression:
[0094] (18);
[0095] In the formula, f cs is the volume fraction of C / SiC in the substrate (ie, the first volume fraction); f glassis the volume fraction of borosilicate in the oxide layer (i.e., the second volume fraction); ZrO in the oxide layer 2 The volume fraction of (that is, the third volume fraction) is .
[0096] SiO 2 -B 2 O 3 As an ideal liquid mixture, its activity is 1, and the activities of each component are based on the matrix components SiC and ZrB 2 The retreat rate is described by:
[0097] (19);
[0098] In the formula, SiO 2 activity; B 2 O 3 Activity; R SiC is the retreat amount of SiC component; V SiC is the volume of the SiC component participating in the reaction.
[0099] Regarding the internal depletion layer flow rate relationship analysis, the depletion layer is located in the raw material (that is, the C-SiC-ZrB 2 The oxygen partial pressure is very low here. 2 CO 2 The product CO and SiO diffuse outwards and reach the entrance of the depletion layer. 2 Reaction to generate CO 2 and SiO 2 According to formula (13), SiO 2 The equilibrium constant of the reaction.
[0100] (20);
[0101] In the formula, SiO 2 Reaction equilibrium constant; is the dimensionless pressure of SiO at position i2; O at position i2 2 The dimensionless pressure of CO reaction is calculated according to formula (11):
[0102] (twenty one);
[0103] In the formula, is the CO reaction equilibrium constant; CO at position i22 The dimensionless pressure of is the dimensionless pressure of CO at position i2. The SiC reaction equilibrium constant is calculated according to formula (12):
[0104] (twenty two);
[0105] In the formula, is the SiC reaction equilibrium constant; is the dimensionless pressure of SiO at position i1; is the dimensionless pressure of CO at position i1; CO at position i1 2 The dimensionless pressure of is the activity of SiC reaction at position i1. According to the chemical reaction stoichiometry of formula (12), CO and CO 2 According to the chemical reaction stoichiometry of formula (15), SiO and O 2 The flow rate relationship between each other:
[0106] (twenty three);
[0107] In the formula, is the flow rate of CO in area 12; is the flow rate of SiO in region 12; For CO 2 flow rate in zone 12; O 2 The flow rate in region 23. The negative sign indicates that the two components diffuse in opposite directions. If outward diffusion is positive and inward diffusion is negative, then CO, SiO and CO 2 The relationship between the flow rate and the partial pressure at both ends of the cavity is:
[0108] (twenty four);
[0109] in, For CO 2 flow rate in zone 12; For area 12, CO 2 The diffusion coefficient of ; R is the universal gas constant; T is the surface temperature of the material; CO at position i2 2 pressure; CO at position i1 2 Pressure; D CO-12 is the diffusion coefficient of CO in region 12; D SiO-12 is the diffusion coefficient of SiO in region 12; P CO-i2 is the pressure of CO at position i2; P CO-i1is the pressure of CO at position i1; P SiO-i2 is the pressure of SiO at position i2; P SiO-i1 is the pressure of SiO at position i1. The second subscript of the flux and diffusion coefficient refers to the area between the interfaces.
[0110] In the depletion layer, it is necessary to determine the gaseous components (CO, CO 2 , SiO) pressure, according to equations (17), (20) to (24), solve in the following order:
[0111] (25);
[0112] In the formula, at this time and l 12 is the unknown quantity, For area 23 O 2 Flow rate; O at position i2 2 The dimensionless pressure of for ZrO 2 The activity of the generating reaction; B at position i2 2 O 3 The activity of the generating reaction; ZrB 2 The activity of the oxidation reaction; ZrB 2 The equilibrium constant of an oxidation reaction; is the dimensionless pressure of SiO at position i2; SiO 2 The activity of the generating reaction; is the activity of SiO oxidation reaction; is O at position i2 2 pressure; is the dimensionless pressure of SiO at position i1; is the dimensionless pressure of SiO at position i2; is the dimensionless pressure of CO at position i1; CO in area 12 2 The diffusion coefficient of is the equilibrium constant of CO oxidation reaction; O at position i2 2 The dimensionless pressure of is the activity of SiC oxidation reaction at position i1; SiC and CO 2 The equilibrium constant of a reaction; is the dimensionless pressure of SiO at position i2; CO at position i12 The dimensionless pressure of is the dimensionless pressure of CO at position i2; CO at position i2 2 The dimensionless pressure.
[0113] Regarding the evolution analysis of the solid oxide layer, this layer is mainly ZrO 2 Solid oxide, it has many winding interconnected pores filled with glassy SiO 2 -B2O 3 Substance, O 2 The oxygen flow rate in the region 23 between interfaces i2 and i3 and in the region a3 between i3 and a is , They are:
[0114] (26);
[0115] In the formula, O 2 In SiO 2 -B 2 O 3 The permeability coefficient in O 2 SiO in region 3a 2 -B 2 O 3 The permeability coefficient in O 2 The pressure at position a; O 2 The pressure at position i3. = , we can get:
[0116] (27);
[0117] in, O 2 Pressure at position i3. Dissolved in SiO 2 -B 2 O 3 O 2 Consumed along two pathways: one part oxidizes SiO / CO; the other part oxidizes ZrB 2 . Solid oxide layer ZrO 2 Thickness change rate, ZrB 2 And the retreat rate of SiC is:
[0118] (28);
[0119] Where t is time; R S represents the amount of retreat. The depletion layer thickness is ZrB 2 The difference between the retreat amount of SiC and SiC.
[0120] About Low Temperature Surface SiO 2 -B 2 O 3 Analysis of glass layer evolution shows that under conditions of lower temperature and lower flow rate, the surface glass layer can be maintained, e.g. Figure 3 As shown in the figure, the thickness of the surface glass material changes with time. 2 and B 2 O 3 The generation rate and surface evaporation loss rate of ZrO and the filling growth 2 Porosity determination.
[0121] (29);
[0122] In the equations, the subscript “vap” indicates evaporation; l specimen is the length of the sample; μ is the viscosity of the ambient fluid; ρ is the density of the ambient fluid; v is the velocity of the ambient fluid. The thickness of the concentration boundary layer is closely related to the volatilization of the component; J speces-vap is the component evaporation flow rate; For B 2 O 3 Evaporation flow rate of the component; D speces is the diffusion coefficient of the component; P speces-vap is the evaporation pressure of the component; δ bdry is the concentration boundary layer thickness; v fluid is the dynamic viscosity coefficient of the liquid; ρ fluid is the liquid density; μ fluid is the viscosity coefficient of the liquid; SiO 2 evaporation rate.
[0123] The viscosity of the surface glass will limit the maximum thickness l that the outer glass material can support under the action of gravity. 3a-max According to the theory of liquid film falling, under laminar flow, this finite thickness is:
[0124] (30);
[0125] In the formula, the subscript "B 2 O 3 -SiO 2 ” indicates the borosilicate present in the surface region 3-a; SiO 2 -B 2 O 3 The molar mass of the mixture; B per unit area 2 O 3 -SiO 2 The rate of change of For B 2 O 3 -SiO 2 The viscosity coefficient; SiO 2 -B 2 O 3 The density of the mixture; g is the acceleration due to gravity; sin(φ) is the sine of the angle between the oxidation surface of the sample and the vertical direction.
[0126] Net weight gain gain , oxygen consumption, evaporation W evap They are as follows:
[0127] (31);
[0128] Where W g is the net change in sample mass; is oxygen consumption; W evap is the evaporation amount, the gaseous substance evaporates.
[0129] Regarding the evolution analysis of high temperature liquid-solid oxide layer, for high temperature and / or high flow rate of ambient fluid, SiO 2 The evaporation rate of (g) and / or SiO(g) is very high, the glassy layer on the surface will be lost, and the glassy liquid area will retreat to the area 2-3, such as Figure 4 Using 3i to identify the position of the receding glass layer, the oxygen flow balance will determine the oxygen partial pressure at the interface i3i at position 3i , , as shown below:
[0130] (32);
[0131] because , then we can get:
[0132] (33);
[0133] Gaseous components (SiO 2 , B 2 O 3 The diffusion flow of SiO determines the retreat rate of the interface i3i. The ratio of the thickness of the glassy material layer to the thickness of region 2-3 is denoted as b, and its evolution over time is:
[0134] (34);
[0135] The right side of the evolution equation is B 2 O 3 and SiO 2 The last term takes into account the increase in l with time increments. 23 . The negative sign in the equation takes the flow direction into consideration. The ceramic weight gain is as follows:
[0136] (35);
[0137] In addition, regarding the non-depletion layer oxidation model, the ZrB 2 Modeling of C / SiC oxidation with medium or low content in base ceramics. For high SiC content, SiC depletion layer is not easy to appear, so the modeling method is different from the previous case. According to the application, only the modeling of the surface layer with borosilicate is given here, such as Figure 5 As shown in Figure 1, the case of retreat into a solid oxide layer can be modeled similarly. Oxygen dissolves in the surface borosilicate, diffuses through it, and finally penetrates through the pores to reach the substrate below the oxide layer, oxidizing the C / SiC / ZrB 2 The reaction of C / SiC can be expressed as:
[0138] (36);
[0139] The consumption rate of C / SiC and O 2 The flow relationship is:
[0140] (37);
[0141] ZGar 2 The oxidation is still in equation (16), and the consumption rate can be expressed as the oxygen flow rate relationship:
[0142] (38);
[0143] The disappearance of the hole area, i.e. 12 = 0, which means that interfaces i1 and i2 coincide. To maintain consistency with the previous model, the symbol 2(1) is used here. When there is no SiC depletion layer, the modeling of the solid-liquid oxide layer is different from the previous model. Then the oxygen flow in region 2(1)3 between interfaces i2(i1) and i3 and region a3 between i3 and a is , They are:
[0144] (39);
[0145] Same reason , then we can get;
[0146] (40);
[0147] The oxygen that enters the material reacts with the substrate and is consumed, that is:
[0148] (41);
[0149] Under oxygen erosion, C / SiC and ZrB 2 Equal cross-section retreat, that is , then:
[0150] (42);
[0151] Oxide layer thickness and the substrate retreat amounts are:
[0152] (43);
[0153] In the formula, R substrate is the amount of substrate retreat. The thickness of the surface glassy material evolves with time as follows:
[0154] (44);
[0155] Net weight gain, oxygen consumption and evaporation are
[0156] (45).
[0157] Furthermore, regarding the criterion for the presence or absence of a depletion layer, when the ceramic contains a high content of SiC, no SiC depletion layer is formed. The criterion for the minimum SiC content is: If there is a SiC depletion layer, then the equal sign of equation (42) should be a greater than sign, and the equation can be transformed into:
[0158] (46);
[0159] Assuming that the oxygen flow rate is proportional to the reaction rate constant and exposure area of the components, equation (1) can be obtained after conversion.
[0160] In summary, the theoretical formula derived above is universal and can cover the same type of materials with different components. The universal relationship given in this embodiment determines the ablation retreat and mass loss of ceramic materials. Figure 6As shown in the figure, the oxidation weight gain (WeightGain) evaluated by different methods (Talmy test data, Parthasarathy, Zshuguang) was recorded at different temperatures (1473K, 1573K, 1773K) for 2h and at different SiC component content (Volume) percentages. It can be seen that this method (i.e. Figure 6 Zshuguang in the paper has the advantages of high calculation accuracy, low cost, short cycle and easy operation. In addition, it should be understood that if HfB 2 Component replacement of ZrB in ceramics 2 components, the above evaluation method has not been substantially modified, that is, the technical solution described in this method is also applicable to C-SiC-HfB 2 ceramics.
[0161] See also Figure 7 As shown, the embodiment of the present application also discloses a device for evaluating the anti-ablation performance of ultra-high temperature ceramics, including:
[0162] The ratio information acquisition module 11 is used to obtain the ratio information of C-SiC-ZrB 2 The component ratio information corresponding to the ceramic; wherein the component ratio information is C component, SiC component and ZrB 2 The ratio information of the components;
[0163] The porosity acquisition module 12 is used to determine the porosity of the C-SiC-ZrB after oxidation in a preset high-temperature oxygen environment based on the component ratio information. 2 The porosity of the surface oxide film of the ceramic;
[0164] The depletion layer judgment module 13 is used to judge the depletion layer of the oxidized C-SiC-ZrB based on the porosity and the preset depletion layer judgment rule. 2 Whether there is a silicon carbide depletion layer between the ceramic and the oxide to obtain the corresponding judgment result;
[0165] A mathematical model building module 14 is used to build a corresponding mathematical model according to the judgment result and the corresponding environmental conditions to obtain a corresponding ablation calculation model;
[0166] The parameter calculation module 15 is used to determine the C-SiC-ZrB 2 The ablation characteristic parameters corresponding to the ceramic are used to complete the corresponding ceramic anti-ablation performance evaluation operation; wherein the ablation characteristic parameters include the corresponding oxide layer thickness, ceramic retreat amount and ceramic weight gain.
[0167] Among them, for more specific working processes of the above-mentioned modules, please refer to the corresponding contents disclosed in the aforementioned embodiments, which will not be repeated here.
[0168] It can be seen that this application is first based on C-SiC-ZrB 2 The porosity of the oxide layer is determined based on the composition ratio information of the ceramic, and then the presence or absence of a silicon carbide depletion layer is determined. Then, the corresponding ablation calculation model is determined based on the judgment result and environmental conditions, and the ablation calculation model is used to obtain the C-SiC-ZrB 2 The corresponding oxide layer thickness, ceramic retreat and ceramic weight gain of the ceramic are used to complete the corresponding anti-ablation performance evaluation operation. In this way, the current problem of determining the anti-ablation performance of ceramic materials under service conditions by direct measurement is effectively solved, and the accuracy and efficiency of performance evaluation are improved, thereby improving the efficiency of high-speed aircraft thermal protection structure design and analysis, and greatly saving manpower, financial and material resources.
[0169] In some specific embodiments, the depletion layer determination module 13 may specifically include:
[0170] A threshold value acquisition unit is used for obtaining a threshold value based on the porosity and the C-SiC-ZrB 2 The mole fraction of SiC in the ceramic is calculated using a preset judgment formula to obtain a corresponding target threshold;
[0171] A judgment result acquisition unit is used to judge the C-SiC-ZrB 2 Whether the first volume fraction of C / SiC in the ceramic is greater than the target threshold value, so as to obtain a corresponding judgment result.
[0172] In some specific embodiments, the mathematical model building module 14 may specifically include:
[0173] A first model building unit, configured to determine the presence of a silicon carbide depletion layer when the judgment result indicates that the first volume fraction is not greater than the target threshold, and to build a high-temperature solid-state hybrid layer model or a low-temperature surface glass layer model under corresponding conditions by selecting corresponding environmental conditions;
[0174] The second model building unit is used to determine that the silicon carbide depletion layer does not exist when the judgment result indicates that the first volume fraction is greater than the target threshold, and to construct a high-temperature solid-state mixed layer model or a low-temperature surface glass layer model under corresponding conditions by selecting corresponding environmental conditions to obtain a corresponding ablation calculation model.
[0175] In some specific embodiments, the first model building unit may specifically include:
[0176] The first model building subunit is used to build a mathematical model by performing corresponding thermochemical reaction analysis, internal depletion layer flow rate relationship analysis, solid oxide layer evolution analysis, high temperature liquid-solid oxide layer evolution analysis or low temperature surface SiO 2 -B 2 O 3 The glass layer evolution is analyzed, and a formula is derived based on the first volume fraction, the porosity, and the mole fraction corresponding to the SiC to obtain the corresponding ablation calculation model.
[0177] In some specific embodiments, the parameter calculation module 15 may specifically include:
[0178] A volume fraction acquisition unit is used to calculate the oxidized C-SiC-ZrB based on the porosity, the mole fraction corresponding to the SiC, and the first volume fraction. 2 Borosilicate and ZrO in the oxide layer of ceramics 2 , to obtain the corresponding second volume fraction and third volume fraction;
[0179] The performance evaluation completion unit is used to determine the performance of the C-SiC-ZrB based on the ablation calculation model, the second volume fraction and the third volume fraction. 2 The corresponding oxide layer thickness, ceramic retreat amount and ceramic weight gain of the ceramic are used to complete the corresponding ceramic anti-ablation performance evaluation operation.
[0180] In some specific embodiments, the performance evaluation completion unit may specifically include:
[0181] a thickness calculation subunit, for performing corresponding solid oxide thickness calculation and surface glassy material thickness calculation by using the ablation calculation model, the second volume fraction and the third volume fraction when the ablation calculation model is a high-temperature solid mixed layer model, so as to obtain corresponding first thickness and second thickness;
[0182] The oxide layer thickness determination unit is used to combine the first thickness and the second thickness to obtain the corresponding oxide layer thickness.
[0183] Furthermore, the present application also discloses an electronic device. Figure 8 This is a structural diagram of an electronic device 20 according to an exemplary embodiment. The content in the diagram cannot be regarded as any limitation on the scope of use of the present application.
[0184] Figure 8A schematic diagram of the structure of an electronic device 20 provided in an embodiment of the present application. The electronic device 20 may specifically include: at least one processor 21, at least one memory 22, a power supply 23, a communication interface 24, an input / output interface 25, and a communication bus 26. The memory 22 is used to store a computer program, which is loaded and executed by the processor 21 to implement the relevant steps in the method for evaluating the anti-ablation performance of ultra-high temperature ceramics disclosed in any of the aforementioned embodiments. In addition, the electronic device 20 in this embodiment may specifically be an electronic computer.
[0185] In this embodiment, the power supply 23 is used to provide working voltage for each hardware device on the electronic device 20; the communication interface 24 can create a data transmission channel between the electronic device 20 and the external device, and the communication protocol it follows is any communication protocol that can be applied to the technical solution of the present application, and is not specifically limited here; the input and output interface 25 is used to obtain external input data or output data to the outside world, and its specific interface type can be selected according to specific application needs and is not specifically limited here.
[0186] In addition, the memory 22, as a carrier for storing resources, can be a read-only memory, a random access memory, a disk or an optical disk, etc. The resources stored thereon can include an operating system 221, a computer program 222, etc., and the storage method can be temporary storage or permanent storage.
[0187] The operating system 221 is used to manage and control the hardware devices and computer program 222 on the electronic device 20, and can be Windows Server, Netware, Unix, Linux, etc. In addition to the computer program that can be used to complete the ultra-high temperature ceramic ablation resistance performance evaluation method performed by the electronic device 20 disclosed in any of the aforementioned embodiments, the computer program 222 can further include computer programs that can be used to complete other specific tasks.
[0188] Furthermore, the present application also discloses a computer-readable storage medium for storing a computer program; wherein, when the computer program is executed by a processor, the aforementioned ultra-high temperature ceramic ablation resistance evaluation method disclosed above is implemented. The specific steps of the method can be referred to the corresponding contents disclosed in the aforementioned embodiments, and will not be repeated here.
[0189] In this specification, each embodiment is described in a progressive manner, and each embodiment focuses on the differences from other embodiments. The same or similar parts between the embodiments can be referred to each other. For the device disclosed in the embodiment, since it corresponds to the method disclosed in the embodiment, the description is relatively simple, and the relevant parts can be referred to the method part.
[0190] Professionals may further appreciate that the units and algorithm steps of each example described in conjunction with the embodiments disclosed herein can be implemented in electronic hardware, computer software, or a combination of the two. In order to clearly illustrate the interchangeability of hardware and software, the composition and steps of each example have been generally described in the above description according to function. Whether these functions are performed in hardware or software depends on the specific application and design constraints of the technical solution. Professionals and technicians may use different methods to implement the described functions for each specific application, but such implementation should not be considered to be beyond the scope of this application.
[0191] The steps of the method or algorithm described in conjunction with the embodiments disclosed herein may be implemented directly using hardware, a software module executed by a processor, or a combination of the two. The software module may be placed in a random access memory (RAM), a memory, a read-only memory (ROM), an electrically programmable ROM, an electrically erasable programmable ROM, a register, a hard disk, a removable disk, a CD-ROM, or any other form of storage medium known in the art.
[0192] Finally, it should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise a ..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0193] The technical solution provided by the present application is introduced in detail above. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the method of the present application and its core idea. At the same time, for general technicians in this field, according to the idea of the present application, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present application.
Claims
1. A method for evaluating the anti-ablation performance of ultra-high temperature ceramics, characterized in that: include: Acquire component ratio information corresponding to C-SiC-ZrB2 ceramics; wherein the component ratio information is ratio information of C component, SiC component and ZrB2 component; Determine the porosity of the surface oxide film of the C-SiC-ZrB2 ceramic after oxidation in a preset high-temperature aerobic environment based on the component ratio information; Based on the porosity and the preset depletion layer judgment rule, it is judged whether there is a silicon carbide depletion layer between the oxidized C-SiC-ZrB2 ceramic and the oxide to obtain a corresponding judgment result; Constructing a corresponding mathematical model according to the judgment result and the corresponding environmental conditions to obtain a corresponding ablation calculation model; Determine the ablation characteristic parameters corresponding to the C-SiC-ZrB2 ceramic based on the ablation calculation model to complete the corresponding ceramic anti-ablation performance evaluation operation; wherein the ablation characteristic parameters include the corresponding oxide layer thickness, ceramic retreat amount and ceramic weight gain; Wherein, judging whether there is a silicon carbide depletion layer between the oxidized C-SiC-ZrB2 ceramic and the oxide based on the porosity and the preset depletion layer judgment rule to obtain a corresponding judgment result includes: Calculating based on the porosity, the mole fraction corresponding to SiC in the C-SiC-ZrB2 ceramic, and a preset determination formula to obtain a corresponding target threshold; Determine whether the first volume fraction of C / SiC in the C-SiC-ZrB2 ceramic is greater than the target threshold value to obtain a corresponding determination result; The corresponding mathematical model is constructed according to the judgment result and the corresponding environmental conditions to obtain the corresponding ablation calculation model, including: When the judgment result shows that the first volume fraction is not greater than the target threshold, it is determined that a silicon carbide depletion layer exists, and a high-temperature solid-state hybrid layer model or a low-temperature surface glass layer model is constructed under corresponding conditions by selecting corresponding environmental conditions; When the judgment result indicates that the first volume fraction is greater than the target threshold, it is determined that the silicon carbide depletion layer does not exist, and a high-temperature solid-state mixed layer model or a low-temperature surface glass layer model is constructed under corresponding conditions by selecting corresponding environmental conditions to obtain a corresponding ablation calculation model; The method of selecting corresponding environmental conditions to construct a high-temperature solid mixed layer model or a low-temperature surface glass layer model under corresponding conditions includes: In the process of constructing the mathematical model, the corresponding thermochemical reaction analysis, internal depletion layer flow rate relationship analysis, solid oxide layer evolution analysis, high temperature liquid-solid oxide layer evolution analysis or low temperature surface SiO2-B2O3 glass layer evolution analysis are carried out, and the formula is derived based on the first volume fraction, the porosity and the mole fraction corresponding to the SiC to obtain the corresponding ablation calculation model.
2. The method for evaluating the anti-ablation performance of ultra-high temperature ceramics according to claim 1, characterized in that: The step of determining the ablation characteristic parameters corresponding to the C-SiC-ZrB2 ceramic based on the ablation calculation model to complete the corresponding ceramic ablation resistance performance evaluation operation includes: Calculating the volume fractions of borosilicate and ZrO2 in the oxide layer of the oxidized C-SiC-ZrB2 ceramic based on the porosity, the molar fraction corresponding to the SiC, and the first volume fraction to obtain corresponding second volume fractions and third volume fractions; Based on the ablation calculation model, the second volume fraction and the third volume fraction, the oxide layer thickness, ceramic retreat amount and ceramic weight gain corresponding to the C-SiC-ZrB2 ceramic are determined to complete the corresponding ceramic ablation resistance evaluation operation.
3. The method for evaluating the anti-ablation performance of ultra-high temperature ceramics according to claim 2, characterized in that: The step of determining the oxide layer thickness corresponding to the C-SiC-ZrB2 ceramic based on the ablation calculation model, the second volume fraction, and the third volume fraction comprises: When the ablation calculation model is a high-temperature solid mixed layer model, the corresponding solid oxide thickness calculation and surface glassy material thickness calculation are performed through the ablation calculation model, the second volume fraction, and the third volume fraction to obtain the corresponding first thickness and second thickness; The first thickness and the second thickness are combined to obtain the corresponding oxide layer thickness.
4. An ultra-high temperature ceramic ablation resistance evaluation device, characterized in that: include: A ratio information acquisition module, used to acquire component ratio information corresponding to the C-SiC-ZrB2 ceramic; wherein the component ratio information is the ratio information of the C component, the SiC component and the ZrB2 component; A porosity acquisition module, used to determine the porosity of the surface oxide film of the C-SiC-ZrB2 ceramic after oxidation in a preset high-temperature aerobic environment based on the component ratio information; A depletion layer judgment module, used to judge whether there is a silicon carbide depletion layer between the oxidized C-SiC-ZrB2 ceramic and the oxide based on the porosity and a preset depletion layer judgment rule, so as to obtain a corresponding judgment result; A mathematical model building module, used to build a corresponding mathematical model according to the judgment result and the corresponding environmental conditions to obtain a corresponding ablation calculation model; A parameter calculation module, used to determine the ablation characteristic parameters corresponding to the C-SiC-ZrB2 ceramic based on the ablation calculation model, so as to complete the corresponding ceramic anti-ablation performance evaluation operation; wherein the ablation characteristic parameters include the corresponding oxide layer thickness, ceramic retreat amount and ceramic weight gain; Wherein, the depletion layer judgment module includes: A threshold value acquisition unit, used to calculate based on the porosity, the mole fraction corresponding to SiC in the C-SiC-ZrB2 ceramic and a preset determination formula to obtain a corresponding target threshold value; A judgment result acquisition unit, used to judge whether the first volume fraction of C / SiC in the C-SiC-ZrB2 ceramic is greater than the target threshold value, so as to obtain a corresponding judgment result; The mathematical model building module comprises: A first model building unit, configured to determine the presence of a silicon carbide depletion layer when the judgment result indicates that the first volume fraction is not greater than the target threshold, and to build a high-temperature solid-state hybrid layer model or a low-temperature surface glass layer model under corresponding conditions by selecting corresponding environmental conditions; A second model building unit is configured to determine that the silicon carbide depletion layer does not exist when the judgment result indicates that the first volume fraction is greater than the target threshold, and to select corresponding environmental conditions to perform high-temperature solid-state mixed layer model building or low-temperature surface glass layer model building under corresponding conditions to obtain a corresponding ablation calculation model; The first model building unit comprises: The first model building subunit is used to derive a formula based on the first volume fraction, the porosity and the mole fraction corresponding to the SiC to obtain the corresponding ablation calculation model during the mathematical model construction by performing corresponding thermochemical reaction analysis, internal depletion layer flow rate relationship analysis, solid oxide layer evolution analysis and high temperature liquid-solid oxide layer evolution analysis or low temperature surface SiO2-B2O3 glass layer evolution analysis.
5. The ultra-high temperature ceramic ablation resistance evaluation device according to claim 4, characterized in that: The depletion layer judgment module comprises: A threshold value acquisition unit, used to calculate based on the porosity, the mole fraction corresponding to SiC in the C-SiC-ZrB2 ceramic and a preset determination formula to obtain a corresponding target threshold value; The judgment result acquisition unit is used to judge whether the first volume fraction of C / SiC in the C-SiC-ZrB2 ceramic is greater than the target threshold value to obtain a corresponding judgment result.
6. An electronic device, characterized in that: include: Memory, used to store computer programs; A processor, configured to execute the computer program to implement the method for evaluating the anti-ablation performance of ultra-high temperature ceramics as claimed in any one of claims 1 to 3.
7. A computer-readable storage medium, characterized in that: Used to store a computer program, which, when executed by a processor, implements the method for evaluating the anti-ablation performance of ultra-high temperature ceramics as described in any one of claims 1 to 3.