Preparation method of non-aqueous lithium ion battery electrolyte additive

By carrying out a constant temperature reaction in a dry reactor and using distillation and beating purification processes, the problems of using highly toxic chemicals and harsh conditions in the existing technology are solved, and efficient and safe diallyl phosphate and diphosphate diphosphate are achieved. The preparation of propargyl ester salt, triallyl phosphate and triacetylenyl phosphate is suitable for industrial production.

CN118867386APending Publication Date: 2024-10-29SUZHOU DEGAS ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410895813.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The preparation methods of diallyl phosphate, dipropargyl phosphate, triallyl phosphate and tripropargyl phosphate in the prior art involve the reaction of highly toxic chemicals allyl alcohol/propargyl alcohol and phosphorus oxychloride, Hydrogen chloride waste gas is produced, the reaction conditions are harsh, the yield is low, and the product purity is low, making it unsuitable for industrial production.

Method used

A method for preparing non-aqueous lithium ion battery electrolyte additives is adopted, by adding phosphate ester salt or its derivatives and solvent in a dry reactor, controlling the reaction temperature at 80°C to 150°C, and performing a constant temperature reaction for 6 to 12 hours. Use distillation and beating purification processes to avoid highly toxic raw materials, simplify the process, and improve purity and conversion rate.

Benefits of technology

The reaction without using hazardous chemicals is realized, the reaction conversion rate and product purity are improved, and the process flow is simplified, so that the prepared diallyl phosphate salt, dipropargyl phosphate salt, triallyl phosphate and triyne phosphate are prepared Pi ester is more suitable for industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to a preparation method of a non-aqueous lithium ion battery electrolyte additive, which comprises the following steps: reacting phosphate salt, an allyl ester derivative, a propargyl ester derivative and a solvent in a reactor provided with a rectification device at the temperature of 80-150 DEG C to generate diallyl phosphate salt or tripropargyl phosphate salt, pulping and purifying; the method comprises the following steps: carrying out a reaction on phosphate, an allyl ester derivative or a propargyl ester derivative in a reactor provided with a rectification device to generate triallyl phosphate or tripropargyl phosphate, and carrying out rectification and purification; the method provided by the invention uses few raw materials, does not involve dangerous chemicals, and is safe in reaction process and simple to operate; the method has the advantages of high reaction conversion rate, few impurities in the material obtained after the reaction, the diallyl phosphate salt and the dipropargyl phosphate salt are powdery solids, the boiling points of the triallyl phosphate and the tripropargyl phosphate are greatly different from the boiling points of other substances in the system, and the method is easy to separate and purify and suitable for industrial production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of lithium ion battery electrolyte additives, and in particular to a method for preparing a non-aqueous lithium ion battery electrolyte additive. Background Art

[0002] Lithium-ion batteries have significant advantages such as low energy consumption, high specific capacity and specific energy, high operating voltage, long cycle life, low self-discharge, environmental friendliness, good cycle performance, and long life. They are widely used in portable electronic devices such as laptops, mobile phones, cameras, and mining lamps. With the increasing demand for environmentally friendly, safe and stable power sources and the development of electric vehicles, lithium-ion batteries, as green, environmentally friendly and high-energy batteries, have been more widely used.

[0003] Diallyl phosphate, dipropargyl phosphate, triallyl phosphate and tripropargyl phosphate are four new electrolyte additives for non-aqueous lithium-ion batteries. The electrolyte containing diallyl phosphate, dipropargyl phosphate, triallyl phosphate or tripropargyl phosphate helps to form a stable and dense SEI film on the electrode surface, preventing further decomposition of solvent molecules, significantly improving coulombic efficiency, and maintaining high capacity after long-term cycling.

[0004] Diallyl phosphate salts, diallyl phosphate salts, triallyl phosphate and tripropargyl phosphate are used in high-nickel ternary lithium battery systems, which can effectively inhibit the decomposition of the electrolyte at the positive electrode and the dissolution of metal ions such as manganese and cobalt. They can form films on the positive and negative electrodes, effectively improve the high-temperature storage and cycle performance of the ternary lithium battery, and improve the safety performance of the battery.

[0005] According to the public information of the prior art, the current preparation methods of triallyl phosphate and tripropargyl phosphate mainly use allyl alcohol or propargyl alcohol and phosphorus oxychloride in an organic solvent system, react under the action of an acid binding agent, and then filter and wash with water, dry, and distill to obtain the product. The preparation of diallyl phosphate salt and dipropargyl phosphate salt also requires the reaction of allyl alcohol or propargyl alcohol and phosphorus oxychloride. However, the defect of this method is that the raw material allyl alcohol / propargyl alcohol involved is a highly toxic chemical, the reaction produces a large amount of hydrogen chloride waste gas, etc., and the reaction conditions are relatively harsh. For example, in CN201710203013.2, the reaction conditions are below -30°C when phosphorus oxychloride is added dropwise. At the same time, the method has the disadvantages of low reaction yield and low product purity, and is not suitable for industrial production.

[0006] Therefore, a novel method for preparing diallyl phosphate salt, dipropargyl phosphate salt, triallyl phosphate and tripropargyl phosphate is currently needed to overcome the above-mentioned shortcomings and problems existing in the prior art, simplify the process, and be more suitable for industrial production of diallyl phosphate salt, dipropargyl phosphate salt, triallyl phosphate and tripropargyl phosphate. Summary of the invention

[0007] Technical problems to be solved: In view of the technical problems in the prior art that allyl alcohol / propargyl alcohol, the raw materials of diallyl phosphate salts, diallyl phosphate salts, triallyl phosphate and tripropargyl phosphate, are highly toxic chemicals, the reaction produces a large amount of hydrogen chloride waste gas, etc., and the reaction conditions are relatively harsh, the reaction yield is low, the product purity is low, and it is not suitable for industrial production, a method for preparing a non-aqueous lithium-ion battery electrolyte additive is provided, which does not involve highly toxic chemical raw materials, has a simple process and is easy to operate, and is more suitable for the industrial production of diallyl phosphate salts, diallyl phosphate salts, triallyl phosphate and tripropargyl phosphate.

[0008] The present application relates to a method for preparing a non-aqueous lithium-ion battery electrolyte additive, wherein the non-aqueous lithium-ion battery electrolyte additive is one or more of diallyl phosphate salt, dipropargyl phosphate salt, triallyl phosphate, and tripropargyl phosphate, and the specific steps include:

[0009] The first step is to add phosphate salt or phosphate ester, allyl ester derivative or propargyl ester derivative, and solvent into a dry reactor equipped with a distillation device and a stirring device;

[0010] Step 2: Under stirring, control the reaction temperature to 80°C to 150°C, control the temperature of the distillation tube to maintain at 60-100°C, and react at a constant temperature;

[0011] Step 3: After the reaction is completed, the product is purified by distillation or pulping to obtain diallyl phosphate salt, diallyl phosphate salt, triallyl phosphate or tripropargyl phosphate.

[0012] Furthermore, the diallyl phosphate salt or the diallyl phosphate salt is prepared by pulping and purifying after reacting an allyl ester derivative or a propargyl ester derivative, a phosphate salt and a solvent.

[0013] Furthermore, the triallyl phosphate or tripropargyl phosphate is obtained by reacting an allyl ester derivative or a propargyl ester derivative, a phosphate ester and a solvent, followed by distillation and purification.

[0014] Furthermore, the isothermal reaction time in the second step is 6 to 12 hours.

[0015] Furthermore, the molar ratio of the phosphate salt to the allyl derivative or the propargyl derivative is 1:2.1 to 1:2.5.

[0016] Furthermore, the molar ratio of the phosphate ester to the allyl derivative or the propargyl derivative is 1:3.1 to 1:3.5.

[0017] Furthermore, the phosphate ester salt is one or more of dimethyl phosphate lithium salt, dimethyl phosphate sodium salt, dimethyl phosphate potassium salt, diethyl phosphate lithium salt, diethyl phosphate sodium salt, diethyl phosphate potassium salt; the phosphate ester is trimethyl phosphate and / or triethyl phosphate; the allyl ester derivative is one or more of allyl hexanoate, allyl propionate, allyl acetate, allyl methacrylate, allyl acetoacetate, allyl phenoxyacetate; the propargyl ester derivative is one or more of propargyl acetate, propargyl benzoate, propargyl acrylate, propargyl methacrylate.

[0018] Furthermore, the solvent is one or more of N,N-dimethylformamide, N,N-diethylformamide, N-methylformamide, N-ethylformamide, dimethyl sulfoxide, tetramethylurea, 1,1-dimethylurea, and 1,3-dimethylurea.

[0019] Furthermore, the beating and purification in the third step is specifically to spin-dry the product, pulp the solid with 200 ml of dimethyl sulfoxide × 3 times, filter and wash it with 60 ml of dichloromethane × 3 times, and spin-dry again.

[0020] Furthermore, the distillation and purification in the third step is specifically to subject the product to vacuum distillation and collect fractions.

[0021] Beneficial effects:

[0022] 1. The method for preparing diallyl phosphate salt, dipropargyl phosphate salt, triallyl phosphate and tripropargyl phosphate in the present application uses a small variety of reaction raw materials, does not involve hazardous chemicals, and has a safe reaction process and simple operation;

[0023] 2. The reaction described in the present application has a high reaction conversion rate, and the product contains fewer impurities. Diallyl phosphate salt and dipropargyl phosphate salt are powdered solids at room temperature. The boiling points of triallyl phosphate (255±30°C) and tripropargyl phosphate (275±30°C) are quite different from the boiling points of other substances in the system. For example, the highest boiling point of the impurities in Example 3 of the present application is 197°C; the highest boiling point of the impurities in Example 4 is 215°C, which is easy to separate and purify, and is more suitable for industrial production;

[0024] 3. The product obtained by the reaction described in this scheme is more stable than the raw material, and the generated methyl / ethyl carboxylate has the lowest boiling point in the corresponding system and can be continuously evaporated during the reaction, which promotes the forward progress of the reaction from both thermodynamic and kinetic aspects and greatly improves the conversion rate. DETAILED DESCRIPTION

[0025] The following are only embodiments of the present invention, and are not intended to limit the scope of the present invention. The present invention can be implemented in different forms, and all contents made using the contents of the present invention specification are included in the scope of patent protection of the present invention. The embodiments are provided to make the contents disclosed in the present invention more thorough and comprehensive.

[0026] In the present invention, the temperature of the reaction between the phosphate salt or phosphate ester and the allyl ester derivative or propargyl ester derivative and the temperature of the distillation tube are usually determined according to the boiling points of the reactants and the products. Generally, the products are allowed to leave the system while the reactants are retained while ensuring sufficient temperature to promote the reaction. In the reaction of the phosphate salt or phosphate ester and the allyl ester derivative or propargyl ester derivative of the present invention, if the reaction temperature is lower than 80°C, the formation of diallyl phosphate in the reaction of phosphoric acid and a certain allyl ester is slow and the reaction time is long. However, if the reaction temperature is higher than 150°C, other impurities are generated.

[0027] The reaction time of the phosphate salt or phosphate ester and the allyl derivative or propargyl derivative is usually 6 to 12 hours, the molar ratio of the phosphate salt to the allyl derivative or propargyl derivative is 1:2.1 to 1:2.5, and the molar ratio of the phosphate ester to the allyl derivative or propargyl derivative is 1:3.1 to 1:3.5.

[0028] The phosphate salt is one or more of dimethyl phosphate lithium salt, dimethyl phosphate sodium salt, dimethyl phosphate potassium salt, diethyl phosphate lithium salt, diethyl phosphate sodium salt, diethyl phosphate potassium salt; the phosphate ester is trimethyl phosphate and / or triethyl phosphate; the allyl ester derivative is one or more of allyl hexanoate, allyl propionate, allyl acetate, allyl methacrylate, allyl acetoacetate, allyl phenoxyacetate; the propargyl ester derivative is one or more of propargyl acetate, propargyl benzoate, propargyl acrylate, propargyl methacrylate; the solvent is one or more of N,N-dimethylformamide, N,N-diethylformamide, N-methylformamide, N-ethylformamide, dimethyl sulfoxide, tetramethyl urea, 1,1-dimethylurea, 1,3-dimethylurea.

[0029] Example 1

[0030] A method for preparing lithium diallyl phosphate salt, comprising the following steps:

[0031] Step 1: Add 132 g (1 mol) of dimethyl phosphate lithium salt, 210.3 g (2.1 mol) of allyl acetate, 400 ml of N,N-diethylformamide, and 100 ml of 1,3-dimethylurea into a dry 1000 ml eggplant-shaped bottle equipped with a distillation device and a stirring device;

[0032] Step 2: Under stirring, control the reaction temperature to 90°C, control the temperature of the distillation tube to maintain at 60°C, and react at a constant temperature for 8 hours;

[0033] Step 3: After the reaction is completed, the solid is spin-dried, and the solid is pulped with 200 ml of dimethyl sulfoxide × 3 times, filtered and washed with 60 ml of dichloromethane × 3 times, and spin-dried to obtain 163.3 g of lithium diallyl phosphate salt with a product purity of 99.81%.

[0034] Example 2

[0035] A method for preparing dipropargyl phosphate potassium salt, comprising the following steps:

[0036] Step 1: Add 192.2 g (1 mol) of diethyl phosphate potassium salt, 215.9 g (2.2 mol) of propargyl acetate, 400 ml of N,N-dimethylformamide, and 100 ml of tetramethylurea into a dry 1000 ml eggplant-shaped bottle equipped with a distillation device and a stirring device;

[0037] Step 2: Under stirring, control the reaction temperature to 105°C, control the temperature of the distillation tube to maintain at 80°C, and react at a constant temperature for 9 hours;

[0038] Step 3: After the reaction is completed, the solid is spin-dried, and the solid is pulped with 200 ml of dimethyl sulfoxide × 3 times, filtered and washed with 60 ml of dichloromethane × 3 times, and spin-dried to obtain 173.3 g of potassium dipropargyl phosphate with a product purity of 99.87%.

[0039] Example 3

[0040] A method for preparing triallyl phosphate, comprising the following steps:

[0041] Step 1: Add 140.1 g (1 mol) of trimethyl phosphate and 376.7 g (3.3 mol) of allyl propionate into a dry 500 ml eggplant-shaped bottle equipped with a distillation device and a stirring device;

[0042] Step 2: Under stirring, control the reaction temperature to 115°C, control the temperature of the distillation tube to maintain at 100°C, and react at a constant temperature for 10 hours;

[0043] Step 3: After the reaction is completed, the obtained crude triallyl phosphate is subjected to vacuum distillation, and the 81-83°C / 0.1 mmHg fraction is collected to obtain 192.5 g of triallyl phosphate with a product purity of 99.82%.

[0044] Example 4

[0045] A method for preparing tripropargyl phosphate, comprising the following steps:

[0046] Step 1: Add 182.2 g (1 mol) of triethyl phosphate and 314 g (3.2 mol) of propargyl acetate into a dry 500 ml eggplant-shaped bottle equipped with a distillation device and a stirring device;

[0047] Step 2: Under stirring, control the reaction temperature to 100°C, control the temperature of the distillation tube to maintain at 60°C, and react at a constant temperature for 6 hours;

[0048] Step 3: After the reaction is completed, the obtained crude tripropargyl phosphate is subjected to vacuum distillation, and the 114-116°C / 0.5mmHg fraction is collected to obtain 192.5g of tripropargyl phosphate with a product purity of 99.82%.

[0049] The above is only an embodiment of the present invention. To avoid unnecessary repetition, the present invention will not repeat various possible combinations. However, it should be noted that all the specific features described in the present invention are within the scope of patent protection of the present invention.

Claims

1. A method for preparing a non-aqueous lithium-ion battery electrolyte additive, characterized in that: The non-aqueous lithium-ion battery electrolyte additive is one or more of diallyl phosphate salt, dipropargyl phosphate salt, triallyl phosphate, and tripropargyl phosphate, and the specific steps are as follows: The first step is to add phosphate salt or phosphate ester, allyl ester derivative or propargyl ester derivative, and solvent into a dry reactor equipped with a distillation device and a stirring device; Step 2: Under stirring, control the reaction temperature to 80°C to 150°C, control the temperature of the distillation tube to maintain at 60-100°C, and react at a constant temperature; Step 3: After the reaction is completed, the product is purified by distillation or pulping to obtain diallyl phosphate salt, diallyl phosphate salt, triallyl phosphate or tripropargyl phosphate.

2. The method for preparing a non-aqueous lithium ion battery electrolyte additive according to claim 1, characterized in that: The diallyl phosphate salt or the diallyl phosphate salt is prepared by pulping and purifying after reacting an allyl ester derivative or a propargyl ester derivative, a phosphate salt and a solvent.

3. The method for preparing a non-aqueous lithium-ion battery electrolyte additive according to claim 1, characterized in that: The triallyl phosphate or tripropargyl phosphate is prepared by distillation and purification after the reaction of an allyl ester derivative or a propargyl ester derivative, a phosphate ester and a solvent.

4. The method for preparing a non-aqueous lithium-ion battery electrolyte additive according to claim 1, characterized in that: The isothermal reaction time in the second step is 6 to 12 hours.

5. The method for preparing a non-aqueous lithium ion battery electrolyte additive according to claim 2, characterized in that: The molar ratio of the phosphate salt to the allyl derivative or the propargyl derivative is 1:2.1 to 1:2.

5.

6. The method for preparing a non-aqueous lithium-ion battery electrolyte additive according to claim 3, characterized in that: The molar ratio of the phosphate ester to the allyl derivative or the propargyl derivative is 1:3.1 to 1:3.

5.

7. The method for preparing a non-aqueous lithium-ion battery electrolyte additive according to claim 1, characterized in that: The phosphate ester salt is one or more of dimethyl phosphate lithium salt, dimethyl phosphate sodium salt, dimethyl phosphate potassium salt, diethyl phosphate lithium salt, diethyl phosphate sodium salt, diethyl phosphate potassium salt; the phosphate ester is trimethyl phosphate and / or triethyl phosphate; the allyl ester derivative is one or more of allyl hexanoate, allyl propionate, allyl acetate, allyl methacrylate, allyl acetoacetate, and allyl phenoxyacetate; the propargyl ester derivative is one or more of propargyl acetate, propargyl benzoate, propargyl acrylate, and propargyl methacrylate.

8. The method for preparing a non-aqueous lithium-ion battery electrolyte additive according to claim 1, characterized in that: The solvent is one or more of N,N-dimethylformamide, N,N-diethylformamide, N-methylformamide, N-ethylformamide, dimethyl sulfoxide, tetramethylurea, 1,1-dimethylurea, and 1,3-dimethylurea.

9. The method for preparing a non-aqueous lithium-ion battery electrolyte additive according to claim 1, characterized in that: The beating purification in the third step specifically comprises spinning the product to dryness, beating the solid with 200 ml of dimethyl sulfoxide × 3 times, filtering and washing it with 60 ml of dichloromethane × 3 times, and spinning it to dryness again.

10. The method for preparing a non-aqueous lithium-ion battery electrolyte additive according to claim 1, characterized in that: The distillation and purification in the third step specifically involves subjecting the product to vacuum distillation and collecting fractions.