Nano rare earth oxide and preparation method thereof

Through the complexation of organic acid ions and rare earth ions, the nucleation and crystal growth process of nano rare earth oxides are regulated, and the problem of difficult crystal growth in precipitation is solved, and the low-cost nano rare earth oxides suitable for industrial production are achieved. Prepared, the obtained product has good dispersion and purity.

CN118908263AInactive Publication Date: 2024-11-08BAOTOU RESEARCH INSTITUTE OF RARE EARTHS
View PDF 0 Cites 13 Cited by

Patent Information

Application Number
CN202410950754.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-08
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing precipitation method for preparing nano rare earth oxides has problems such as difficult to control the crystal growth process, high cost, low purity and difficult wastewater treatment, and it is difficult to be suitable for industrial production.

Method used

By introducing organic acid ions and rare earth ions to form organic rare earth ions, nucleation process and crystal growth are regulated, and a mixed solution of organic acid or organic acid salt solution and rare earth compounds are used to insulate and react with precipitant, and then calcination is performed to obtain nano rare earths Oxide.

Benefits of technology

The preparation of nano rare earth oxides with low cost, simple equipment and easy to operate is achieved. The average particle size of the obtained product is 20-100 nm, which is suitable for industrial production. It inhibits particle agglomeration through physical barriers, and improves the dispersion and purity of the product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118908263A_ABST
    Figure CN118908263A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of nano materials, in particular to a nano rare earth oxide and a preparation method thereof. According to the specific technical scheme, the preparation method of the nano rare earth oxide comprises the following steps: carrying out heat preservation reaction on a mixed solution of an organic acid or organic acid salt solution and a rare earth compound and a precipitator, filtering, washing, drying and calcining to obtain the nano rare earth oxide. According to the preparation method provided by the invention, the organic acid radical ions are introduced to be complexed with the rare earth ions to form the organic rare earth coordination ions by regulating and controlling the preparation of the solution and the feeding mode of each raw material, so that the nucleation process is accelerated, and the crystal growth process is regulated and controlled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of nano materials, and in particular to a nano rare earth oxide and a preparation method thereof. Background Art

[0002] Nanomaterials have many excellent properties, such as quantum size effect, small size effect, surface and interface effect, and macro quantum tunneling effect. These excellent properties make them widely used in electricity, optics, biology, and medicine. Rare earth elements have become a hot topic of research due to their unique 4f electronic structure. They are used in luminescence, polishing, magnetic material catalysis, and other fields. They are also widely used in high-tech fields such as ceramics, superconductors, and laser materials. They are considered to be a treasure trove of new light sources, new magnetic sources, new energy, and new materials. They are also "vitamins" for transforming traditional industries and improving traditional products. Nano rare earth materials have the properties of both nano materials and rare earth compounds, and can greatly improve the performance of materials.

[0003] The methods for preparing nano rare earth oxides mainly include solid phase synthesis, hydrothermal synthesis, sol-gel method, spray pyrolysis, microemulsion method and precipitation method. The particle size and dispersibility of the products produced by the solid phase synthesis method are difficult to meet the requirements. Although high-quality nano products can be prepared by hydrothermal method, sol-gel method, spray pyrolysis method, microemulsion method, etc., they are difficult to mass produce due to high cost, low efficiency, long cycle and other problems. So far, precipitation method is still the best choice for preparing nano oxide powder. Precipitation method can control the chemical composition of materials very accurately, and the cost of raw materials is low, the requirements for equipment are also low, the process is simple, the operation is convenient, and the surface activity and purity of the obtained products are high. However, the precipitation method is difficult to control the speed of forming crystal nuclei during precipitation, and the crystal growth process needs to be precisely controlled. Therefore, it is difficult to prepare nano rare earth compounds with specific morphology and particle size.

[0004] At present, there are some patent reports on the use of precipitation method to prepare nano rare earth oxides. In Chinese invention patent CN108975378A, a mixed solution is formed by adding a composite dispersant to a carbonate solution, and the mixed solution is reversely added dropwise to a dysprosium-containing liquid for post-treatment to prepare a small-particle dysprosium oxide powder. The addition of a variety of alcohols and polymer dispersants during the preparation process of this method will bring about a series of problems such as low purity of dysprosium oxide and difficulty in wastewater treatment, which is not suitable for industrial production. Chinese invention patent CN108083316A uses rare earth salts, precipitants and betaine-type surfactants as raw materials to prepare nano rare earth oxides. The method introduces surfactants to prepare nano rare earth oxide products with low purity and high cost. Therefore, it is necessary to develop a method for preparing rare earth nanomaterials with a controllable crystal growth process, low cost and mass production by precipitation method. Summary of the invention

[0005] In view of the shortcomings of the prior art, the present invention provides a nano rare earth oxide and a preparation method thereof, wherein the method introduces organic acid radical ions to form organic rare earth complex ions by regulating the configuration of the solution and the feeding method of each raw material, so as to accelerate the nucleation process and regulate the crystal growth process. The organic rare earth complex ions play a physical barrier role to inhibit the agglomeration between particles, and at the same time inhibit the growth of the nano rare earth oxide precursor, thereby obtaining a granular rare earth oxide with good dispersibility and an average particle size of 20 to 100 nm.

[0006] To achieve the above objectives, the present invention is implemented through the following technical solutions:

[0007] The invention discloses a method for preparing nano rare earth oxide. After a mixed solution of an organic acid or organic acid salt solution and a rare earth compound and a precipitant are subjected to heat preservation reaction, the precursor is calcined to obtain the nano rare earth oxide.

[0008] Preferably, the molar concentration of the precipitant is 1.5-2.3 mol / L, and the molar ratio of the rare earth ions to the precipitant is 1:2.5-4.5.

[0009] Preferably, the mixed solution and the precipitant are mixed by dropping, and when they are dropped simultaneously, the dropping rate ratio of the mixed solution to the precipitant is 1:1.5-2.5.

[0010] Preferably, the temperature of the heat preservation reaction is 40-70° C., and the reaction time is 0.5-1 h.

[0011] Preferably, after the insulation reaction is completed, the end point pH value is 6.4 to 6.7.

[0012] Preferably, the calcination temperature is 700-900° C., and the calcination time is 1-4 hours.

[0013] Preferably, the rare earth compound is one or more of rare earth nitrate, rare earth chloride, rare earth sulfate, and rare earth acetate; the organic acid is one or more of tartaric acid, malic acid, and citric acid; the organic acid salt is one or more of sodium tartrate, ammonium tartrate, ammonium malate, sodium malate, ammonium citrate, and sodium citrate; and the precipitant is one of an ammonia precipitant and a sodium precipitant.

[0014] Preferably, the ammonia precipitant is one or more of ammonia water, ammonium bicarbonate, and ammonium carbonate; the sodium precipitant is one or more of sodium hydroxide, sodium bicarbonate, and sodium carbonate.

[0015] Preferably, the molar ratio of the tartaric acid, malic acid and salts thereof to the rare earth ions is 1:1-5; the molar ratio of the citric acid and salts thereof to the rare earth ions is 1:2-5.

[0016] Correspondingly, the nano rare earth oxide prepared by the above preparation method has an average particle size of 20 to 100 nm.

[0017] The present invention has the following beneficial effects:

[0018] 1. Compared with the hydrothermal method and sol-gel method used to prepare nano rare earth oxides, the organic complex precipitation method used in the present invention has low cost, simple equipment and easy operation. The prepared nano rare earth oxide precursor is easy to filter and does not require centrifugation operation, so it can be industrialized.

[0019] 2. The present invention regulates the preparation of the solution and the feeding method of each raw material, introduces organic acid radical ions to form organic rare earth complex ions by complexing with rare earth ions, thereby accelerating the nucleation process and regulating the crystal growth process. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 The present invention is a flow chart for preparing the nano rare earth oxide;

[0021] Figure 2 This is a SEM image of the nano-lanthanum oxide prepared in Example 1;

[0022] Figure 3 This is a SEM image of lanthanum oxide prepared in Comparative Example 1;

[0023] Figure 4 This is a SEM image of lanthanum oxide prepared in Comparative Example 2;

[0024] Figure 5 This is the SEM image of lanthanum oxide prepared in Comparative Example 3. DETAILED DESCRIPTION

[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0026] Unless otherwise specified, the technical means used in the embodiments are conventional means well known to those skilled in the art.

[0027] 1.Reference Figure 1 As shown, the present invention discloses a method for preparing nano rare earth oxide, the process is: after a mixed solution of an organic acid or organic acid salt solution and a rare earth compound and a precipitant are subjected to heat preservation reaction, the precursor is filtered, washed, dried and calcined to obtain the nano rare earth oxide.

[0028] Wherein, the molar concentration of the precipitant is 1.5-2.3 mol / L, more preferably 1.8-2.2 mol / L; the molar ratio of the rare earth ion to the precipitant is 1:2.5-4.5, more preferably 1:3.0-4.0. The mixed solution and the precipitant are mixed in a dropwise manner. When added dropwise at the same time, the dripping rate ratio of the mixed solution to the precipitant is 1:1.5-2.5, more preferably 1:1.8-2.2, that is, when added dropwise at the same time, the ratio of the number of moles of the mixed solution and the precipitant dripping into the bottom liquid per minute, mol / min. When the simultaneous dripping method is not adopted, regardless of the dripping rate, the mixed solution is dripped into the precipitant, or the precipitant is dripped into the mixed solution to achieve the purpose of the invention.

[0029] Further, the temperature of the insulation reaction is 40-70°C, and the reaction time is 0.5-1h. After the insulation reaction is completed, the end point pH value is 6.4-6.7. The calcination temperature is 700-900°C, more preferably 750-850°C, and the calcination time is 1-4h. The end point pH is the pH value of the system after the reaction is completed, which is determined by the amount of precipitant added.

[0030] Further, the rare earth compound is one or more of rare earth nitrate, rare earth chloride, rare earth sulfate, and rare earth acetate; the organic acid is one or more of tartaric acid, malic acid, and citric acid; the organic acid salt is one or more of sodium tartrate, ammonium tartrate, ammonium malate, sodium malate, ammonium citrate, and sodium citrate; the precipitant is one of an ammonia precipitant and a sodium precipitant. The ammonia precipitant is one or more of ammonia water, ammonium bicarbonate, and ammonium carbonate; the sodium precipitant is one or more of sodium hydroxide, sodium bicarbonate, and sodium carbonate.

[0031] Wherein, the tartaric acid, malic acid and its salt and rare earth ion (RE 3+ ) is 1:1 to 5, more preferably 1:2 to 4; the citric acid and its salt and the rare earth ion (RE 3+ ) is 1:2 to 5, more preferably 1:3 to 4.

[0032] 2. The present invention prepares nano rare earth oxide according to the above method, and the average particle size of the nano rare earth oxide is 20 to 100 nm.

[0033] The present invention will be further described below in conjunction with specific embodiments.

[0034] Example 1

[0035] Preparation of Nano Rare Earth Oxides:

[0036] (1) Preparation of organic acid rare earth complex solution: prepare a 200 g / L lanthanum chloride solution and a 2 mol / L tartaric acid aqueous solution at the same time, and mix the two to obtain a mixed solution.

[0037] (2) Organic acid rare earth precipitation reaction: At 70°C, with water as the base liquid, the mixed liquid and an aqueous solution of ammonium bicarbonate (with a concentration of 2 mol / L) were simultaneously added dropwise to the base liquid for reaction, and the relative dropping speed was controlled so that the molar ratio of lanthanum chloride to ammonium bicarbonate was 1:3 during the dropping process. After the dropping was completed, the reaction was continued at 70°C for 0.5 h, and the reaction end point pH was 6.5.

[0038] (3) The reaction solution was filtered and washed with ethanol solution. The filter cake was dried to obtain a precursor. The precursor was calcined at 800°C for 2h to obtain nano-lanthanum oxide. The SEM image of nano-lanthanum oxide is shown in Figure 2 The average particle size of the obtained nano lanthanum oxide is 40 to 65 nm.

[0039] Example 2

[0040] Preparation of Nano Rare Earth Oxides:

[0041] (1) A cerium chloride solution with a concentration of 100 g / L was prepared and mixed with a sodium citrate aqueous solution with a concentration of 2.2 mol / L to obtain a mixed solution.

[0042] (2) At 40°C, a 2 mol / L dilute ammonia solution was added dropwise to the mixture for reaction. After the addition was completed, the reaction was continued at 40°C for 0.5 h. The pH value at the end of the reaction was 6.6.

[0043] (3) The reaction liquid is filtered and washed with an ethanol solution to obtain a filter cake and a filtrate. The filter cake is dried to obtain a precursor. The precursor is calcined at 800° C. for 2 h to obtain nano cerium oxide. The average particle size of the obtained nano cerium oxide is 35 to 50 nm.

[0044] Example 3

[0045] Preparation of Nano Rare Earth Oxides:

[0046] (1) A 50 g / L dysprosium chloride solution was prepared and mixed with a 2 mol / L malic acid aqueous solution to obtain a mixed solution.

[0047] (2) The mixed solution was added dropwise to a 2 mol / L ammonium bicarbonate solution at 60°C for reaction. After the addition was completed, the mixture was kept warm and the reaction was continued for 0.5 h. The pH value at the end of the reaction was 6.5.

[0048] (3) The reaction solution is filtered and washed with an ethanol solution. The filter cake is dried to obtain a precursor. The precursor is calcined at 750° C. for 2 h to obtain nano-dysprosium oxide. The average particle size of the obtained nano-dysprosium oxide is 20 to 35 nm.

[0049] Example 4

[0050] The only difference from Example 1 is that the reaction temperature during the dropwise addition process is 50° C. The average particle size of the obtained nano-lanthanum oxide is 35-45 nm.

[0051] Example 5

[0052] The only difference from Example 1 is that the molar ratio of lanthanum chloride to ammonium bicarbonate during the dropwise addition is 1:2.5. The average particle size of the obtained nano lanthanum oxide is 50-80 nm.

[0053] Comparative Example 1

[0054] The only difference from Example 1 is that citric acid and its salts are mixed with RE 3+ The molar ratio of lanthanum oxide is 1:20. The obtained lanthanum oxide is a layered aggregate, and the SEM image is as follows Figure 3 .

[0055] Comparative Example 2

[0056] The only difference from Example 1 is that the pH value at the end point of the reaction is controlled to be 4. The obtained lanthanum oxide is a micron-sized aggregate, as shown in the SEM image. Figure 4 .

[0057] Comparative Example 3

[0058] The only difference from Example 1 is that the calcination temperature is 450°C. The obtained lanthanum oxide is agglomerates, and the SEM image is as follows: Figure 5 .

[0059] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing nano rare earth oxide, characterized in that: After the mixed solution of organic acid or organic acid salt solution and rare earth compound and precipitant are subjected to heat preservation reaction, the precursor is calcined to obtain nano rare earth oxide.

2. The preparation method according to claim 1, characterized in that: The molar concentration of the precipitant is 1.5-2.3 mol / L, and the molar ratio of the rare earth ion to the precipitant is 1:2.5-4.

5.

3. The preparation method according to claim 1, characterized in that: The mixed solution and the precipitant are mixed in a dropwise manner. When the mixed solution and the precipitant are added dropwise at the same time, the drop rate ratio of the mixed solution to the precipitant is 1:1.5-2.

5.

4. The preparation method according to claim 1, characterized in that: The temperature of the heat preservation reaction is 40-70°C, and the reaction time is 0.5-1h.

5. The preparation method according to claim 1, characterized in that: After the heat preservation reaction is completed, the end point pH value is 6.4-6.

7.

6. The preparation method according to claim 1, characterized in that: The calcination temperature is 700-900°C, and the calcination time is 1-4h.

7. The preparation method according to claim 1, characterized in that: The rare earth compound is one or more of rare earth nitrate, rare earth chloride, rare earth sulfate, and rare earth acetate; the organic acid is one or more of tartaric acid, malic acid, and citric acid; the organic acid salt is one or more of sodium tartrate, ammonium tartrate, ammonium malate, sodium malate, ammonium citrate, and sodium citrate; and the precipitant is one of an ammonia precipitant and a sodium precipitant.

8. The preparation method according to claim 7, characterized in that: The ammonia precipitant is one or more of ammonia water, ammonium bicarbonate, and ammonium carbonate; the sodium precipitant is one or more of sodium hydroxide, sodium bicarbonate, and sodium carbonate.

9. The preparation method according to claim 7, characterized in that: The molar ratio of the tartaric acid, malic acid and their salts to the rare earth ions is 1:1-5; the molar ratio of the citric acid and their salts to the rare earth ions is 1:2-5.

10. A nano rare earth oxide prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The average particle size of the nano rare earth oxide is 20-100 nm.

Citation Information

Cited By

  • Rare earth-molybdenum antibacterial material and preparation method thereof

    CN120477207A

  • Rare earth-molybdenum antibacterial material and preparation method thereof

    CN120477207B

  • Preparation method of rare earth antibacterial material

    CN120477208A

  • Preparation method of rare earth antibacterial material

    CN120477208B

  • Preparation method of rare earth antibacterial carrier

    CN120477209A