2D / 3D perovskite constructed based on formamidine spacer ligand and preparation method and application thereof
By using formamidine spacer ligands to construct 2D/3D perovskite films in perovskite solar cells, the stability and carrier transport problems of perovskite solar cells are solved, and solar cell performance with high efficiency and long life is achieved. .
Patent Information
- Application Number
- CN202410892932.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-04
- Publication Date
- 2024-10-29
AI Technical Summary
Stability issues in perovskite solar cells, especially the performance degradation of 3D perovskite structures under thermal and light stress, and poor carrier transport in 2D perovskites.
Using 2D/3D perovskites based on formamidine spacer ligands, RP-type or DJ-type 2D/3D perovskite films are formed by introducing formamidine organic spacer ligands into the perovskite precursor solution and annealing them on a hot stage. , used to construct the perovskite active layer of trans-perovskite solar cells.
The photoelectric conversion efficiency and stability of perovskite solar cells are significantly improved, and the initial efficiency of more than 80% can be maintained under high humidity and high temperature conditions, extending the service life of the equipment.
Smart Images

Figure CN118870941A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of solar cells, and in particular relates to a 2D / 3D perovskite constructed based on a formamidine spacer ligand, and a preparation method and application thereof. Background Art
[0002] Perovskite solar cells have the characteristics of low manufacturing cost, simple preparation process, high absorption coefficient, high defect tolerance and long carrier lifetime. As the most promising photovoltaic device after silicon-based solar cells, PCE has increased from the initial 3.8% to the current 26.15%, which is close to the efficiency of silicon-based cells in just a dozen years. However, the stability problem of perovskite solar cells has been urgently needed to be solved since its advent. Traditional 3D perovskites have a cubic crystal structure with the general formula ABX3. Due to the weak hydrogen bonds or ionic bonds between the A cations and the corner-sharing BX6 octahedrons, the coordination structure of 3D perovskite compounds is easily destroyed by water or polar solvents, and can accelerate the ion migration inside the perovskite and the transition from the black phase to the yellow phase under thermal stress and light stress, thereby exacerbating the degradation of device performance. Unlike 3D perovskites, 2D perovskites use bulky organic cations to separate the inorganic BX6 plates on both sides, which can greatly improve the resistance to external stimuli such as moisture, light, and thermal stress. In 2D perovskites, large organic cations play the role of a hydrophobic layer, protecting the BX6 octahedron sandwiched in the middle from hydrolysis, while providing strong steric hindrance, effectively inhibiting ion migration, and enhancing structural stability. In addition, compared with the small A-site cations in 3D, the bulky organic cations can enhance the interaction with the inorganic octahedron, further improving the stability of 2D perovskites.
[0003] When bulky cations are incorporated into the 3D perovskite structure in a small amount, the 3D structure can be induced to transform into a low dimensional structure, thereby forming a 2D / 3D hybrid perovskite structure. Bulk organic cations make 2D perovskites have good hydrophobicity and excellent chemical stability, while inhibiting the ion migration of 3D perovskites. Although pure phase 2D or low-n quasi-2D perovskites can be used as one of the strong candidates for perovskite materials, their macromolecular spacer layers form a relatively insulating thin layer between the inorganic layers, which hinders the effective transport of carriers and is not conducive to the realization of high-performance PSCs. At the same time, the large band gap of 2D perovskites leads to a reduction in the light absorption spectrum range, and the large exciton binding energy is not conducive to the separation of photoexcited electron-hole pairs. Therefore, the construction of 2D / 3D hybrid perovskites can achieve the high-efficiency photovoltaic performance of 3D perovskites, and can also isolate the fragile 3D perovskite film from moisture and oxygen, inhibiting ion migration to improve the stability of perovskites. In addition, the construction of efficient and stable 2D / 3D hybrid perovskite devices requires a clever balance between the composition and structure of 2D and 3D perovskites to meet the performance requirements of solar cell devices.
[0004] To date, RP-type perovskites are the most studied systems for preparing 2D / 3D perovskites, but there are van der Waals gaps between the inorganic layers of RP-type 2D perovskites, which affects the further improvement of the stability of perovskites. In DJ-type 2D perovskites, adjacent inorganic layers are directly bridged together by diamine spacers to produce strong hydrogen bonds, thereby eliminating the van der Waals gap, shortening the interlayer distance, and enhancing the interaction between the layers, thereby improving stability and the ability to transfer charge. DJ-type 2D perovskites have better carrier transport than RP-type 2D perovskites, and can be better used to improve the photovoltaic efficiency and stability of corresponding devices. However, at present, dimethylamine spacer ligands are mainly used in DJ-type 2D / 3D perovskites, and there are few studies on the use of dimethylamidine spacer ligands in DJ-type 2D perovskites, and the internal mechanism of action is still unclear. Compared with dimethylamine spacer ligands, dimethylamidine spacer ligands will form more hydrogen bonds, further improving the photovoltaic performance of perovskite solar cells. In addition, the synergistic effect between the dimethoate spacer ligands and the perovskite components remains to be further explored.
[0005] Therefore, there is an urgent need to systematically and in-depth explore the mechanism by which the diformamidine group exerts its effects, and to reveal the differences between the two in regulating film morphology, energy band arrangement, charge transport, stability, etc. by comparing the 2D / 3D perovskite films and device properties prepared with diformamidine spaced ligands and monoformamidine spaced ligands. Summary of the invention
[0006] In view of this, one of the objects of the present invention is to provide a method for preparing a 2D / 3D perovskite constructed based on a single formamidine spacer ligand; a second object of the present invention is to provide a 2D / 3D perovskite constructed based on a double formamidine spacer ligand; a third object of the present invention is to provide an application of a 2D / 3D perovskite constructed based on a formamidine spacer ligand in the preparation of an inverse perovskite solar cell; a fourth object of the present invention is to provide an inverse perovskite solar cell; and a fifth object of the present invention is to provide a method for preparing an inverse perovskite solar cell.
[0007] In order to achieve the above object, the present invention provides the following technical solutions:
[0008] 1. A preparation method of a 2D / 3D perovskite based on a formamidine spacer ligand, the preparation method comprising: introducing an organic spacer ligand into a perovskite precursor solution, then spin coating the solution on a substrate, and dripping an anti-solvent before the spin coating process is completed, and then placing the solution on a hot plate for annealing to obtain a 2D / 3D perovskite;
[0009] The perovskite precursor solution is an ABX3 type precursor solution;
[0010] The organic spacer ligand is a formamidine spacer ligand.
[0011] Preferably, the anti-solvent is chlorobenzene, wherein the anti-solvent is added within the last 5 to 10 seconds before the end of the spin coating process;
[0012] The A in the ABX3 type precursor solution includes MA + , FA + , Cs + or Rb + Any one or more of B including Pb 2+ Sn 2+ Or Ge 2+ Any one or more of the following, X includes Cl-, Br - Or any one or more of I-.
[0013] Further preferably, the solvent in the ABX3-type precursor solution is any one or more of dimethyl sulfoxide (DMSO), diethyl sulfoxide (DESO), N,N-dimethylformamide (DMF), N,N-diethylformamide (DEF), N,N-dimethylacetamide (DMAC) or N-methylpyrrolidone (NMP).
[0014] Preferably, the formamidine spacer ligand contains at least one formamidine group.
[0015] More preferably, the carboxamidine spacer ligand is any one of benzamidine hydrochloride or benzadiamine hydrochloride.
[0016] Preferably, the mass ratio of ABX3 to formamidine spacer ligand in the ABX3 type perovskite precursor solution is 800-1500:0.02-44.0.
[0017] Preferably, the spin coating process is as follows: first, spin coating at a rotation speed of 1000 to 2000 rpm for 10 to 20 seconds, and then continue to spin coating at a rotation speed of 2000 to 4000 rpm for 30 to 50 seconds;
[0018] The annealing is specifically: annealing on a hot plate at 100-150° C. for 30-60 minutes.
[0019] 2. 2D / 3D perovskite based on formamidine spacer ligand prepared according to the above method.
[0020] Preferably, the 2D perovskite in the 2D / 3D perovskite constructed based on formamidine spacer ligands is any one of RP-type 2D perovskite and DJ-type 2D perovskite, the 3D perovskite in the 2D / 3D perovskite constructed based on formamidine spacer ligands is ABX3-type perovskite, and the 2D / 3D perovskite in the 2D / 3D perovskite constructed based on formamidine spacer ligands is RP-type 2D / 3D perovskite or DJ-type 2D / 3D perovskite.
[0021] 3. Application of the above-mentioned 2D / 3D perovskite constructed based on formamidine spacer ligands in the preparation of inverse perovskite solar cells.
[0022] 4. An inverted perovskite solar cell, which is composed of a conductive substrate layer, a hole transport layer, a bottom interface modification layer, a perovskite active layer, an electron transport layer, a cathode interface layer and a back electrode layer from bottom to top, and the perovskite active layer is the above-mentioned 2D / 3D perovskite constructed based on formamidine spacer ligands.
[0023] 5. According to the above inverse perovskite solar cell, the material of the conductive substrate layer is any one of ITO or FTO;
[0024] The material of the hole transport layer is any one or more of nickel oxide, poly 3-hexylthiophene (P3HT), CuSCN, Spiro-OMeTAD or p-tert-butylbenzoic acid (PTAA);
[0025] The material of the bottom interface modification layer is Al2O3;
[0026] The material of the electron transport layer is any one or more of poly(butyl methacrylate) (PCBM), TiO2 or CeO2;
[0027] The material of the cathode interface layer is any one or more of 2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline (BCP) or LiF;
[0028] The material of the back electrode layer is any one or more of Ag, Au or C.
[0029] 6. A method for preparing the above-mentioned inverse perovskite solar cell, the preparation method comprising the following steps:
[0030] (1) Add the material of the conductive substrate layer to a glass cleaning agent and perform ultrasonic cleaning for 20 to 30 minutes, continue to perform ultrasonic cleaning with deionized water for 3 to 6 times (15 to 30 minutes each time), and then use ethanol and isopropanol to clean for 2 to 4 times (30 to 60 minutes each time), and blow dry with nitrogen to obtain a clean conductive substrate layer;
[0031] (2) dissolving the material of the hole transport layer in deionized water, filtering it with a water filter head, and then dripping it onto the clean conductive substrate layer in step (1) using a pipette, spin coating it at a speed of 2500 to 5500 rpm for 30 to 60 seconds, and annealing it at 150 to 200° C. for 10 to 30 minutes to form a hole transport layer on the conductive substrate layer;
[0032] (3) dissolving the material of the bottom interface modification layer in isopropanol, using a pipette to draw 50-100 μL and evenly smearing it on the hole transport layer, spin coating at a speed of 2500-5000 rpm, and annealing on a hot plate at 100-120° C. for 10-20 min to form a bottom interface modification layer on the hole transport layer;
[0033] (4) introducing a carboxamidine-based organic spacer ligand into an ABX3-type perovskite precursor solution, using a pipette to draw 50 to 100 μL and evenly apply it on the bottom interface modification layer, firstly performing the first step of spin coating at a speed of 1000 to 2000 rpm for 10 to 20 seconds, and then performing the second step of spin coating at a speed of 2000 to 4000 rpm for 30 to 50 seconds, adding 150 to 300 μL of chlorobenzene as an anti-solvent at the end of the last 5 to 10 seconds before the end of the second step of spin coating, and then annealing on a hot stage at 100 to 150° C. for 30 to 60 minutes, thereby forming a 2D / 3D perovskite film, i.e., a perovskite active layer, on the bottom interface modification layer;
[0034] (5) dissolving the material of the electron transport layer in chlorobenzene, using a pipette to draw 30 to 60 μL and evenly applying it on the perovskite active layer in step (4), and performing spin coating at a speed of 2500 to 5000 rpm for 40 to 60 seconds to form an electron transport layer on the perovskite active layer;
[0035] (6) dissolving the material of the cathode interface layer in isopropanol, using a pipette to draw 30 to 50 μL and evenly applying it on the electron transport layer, and spin coating at a speed of 800 to 2500 rpm to form the cathode interface layer;
[0036] (7) In step (6), the cathode interface layer is provided with a vacuum degree of less than 1×10 -4 The material of the back electrode layer was evaporated at a pressure of 1.25 Pa to form a back electrode layer with a thickness of 80 to 120 nm.
[0037] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing 2D / 3D perovskite based on formamidine spacer ligands, which mainly comprises introducing formamidine organic spacer ligands (PhFA or PhDFA) into ABX3 type perovskite precursor solution (A is MA + , FA + , Cs + or Rb + Plasma, B is Pb 2+ Sn 2+ Or Ge 2+ Plasma, X is Cl - Br - or I - The present inventors prepared 2D / 3D perovskite with formamidine spacer ligands, which can react with residual lead iodide on the surface of the perovskite film, thereby passivating defects and reducing non-radiative recombination losses; at the same time, the DJ-type 2D perovskite formed by double formamidine spacer ligands can effectively solve the problem that the van der Waals gap between adjacent layers of the RP-type 2D perovskite constructed with single formamidine spacer ligands affects the stability of the perovskite structure and carrier transport.
[0038] The present invention also provides an inverted perovskite solar cell, which mainly uses a 2D / 3D perovskite constructed based on a single formamidine spacer ligand as the perovskite active layer of the solar cell, and the inverted perovskite solar cell formed obtains a photoelectric conversion efficiency of more than 24.51%, greatly improves its working stability, and the inverted perovskite solar cell of the present invention can still maintain 90% of the initial efficiency after 5000 hours under the condition of 20-30% RH, and the inverted perovskite solar cell of the present invention can still maintain more than 80% of the initial efficiency after 600 hours under the conditions of 40-50% humidity and 80°C temperature. Comprehensive analysis found that after the 2D / 3D perovskite constructed based on the formamidine spacer ligand of the present invention is used as the perovskite active layer of the inverted perovskite solar cell, the photoelectric conversion efficiency and stability of the solar cell are significantly improved, which has an important impact on accelerating the commercialization process of perovskite solar cells.
[0039] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:
[0041] Figure 1 is the hydrogen nuclear magnetic resonance spectrum of the solution formed in Example 1 and Comparative Example 1 ( 1 H NMR) spectra;
[0042] Figure 2 is the hydrogen nuclear magnetic resonance spectrum of the solution formed in Example 2 and Comparative Example 2 ( 1 H NMR) spectra;
[0043] Figure 3 The UV absorption spectra of different perovskite films prepared in Example 3 (Target 1), Example 4 (Target 2) and Comparative Example 3 (Control);
[0044] Figure 4 The fluorescence spectra corresponding to the different perovskite films prepared in Example 3 (Target 1), Example 4 (Target 2) and Comparative Example 3 (Control);
[0045] Figure 5 X-ray diffraction patterns corresponding to different perovskite films prepared in Example 3 (Target 1), Example 4 (Target 2) and Comparative Example 3 (Control);
[0046] Figure 6 Grazing incidence wide-angle X-ray scattering images corresponding to different perovskite films prepared in Example 3 (Target 1), Example 4 (Target 2) and Comparative Example 3 (Control);
[0047] Figure 7 JV curves of forward scan (RS) and reverse scan (FS) corresponding to the inverted RP type 2D / 3D perovskite solar cell (2D / 3D-PhFA) prepared in Example 5, the inverted DJ type 2D / 3D perovskite solar cell (2D / 3D-PhDFA) prepared in Example 6, and the inverted 3D perovskite solar cell (3D) prepared in Comparative Example 4;
[0048] Figure 8 External quantum efficiency (EQE) curves and integrated current density diagrams corresponding to the inverted RP-type 2D / 3D perovskite solar cell (2D / 3D-PhFA) prepared in Example 5, the inverted DJ-type 2D / 3D perovskite solar cell (2D / 3D-PhDFA) prepared in Example 6, and the inverted 3D perovskite solar cell (3D) prepared in Comparative Example 4;
[0049] Fig. 9 Stability test graphs of the inverted RP-type 2D / 3D perovskite solar cell (2D / 3D-PhFA) prepared in Example 5, the inverted DJ-type 2D / 3D perovskite solar cell (2D / 3D-PhDFA) prepared in Example 6, and the inverted 3D perovskite solar cell (3D) prepared in Comparative Example 4 under unsealed conditions, at room temperature and a relative humidity of 20-30%;
[0050] Fig.10 Stability test graphs of the inverted RP-type 2D / 3D perovskite solar cell (2D / 3D-PhFA) prepared in Example 5, the inverted DJ-type 2D / 3D perovskite solar cell (2D / 3D-PhDFA) prepared in Example 6, and the inverted 3D perovskite solar cell (3D) prepared in Comparative Example 4 under unsealed conditions at 80° C. and a relative humidity of 40-50%;
[0051] Fig.11 The inverted RP type 2D / 3D perovskite solar cell (2D / 3D-PhFA) prepared in Example 5, the inverted DJ type 2D / 3D perovskite solar cell (2D / 3D-PhDFA) prepared in Example 6, and the inverted 3D perovskite solar cell (3D) prepared in Comparative Example 4 were used under unsealed conditions and at the maximum power point of 100 mW / cm 2 Stability test diagram under illumination (MPP tracking). DETAILED DESCRIPTION
[0052] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments only illustrate the basic concept of the present invention in a schematic manner, and the following embodiments and features in the embodiments can be combined with each other without conflict.
[0053] Example 1
[0054] 10 mg of benzamidine hydrochloride (PhFACl) was dissolved in 0.5 mL of deuterated DMSO and shaken for 20 min.
[0055] Comparative Example 1
[0056] Dissolve 10 mg of benzamidine hydrochloride (PhFACl) and 20 mg of PbI2 in 0.5 mL of deuterated DMSO and shake for 20 min.
[0057] Example 2
[0058] 10 mg of benzadiamine hydrochloride (PhDFACl) was dissolved in 0.5 mL of deuterated DMSO and shaken for 20 min.
[0059] Comparative Example 2
[0060] Dissolve 10 mg of benzadiamine hydrochloride (PhDFACl) and 20 mg of PbI2 in 0.5 mL of deuterated DMSO and shake for 20 min.
[0061] The solutions formed in Examples 1 and 2 and Comparative Examples 1 and 2 were subjected to H NMR spectroscopy test. The experimental results are as follows: Figure 1 and 2 As shown, Figure 1 is the hydrogen nuclear magnetic resonance spectrum of the solutions formed in Example 1 and Comparative Example 1; Figure 2 is the hydrogen nuclear magnetic resonance spectrum of the solution formed in Example 2 and Comparative Example 2. Figure 1 and Figure 2 It can be seen that when PhFA and PhDFA are mixed with PbI2, -NH3 + and = NH 3+ The corresponding peak positions all shifted significantly. 1 In the H NMR spectrum, 8.00 ppm corresponds to the position of the benzene ring. 1 The H peak intensity increased by 3 to 4 times, and the peak position also shifted slightly. 1 The peak intensity and peak position of the 1H peak at the benzene ring position corresponding to 7.90ppm in the H NMR spectrum are almost unchanged. The results show that both PhFA and PhDFA can react with [PbI6] 4- The octahedra interact with each other through NH···I hydrogen bonds, but it can be found that PhDFA molecules can produce more hydrogen bonds than PhFA molecules, while eliminating the van der Waals gap.
[0062] Example 3
[0063] A RP-type 2D / 3D perovskite film based on a monocarboxamidine spacer ligand is prepared by the following method:
[0064] 645.4 mg PbI2, 18.2 mg CsI and 228.2 mg FAI were dissolved in DMSO:DMF (volume ratio of 1:4) to form a perovskite precursor solution, and 1.0 mg PhFACl, after the configuration is completed, the precursor solution is shaken for 20 minutes to obtain a mixed solution; filtered using an organic filter head with a diameter of 13 mm and a pore size of 0.2 um, 50 μL of the mixed solution is drawn with a pipette, and evenly applied on an Al2O3 substrate, first spin-coated at 1000 rpm for 10 s, and then the second spin-coated at 2000 rpm for 30 s (at the end of the penultimate 5 seconds before the end of the second spin-coating process, the drawn 150 μL of chlorobenzene (CB) is quickly and evenly dropped on the center area as an anti-solvent); then annealed on a hot plate at 100°C for 30 minutes to obtain an RP-type 2D / 3D perovskite film constructed based on a single formamidine spacer ligand, that is, a 2D / 3D perovskite constructed based on a formamidine spacer ligand.
[0065] Example 4
[0066] A DJ-type 2D / 3D perovskite film constructed based on a dimethoate spacer ligand, the specific preparation method of which is different from that of Example 3 in that "1.0 mg PhFACl" in Example 3 is replaced by "1.0 mg PhDFACl", and the other conditions remain unchanged.
[0067] Comparative Example 3
[0068] A perovskite film, the specific preparation method is as follows:
[0069] 645.4 mg PbI2, 18.2 mg CsI and 228.2 mg FAI were dissolved in DMSO:DMF (volume ratio of 1:4), shaken for 20 min to obtain a perovskite precursor solution, and filtered using an organic filter head with a diameter of 13 mm and a pore size of 0.2 um; 50 μL of the perovskite precursor solution was taken with a pipette and evenly applied on an Al2O3 substrate, first spin-coated at 1000 rpm for 10 s, and then spin-coated in the second step at 2000 rpm for 30 s (at the end of the penultimate 5 s before the end of the second spin-coating process, the 150 μL CB taken was quickly and evenly dripped on the center area as an anti-solvent); the perovskite film was annealed on a hot stage at 100°C for 30 min to obtain a perovskite film.
[0070] The UV absorption spectra of the different perovskite films prepared in Example 3 (Target 1), Example 4 (Target 2) and Comparative Example 3 (Control) were tested respectively. The experimental results are as follows: Figure 3As shown. From the results, it can be seen that compared with the perovskite film prepared in Comparative Example 3, the band gaps of the two 2D / 3D perovskite films formed by adding PhFACl and PhDFACl in Example 3 and Example 4, respectively, have slightly blue shifted, and the perovskite doped with PhDFA has a more obvious blue shift.
[0071] Fluorescence spectrum tests were performed on Example 3 (Target 1), Example 4 (Target 2) and Comparative Example 3 (Control). The experimental results are as follows: Figure 4 As shown. Figure 4 It can be seen that compared with the 3D perovskite film of the control group in Comparative Example 3, the PL intensity of the perovskite films doped with formamidine organic spacer molecules (PhFACl and PhDFACl) in Examples 3 and 4 was enhanced. At the same time, the intensity of the perovskite film doped with PhDFA was the highest, which was 1 to 2 times higher than that of the 3D perovskite film of the control group. This is closely related to the greater improvement of the crystallization quality of the film by the DJ-type 2D / 3D perovskite formed after the addition of PhDFA. At the same time, a blue shift appeared in the PL spectrum after the addition of PhFA and PhDFA.
[0072] X-ray diffraction tests were performed on Example 3 (Target 1), Example 4 (Target 2) and Comparative Example 3 (Control), and the experimental results are as follows: Figure 5 As shown. Figure 5 It can be seen that the results show that the characteristic peak intensity of the perovskite formed after the organic cation (formamidinium group) is doped in Examples 3 and 4 is significantly higher than the characteristic peak of the perovskite in Comparative Example 3, and the diffraction peak intensity of the perovskite in Example 4 formed after the addition of PhDFA is the strongest, indicating that the addition of PhDFA can improve the crystallinity of the film to a greater extent. More importantly, the appearance of 2D peaks was found in the low angles of the XRD diffraction peaks of the two perovskites doped with organic spacers in Examples 3 and 4, which proves the generation of 2D perovskites. In addition, the appearance of PbI2 peaks was found at the 12.69° position of the perovskite in Comparative Example 3, while the PbI2 peaks were not found at this position in the perovskites of Examples 3 and 4, indicating that the newly added formamidinium organic spacer (benzamidine hydrochloride or benzadiamine hydrochloride) can react with the residual PbI2 to form 2D perovskites, improving the crystallization quality of the film.
[0073] Example 3 (Target 1), Example 4 (Target 2) and Comparative Example 3 (Control) were tested for grazing incidence wide-angle X-ray scattering. The experimental results are as follows: Figure 6 As shown. Figure 6It can be seen from the test results that the perovskite film of Example 3 in the control group is a uniform Debye-Scherrer diffraction ring, and the diffraction ring intensity in all directions is basically the same, indicating that the perovskite crystal of Example 3 has an isotropic orientation distribution. In contrast, the perovskite films of Examples 3 and 4 show obvious 2D phases in the region of small q values, and this corresponds to the 2D peak observed by XRD at low angles, which once again proves the formation of 2D perovskite. At the same time, it can be found from the GIWAXS spectrum that the perovskite film of Example 4 shows a higher diffraction intensity as a whole, and Bragg spots appear, proving that its crystal orientation is better.
[0074] Example 5
[0075] An inverted RP-type 2D / 3D perovskite solar cell, which is composed of an ITO conductive substrate layer, a nickel oxide hole transport layer, an Al2O3 bottom interface modification layer, an RP-type 2D / 3D perovskite film (perovskite active layer) constructed based on PhFACl in Example 3, a PCBM electron transport layer, a BCP cathode interface layer and an Ag back electrode layer from bottom to top. The specific preparation method is as follows:
[0076] (1) After adding glass cleaning agent to the ITO conductive substrate, ultrasonic cleaning was performed for 20 minutes, followed by ultrasonic cleaning with deionized water for 3 times (15 minutes each time), followed by cleaning with ethanol and isopropanol for 2 times (30 minutes each time), and then drying with nitrogen to obtain a clean conductive substrate layer.
[0077] (2) Dissolve nickel oxide in deionized water, filter it using a water filter head, and then drop it onto the pretreated conductive substrate layer using a pipette. Spin coat the solution at 4000 rpm for 30 seconds, and then anneal the sample at 150°C for 10 minutes to form a hole transport layer on the conductive substrate layer.
[0078] (3) Dissolve Al2O3 in isopropanol, use a pipette to take 50 μL and evenly apply it on the nickel oxide hole transport layer, spin coat at 5000 rpm for 30 seconds, and anneal on a hot plate at 100°C for 10 minutes to form a bottom interface modification layer on the hole transport layer.
[0079] (4) 645.4 mg PbI2, 18.2 mg CsI and 228.2 mg FAI were dissolved in DMSO:DMF (volume ratio of 1:4) as a perovskite precursor solution, and 1.0 mg PhFACl was added to the perovskite precursor solution. After the configuration was completed, the precursor solution was oscillated for 20 minutes, filtered using an organic filter head with a diameter of 13 mm and a pore size of 0.2 um, and 50 μL of the perovskite precursor solution was drawn with a pipette and evenly applied on the bottom interface modification layer. The first step of spin coating was performed at 1000 rpm for 10 seconds, and then the second step of spin coating was performed at 2000 rpm for 30 seconds (at the end of the last 5 seconds before the end of the second step of spin coating, the drawn 150 μL CB was quickly and evenly dripped on the center area as an anti-solvent, and then placed on a hot plate at 100°C for annealing for 30 minutes to form an RP-type 2D / 3D perovskite film on the bottom interface modification layer, which is the perovskite active layer.
[0080] (5) Dissolve poly(butyl methacrylate) (PCBM) in chlorobenzene, use a pipette to take 30 μL and evenly apply it on the perovskite active layer in step (4), and spin coat it at a rotation speed of 2500 rpm for 40 s to form an electron transport layer on the perovskite active layer.
[0081] (6) Dissolve 2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline (BCP) in isopropanol, use a pipette to draw 30 μL and evenly apply it on the PCBM in step (5), and spin coat it at a speed of 1000 rpm for 30 seconds to form a cathode interface layer on the electron transport layer;
[0082] (7) In step (6), the electron transport layer is subjected to a vacuum of less than 1×10 -4 Pa pressure evaporated metal Ag to form a back electrode layer with a thickness of 80-120 nm, and finally formed an inverted RP-type 2D / 3D perovskite solar cell (2D / 3D-PhFA).
[0083] Example 6
[0084] A trans DJ type 2D / 3D perovskite solar cell, which consists of an ITO conductive substrate layer, a nickel oxide hole transport layer, an Al2O3 bottom interface modification layer, a DJ type 2D / 3D perovskite film constructed based on PhDFACl as a perovskite active layer, a PCBM electron transport layer, a BCP cathode interface material and an Ag back electrode layer from bottom to top. The difference between the preparation method and Example 5 is that "1.0 mg PhFACl" in step (4) is replaced by "1.0 mg PhDFACl", and the other conditions remain unchanged, so that a trans DJ type 2D / 3D perovskite solar cell (2D / 3D-PhDFA) can be prepared.
[0085] Comparative Example 4
[0086] An inverted 3D perovskite solar cell, which consists of an ITO conductive substrate layer, a nickel oxide hole transport layer, an Al2O3 bottom interface modification layer, the 3D perovskite film in Comparative Example 3, a PCBM electron transport layer, a BCP cathode interface material and an Ag back electrode layer from bottom to top. The difference between the preparation method and Example 5 is that PhFACl is not added to the precursor, and the other conditions remain unchanged, so that an inverted 3D perovskite solar cell (3D) can be prepared.
[0087] The inverse RP type 2D / 3D perovskite solar cell (2D / 3D-PhFA) prepared in Example 5, the inverse DJ type 2D / 3D perovskite solar cell (2D / 3D-PhDFA) prepared in Example 6, and the inverse 3D perovskite solar cell (3D) prepared in Comparative Example 4 were subjected to forward scanning (RS) and reverse scanning (FS) and JV curves were plotted. The experimental results are shown in FIG. Figure 7 shown. Figure 7 The results show that under reverse scanning conditions, the highest efficiency of the inverted 3D perovskite solar cell (3D) prepared in Comparative Example 4 is 22.27% (J SC =24.63mA / cm 2 , V OC =1.089V, FF=83.05%). In comparison, the efficiency of the 2D / 3D perovskite solar cells of Examples 5 and 6 was increased to 24.51% (J SC =25.88mA / cm 2 , V OC =1.130V, FF=83.75%) and 25.02% (J SC =26.07mA / cm 2 , V OC =1.141V, FF=84.12%). It can be found that the photovoltaic performance of the perovskite solar cells formed by the perovskite active layers doped with PhFACl and PhDFACl is improved, and the photovoltaic performance of the perovskite solar cell formed by the perovskite active layer doped with PhDFACl in Example 6 is improved to the greatest extent.
[0088] The external quantum efficiency of the inverted RP type 2D / 3D perovskite solar cell (2D / 3D-PhFA) prepared in Example 5, the inverted DJ type 2D / 3D perovskite solar cell (2D / 3D-PhDFA) prepared in Example 6, and the inverted 3D perovskite solar cell (3D) prepared in Comparative Example 4 were tested. The results are as follows: Figure 8 shown. Figure 8The results show that in the wavelength range of 400-800 nm, the EQE effect of the perovskite solar cell formed by the perovskite active layer doped with PhFACl and PhDFACl is enhanced, and the perovskite solar cell in Example 6 shows a stronger EQE response, which is related to the improvement of crystal quality and the enhancement of carrier extraction ability. At the same time, the integrated current density (24.54 mA / cm 2 , 25.31mA / cm 2 , 25.52mA / cm 2 ) and the J obtained by the actual JV test of the device SC The results match.
[0089] The stability tests were conducted on the inverse RP type 2D / 3D perovskite solar cell (2D / 3D-PhFA) prepared in Example 5, the inverse DJ type 2D / 3D perovskite solar cell (2D / 3D-PhDFA) prepared in Example 6, and the inverse 3D perovskite solar cell (3D) prepared in Comparative Example 4 under different conditions. The experimental results are as follows: Fig. 9 , 10 and 11. Among them, Fig. 9 The stability test diagram of the perovskite solar cells of Example 5, Example 6 and Comparative Example 4 under unsealed conditions at room temperature and a relative humidity of 20-30%. Fig. 9 It can be seen that after 5000 hours of storage, the efficiency of the perovskite solar cell of Comparative Example 4 decays to 70% of the initial efficiency, while the perovskite solar cell of Example 5 maintains 85% of the initial efficiency, and the perovskite solar cell of Example 6 can still maintain more than 90% of the initial efficiency. Fig.10 The stability test diagram of the perovskite solar cells of Example 5, Example 6 and Comparative Example 4 under unsealed conditions at 80°C and a relative humidity of 40-50%. Fig.10 It can be seen that after 600 hours of continuous testing, the efficiency of the perovskite battery in Comparative Example 4 decays to 57% of the initial efficiency, while the perovskite battery in Example 5 still maintains 72% of the initial efficiency, and the perovskite battery in Example 6 can still maintain 85% of the initial efficiency. Fig.11 The perovskite solar cells of Example 5, Example 6 and Comparative Example 4 are used under unsealed conditions and at the maximum power point of 100 mW / cm 2 Stability test chart under light. Fig.11It can be seen that the perovskite cell of comparative example 4 only has 54% of the initial efficiency after 1171 hours of continuous testing, while the perovskite cell of example 5 maintains 90% of the initial efficiency, and the perovskite cell of example 6 can still maintain 96% of the initial efficiency. This shows that the perovskite solar cell formed by the perovskite active layer doped with PhFACl and PhDFACl can increase the stability of use under different conditions.
[0090] Example 7
[0091] In step (4) of Example 5, "645.4 mg PbI2, 18.2 mg CsI and 228.2 mg FAI were dissolved in DMSO:DMF (volume ratio of 1:4) as a perovskite precursor solution, and 1.0 mg PhFACl was added to the perovskite precursor solution" was replaced by "800 mg MASnbCl3 was dissolved in diethyl sulfoxide and then 44 mg PhFACl was added", and "firstly the first step of spin coating was performed at 1000 rpm and 10 s, and then the second step of spin coating was performed at 2000 rpm and 30 s (at the end of the last 5 s before the end of the second step of spin coating, 150 μL CB was quickly and evenly dropped on the center area as an anti-solvent" was modified to "firstly the first step of spin coating was performed at 2000 rpm and 20 s, and then the second step of spin coating was performed at 4000 rpm and 50 s (at the end of the last 10 s before the end of the second step of spin coating, 150 μL CB was quickly and evenly dropped on the center area as an anti-solvent" was modified to "firstly the first step of spin coating was performed at 2000 rpm and 20 s, and then the second step of spin coating was performed at 4000 rpm and 50 s (at the end of the last 10 s before the end of the second step of spin coating, 150 μL CB was quickly and evenly dropped on the center area CB is used as an anti-solvent and is quickly and evenly dropped on the central area", "annealing on a hot stage at 100°C for 30 min" is replaced by "annealing on a hot stage at 150°C for 60 min", and the rest of the method is the same as in Example 5, so that a 2D / 3D perovskite solar cell with an RP-type 2D / 3D perovskite film as a perovskite active layer can be prepared under different conditions.
[0092] Example 8
[0093] In step (4) of Example 7, "dissolve 800 mg MAPbCl3 in diethyl sulfoxide and then add 44 mg PhFACl" is replaced by "dissolve 1500 mg RbGeBr3 in diethyl sulfoxide and then add 0.02 mg PhFACl", and the rest of the method is the same as Example 7. 2D / 3D perovskite solar cells with RP-type 2D / 3D perovskite film as the perovskite active layer can be prepared under different conditions.
[0094] Example 9
[0095] The "PhFACl" in Example 7 and Example 8 was replaced by "PhDFACl" respectively, and the rest of the methods were the same as in Example 7 and Example 8, to obtain a 2D / 3D perovskite solar cell in which a DJ-type 2D / 3D perovskite film was prepared as a perovskite active layer under different conditions.
[0096] Example 10
[0097] In step (1) of Example 3, "ITO" is replaced with "FTO", in step (2), "nickel oxide" is replaced with "any one or more of poly 3-hexylthiophene (P3HT), CuSCN, Spiro-OMeTAD or p-tert-butylbenzoic acid (PTAA)", in step (5), "2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline (BCP)" is replaced with "LiFe", in step (6), "metal Ag" is replaced with "Au or C", and the remaining methods are the same as in Example 3, to obtain inverted perovskite solar cells with RP-type 2D / 3D perovskite films formed of different materials as the perovskite active layer.
[0098] Embodiment 11
[0099] In step (1) of Example 4, "ITO" is replaced with "FTO", in step (2), "nickel oxide" is replaced with "any one or more of poly 3-hexylthiophene (P3HT), CuSCN, Spiro-OMeTAD or p-tert-butylbenzoic acid (PTAA)", in step (5), "2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline (BCP)" is replaced with "LiFe", in step (6), "metal Ag" is replaced with "Au or C", and the remaining methods are the same as in Example 4, to obtain inverted perovskite solar cells with DJ-type 2D / 3D perovskite films formed of different materials as the perovskite active layer.
[0100] The performance of the perovskite solar cells prepared under different conditions in Examples 7 to 11 was also tested according to the method of the perovskite solar cells in Examples 5 and 6. The results were similar to the performance of the perovskite solar cells in Examples 5 and 6, which can further prove that adding formamidine organic spacer ligands (PhFA or PhDFA) to the perovskite active layer of the perovskite solar cell can improve the photoelectric conversion efficiency of the perovskite solar cell and increase the stability.
[0101] In summary, the present invention provides a 2D / 3D perovskite constructed based on formamidine spacer ligands, which can be mainly divided into two cases: one is to construct a DJ-type 2D / 3D perovskite by adding a diformamidine organic spacer ligand into the 3D perovskite precursor solution, which can eliminate the van der Waals gap and strengthen the interaction between the inorganic layers; the second is to use a single formamidine spacer ligand to construct an RP-type 2D / 3D perovskite as a comparison. Studies have found that the 2D perovskites formed by the two formamidine spacer ligands significantly improve the crystallization quality of the film. Further studies have shown that the DJ-type 2D / 3D perovskite constructed with a diformamidine spacer ligand has a larger grain size, better band matching, lower defect state density, and more efficient carrier transport. Finally, the RP-type 2D / 3D perovskite solar cell constructed based on a single formamidine spacer ligand achieved a photoelectric conversion efficiency of 24.51%, and the DJ-type 2D / 3D perovskite solar cell constructed based on a double formamidine spacer ligand achieved a photoelectric conversion efficiency of 25.02%. Most importantly, the environmental stability, high temperature stability, and operational stability of the 2D / 3D perovskite solar cell constructed based on the formamidine spacer ligand are significantly improved compared to the 3D perovskite solar cell. The technology disclosed in the present invention is of great significance to accelerating the commercialization process of perovskite solar cells.
[0102] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A method for preparing 2D / 3D perovskite based on formamidine spacer ligands, It is characterized in that The preparation method is as follows: an organic spacer ligand is introduced into a perovskite precursor solution, and then spin-coated on a substrate, and an anti-solvent is added dropwise before the spin-coating process is completed, and then placed on a hot stage for annealing, so as to obtain a 2D / 3D perovskite; The perovskite precursor solution is ABX 3 Type precursor fluid; The organic spacer ligand is a formamidine spacer ligand.
2. The preparation method according to claim 1, It is characterized in that The anti-solvent is chlorobenzene, wherein the anti-solvent is added within the last 5 to 10 seconds before the end of the spin coating process; The ABX 3 A in the precursor solution includes MA + , FA + , Cs + or Rb + Any one or more of B including Pb 2+ Sn 2+ Or Ge 2+ Any one or more of, X includes Cl - Br - or I - Any one or more of the following; The ABX 3 The solvent in the precursor solution is any one or more of dimethyl sulfoxide, diethyl sulfoxide, N,N-dimethylformamide, N,N-diethylformamide, N,N-dimethylacetamide or N-methylpyrrolidone.
3. The preparation method according to claim 1, It is characterized in that The formamidine spacer ligand contains at least one formamidine group; The carboxamidine spacer ligand is any one of benzamidine hydrochloride or benzadiamine hydrochloride; The ABX 3 ABX in perovskite precursor solution 3 The mass ratio of the ligand to the formamidine spacer is 800-1500:0.02-44.
0.
4. The preparation method according to claim 1, It is characterized in that The spin coating process is specifically as follows: firstly, the coating is performed at a rotation speed of 1000 to 2000 rpm for 10 to 20 seconds, and then the coating is continued at a rotation speed of 2000 to 4000 rpm for 30 to 50 seconds; The annealing is specifically: annealing on a hot plate at 100-150° C. for 30-60 minutes.
5. A 2D / 3D perovskite constructed based on formamidine spacer ligands prepared by the method according to any one of claims 1 to 4.
6. The 2D / 3D perovskite according to claim 5, It is characterized in that The 2D perovskite in the 2D / 3D perovskite constructed based on the formamidine spacer ligand is any one of the RP-type 2D perovskite and the DJ-type 2D perovskite, and the 3D perovskite in the 2D / 3D perovskite constructed based on the formamidine spacer ligand is ABX 3 Type perovskite, the 2D / 3D perovskite in the 2D / 3D perovskite constructed based on the formamidine spacer ligand is an RP type 2D / 3D perovskite or a DJ type 2D / 3D perovskite.
7. Use of the 2D / 3D perovskite constructed based on formamidine spacer ligands according to any one of claims 5 to 6 in the preparation of inverse perovskite solar cells.
8. An inverted perovskite solar cell, which is composed of a conductive substrate layer, a hole transport layer, a bottom interface modification layer, a perovskite active layer, an electron transport layer, a cathode interface layer and a back electrode layer from bottom to top. It is characterized in that The perovskite active layer is a 2D / 3D perovskite constructed based on a formamidine spacer ligand as described in any one of claims 5 to 6.
9. The inverted perovskite solar cell according to claim 8, It is characterized in that The material of the conductive substrate layer is any one of ITO and FTO; The material of the hole transport layer is any one or more of nickel oxide, poly 3-hexylthiophene, CuSCN, Spiro-OMeTAD or p-tert-butylbenzoic acid; The material of the bottom interface modification layer is Al 2 O 3 ; The materials of the electron transport layer are poly(butyl methacrylate), TiO 2 or CeO 2 Any one or more of the following; The material of the cathode interface layer is any one or more of 2,9-dimethyl-4,7-biphenyl-1,10-phenanthroline or LiF; The material of the back electrode layer is any one or more of Ag, Au or C.
10. The method for preparing the inverse perovskite solar cell according to any one of claims 8 to 9, It is characterized in that The preparation method comprises the following steps: (1) adding the material of the conductive substrate layer to a glass cleaning agent and ultrasonically cleaning it for 20 to 30 minutes, and then ultrasonically cleaning it with deionized water for 3 to 6 times, and then cleaning it with ethanol and isopropanol for 2 to 4 times respectively, and drying it with nitrogen to obtain a clean conductive substrate layer; (2) dissolving the material of the hole transport layer in deionized water, filtering it with a water filter head, and then dripping it onto the clean conductive substrate layer in step (1) using a pipette, spin coating it at a speed of 2500 to 5500 rpm for 30 to 60 seconds, and annealing it at 150 to 200° C. for 10 to 30 minutes to form a hole transport layer on the conductive substrate layer; (3) dissolving the material of the bottom interface modification layer in isopropanol, using a pipette to draw 50-100 μL and evenly smearing it on the hole transport layer, spin coating at a speed of 2500-5000 rpm, and annealing on a hot plate at 100-120° C. for 10-20 min to form a bottom interface modification layer on the hole transport layer; (4) Introducing the amidino organic spacer ligand into ABX 3 A 2D / 3D perovskite precursor solution is prepared by using a pipette to draw 50 to 100 μL of the solution and evenly apply it on the bottom interface modification layer. The first step of spin coating is performed at a rotation speed of 1000 to 2000 rpm for 10 to 20 seconds, and then the second step of spin coating is performed at a rotation speed of 2000 to 4000 rpm for 30 to 50 seconds. At the end of the last 5 to 10 seconds before the end of the second step of spin coating, 150 to 300 μL of chlorobenzene is added as an anti-solvent, and then annealed on a hot stage at 100 to 150° C. for 30 to 60 minutes to form a 2D / 3D perovskite film, i.e., a perovskite active layer, on the bottom interface modification layer. (5) dissolving the material of the electron transport layer in chlorobenzene, using a pipette to draw 30 to 60 μL and evenly applying it on the perovskite active layer in step (4), and performing spin coating at a speed of 2500 to 5000 rpm for 40 to 60 seconds to form an electron transport layer on the perovskite active layer; (6) dissolving the material of the cathode interface layer in isopropanol, using a pipette to draw 30 to 50 μL and evenly applying it on the electron transport layer, and spin coating at a speed of 800 to 2500 rpm to form the cathode interface layer; (7) In step (6), the cathode interface layer is provided with a vacuum degree of less than 1×10 -4 The material of the back electrode layer was evaporated at a pressure of 1.25 Pa to form a back electrode layer with a thickness of 80 to 120 nm.