Sliding member and internal combustion engine provided with same

By using 35 or more and 90 or less area % of molybdenum silicide iron-based alloy hard particles in sliding parts to form a particle aggregate, the problem of difficulty in replacing cobalt-based hard particles in the existing technology is solved, and realization of Wear resistance and cost effectiveness at high temperatures.

CN118871601APending Publication Date: 2024-10-29NISSAN MOTOR CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094189.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-28
Filing Date
2022-12-13
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the prior art, it is difficult for hard particles using iron-based alloys to achieve the same wear resistance as cobalt-based hard particles at high temperatures, and cobalt-based hard particles are expensive and difficult to obtain.

Method used

By using 35 area % or more and 90 area % or less of molybdenum silicide iron-based alloy hard particles in the sliding member, a particle aggregate is formed and the matrix particles are combined to improve wear resistance.

Benefits of technology

It achieves the same wear resistance as using cobalt-based hard particles at high temperatures, and avoids the high cost problem of cobalt-based hard particles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure FT_1
    Figure FT_1
  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

This sliding member is provided with, on at least the surface thereof, a particle aggregate of base material particles and hard particles. Furthermore, the hard particles are iron-based alloy particles containing 35-90% by area (inclusive) of molybdenum silicide, and therefore, it is possible to provide a sliding member having wear resistance equivalent to that when cobalt-based hard particles are used.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a sliding component, and more particularly to a sliding component including a particle aggregate in which hard particles are dispersed in a particle group in a matrix particle phase, and an internal combustion engine including the sliding component. Background Art

[0002] In order to cope with the higher performance and higher output of automobile engines, in parts such as valve seats that require wear resistance at high temperatures, the wear resistance and other properties are generally satisfied by imparting cobalt-based hard particles having a hard phase to the matrix particle phase.

[0003] The above-mentioned cobalt-based hard particles are not only expensive but also difficult to obtain in recent years. Therefore, there is a demand for sliding parts having wear resistance up to a high temperature range without using cobalt.

[0004] Patent document 1 discloses that hard particles having a hard phase of molybdenum silicide dispersed in a matrix phase of an iron-based alloy at 3 to 30 area % are used as a substitute material for cobalt-based hard particles having a hard phase, and that the wear resistance of sliding parts can be improved by using a sintered alloy of a mixed powder containing the hard particles.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent No. 3852764

[0008] Problems to be solved by the invention

[0009] However, the proposal described in Patent Document 1 cannot achieve wear resistance equivalent to that of a sliding member using cobalt-based hard particles having a hard phase, and thus there is room for improvement. Summary of the invention

[0010] The present invention has been made in view of the problems of the prior art, and an object of the present invention is to provide a sliding part having wear resistance equivalent to that of a conventional material using cobalt-based hard particles having a hard phase without using the cobalt-based hard particles.

[0011] Technical solutions to solve problems

[0012] The present inventors have repeatedly conducted intensive studies to achieve the above-mentioned object and have found that the above-mentioned object can be achieved by using hard particles of an iron-based alloy containing 35 area % or more and 90 area % or less of molybdenum silicide, thereby completing the present invention.

[0013] That is, the sliding component of the present invention includes a particle assembly of base particles and hard particles at least on the surface.

[0014] Furthermore, the sliding component is characterized in that the hard particles are iron-based alloy particles containing 35 area % or more and 90 area % or less of molybdenum silicide.

[0015] Furthermore, the present invention provides an internal combustion engine, characterized by including the sliding member.

[0016] Effects of the Invention

[0017] According to the present invention, since hard particles of an iron-based alloy containing a desired amount of molybdenum silicide are used, it is possible to provide a sliding part having wear resistance equivalent to that of a case where cobalt-based hard particles having a hard phase are used. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a Fe-Mo phase diagram; here, MoFe2 is the Laves phase, Mo5.1Fe7.9 is the μ phase, and Mo0.38Fe0.62 is the R phase. DETAILED DESCRIPTION

[0019] The sliding component of the present invention will be described in detail.

[0020] The sliding member of the present invention comprises a particle assembly of matrix particles and hard particles at least on the surface, wherein the hard particles are iron-based alloy particles containing 35 area % or more and 90 area % or less of molybdenum silicide.

[0021] In the present invention, "particle aggregate" is an aggregate in which particles (granules) are not completely melted but the surface of the particles is locally softened or melted, and the contact parts of adjacent particles are solidified and combined to form an integrated body. The sliding part of the present invention can be formed as a whole by the above-mentioned particle aggregate, or it can have a coating film formed by the above-mentioned particle aggregate on the surface of the substrate.

[0022] The particle aggregate improves the wear resistance of the sliding part by dispersing hard particles in the matrix particle group.

[0023] <Hard particles>

[0024] In the particle assembly of the present invention, the hard particles are iron alloy particles containing hard molybdenum silicide. The iron alloy particles have a molybdenum silicide content of 35 area % or more and 90 area % or less and a high molybdenum silicide content, so they can exhibit wear resistance equivalent to that of hard particles containing cobalt.

[0025] When the content of molybdenum silicide is less than 35 area %, hard particles with sufficient hardness cannot be obtained. When it exceeds 90 area %, the silicon (Si) content of the hard particles increases, the toughness of the hard particles themselves decreases, and the hard particles become brittle, thereby reducing wear resistance.

[0026] The hard particles of the iron-based alloy contain, in order of the elements contained in large amounts, iron (Fe) as a first element, molybdenum (Mo) as a second element, and silicon (Si) as a third element, and the content of the silicon is preferably 2.3 mass % or more and 16 mass % or less.

[0027] When the silicon content is 2.3 mass % or more, molybdenum silicide is easily precipitated in the hard particles, and the hardness of the hard particles increases. When the silicon content is 16 mass % or less, a decrease in the toughness of the hard particles can be prevented.

[0028] The molybdenum silicide preferably contains a Laves phase (Mo(Fe, Si)2 or Mo(Fe, Si), wherein these (Fe, Si) may contain metal elements below the fourth element). The Laves phase is a metastable phase that decomposes at a relatively low temperature of around 900°C. Therefore, it is exposed on the sliding surface of an internal combustion engine such as a valve seat and oxidized to form molybdenum oxide having lubricity, thereby improving wear resistance.

[0029] The content of molybdenum silicide in the Laves phase (hereinafter sometimes simply referred to as “Laves phase”) of the hard particles is preferably 2.0 area % to 90 area %, more preferably 10 area % to 85 area %, and preferably 30 area % to 80 area %.

[0030] All molybdenum silicides in the hard particles may be Laves phases, and therefore the upper limit of the content of the Laves phase in the hard particles is 90 area %.

[0031] The hard particles containing the Laves phase can be formed by melting an iron-based alloy containing molybdenum (Mo) and silicon (Si) and having iron (Fe) as a main component, homogenizing the alloy, and then precipitating molybdenum silicide.

[0032] like Figure 1 As shown in the Fe-Mo phase diagram, molybdenum silicide forms μ phase and R phase in addition to Laves phase. The above-mentioned Laves phase precipitates at a lower temperature than the μ phase and R phase of molybdenum silicide. Therefore, in order to form the Laves phase, it is necessary to appropriately adjust the cooling rate.

[0033] Specifically, the casting sheet can be formed by pulverizing the iron-based alloy of the above composition into a melt and slowly cooling it, or by blowing water or gas onto the molten iron-based alloy to solidify the fine droplets and particle them by water atomization or gas atomization, but it is preferably produced by water atomization or gas atomization.

[0034] The hard particles obtained by pulverizing the cast pieces of the iron-based alloy described above form a Laves phase because the cooling rate during the production of the cast pieces is slow. However, since the precipitates of molybdenum silicide are easily coarsened, the hardness of the pulverized hard particles and the content of molybdenum silicide are easily varied.

[0035] In addition, the water atomization method and the gas atomization method are generally methods for rapidly solidifying the molten metal so that the components dissolved in the parent metal are sealed in the state of solid solution in the parent phase without precipitation. Therefore, under normal conditions, the Laves phase is not formed.

[0036] In the water atomization method and gas atomization method of the present invention, by adjusting the pressure of water or gas blown onto the molten metal, the dripping speed of the molten metal, the size of the droplets, etc., the cooling rate is slowed down compared to the conventional atomization method, and hard particles precipitated from the Laves phase can be formed.

[0037] Specifically, although it depends on the composition of the iron-based alloy, especially the silicon content, cooling at 104 to 102 K / sec can precipitate molybdenum silicide with a crystallite size of 0.1 to 3 μm, forming hard particles with uniform hardness in which the molybdenum silicide is finely dispersed.

[0038] The mesh size of the sieve for adjusting the particle size of the hard particles is preferably adjusted to 100 or more and 500 or less. In particular, the mesh size of the sieve when manufacturing the particle aggregate using the sintered alloy described later is preferably adjusted to 100 or more and 150 or less, and the mesh size of the sieve when forming by cold spraying is preferably adjusted to 350 or more and 500 or less. By increasing the mesh size of the sieve and reducing the particle size of the hard particles, a dense particle aggregate can be formed.

[0039] <Base material particles>

[0040] As the base material particles, metal or alloy particles currently used for parts requiring wear resistance at high temperatures such as valve seats can be used, and copper-based alloy particles or iron-based alloy particles containing copper (Cu) or iron (Fe) as a main component (50 mass % or more) are preferred.

[0041] The copper-based alloy particles form heat transfer paths with copper having high thermal conductivity, so that the thermal conductivity of the particle aggregate becomes high and the cooling performance is improved, and thus, as a result, the heat resistance is improved.

[0042] Examples of the copper-based alloy particles include Cu—Ni—Si alloy particles, Cu—Cr alloy particles, Cu—Zr alloy particles, and Cu—Ti alloy particles. Among them, Cu—Ni—Si alloy particles are preferred.

[0043] Since nickel easily combines with silicon to precipitate in Cu-Ni-Si alloy particles, a structure of nickel silicide precipitation is formed in the matrix, which is precipitation-strengthened, and the hardness of the matrix particles themselves becomes higher, which can combine with the above-mentioned hard particles to improve wear resistance.

[0044] As the iron-based alloy particles, Fe-Mo alloy particles, Fe-Cr alloy particles, high-speed steel such as SKH53, etc. can be used. In addition, pure Fe particles can be used in which C diffuses to form an Fe-C alloy by mixing with graphite particles and sintering.

[0045] Furthermore, if the copper-based alloy particles and the iron-based alloy particles are solid solution particles, when forming a particle aggregate by cold spraying described later, the particles are strongly bonded to each other and precipitated and solidified, and wear resistance can be further improved.

[0046] The solid solution particles can be produced by a water atomization method or a gas atomization method.

[0047] The average particle size (D50) of the substrate particles is preferably 20 μm to 40 μm. The average particle size of the particles is measured by a laser diffraction / scattering method using MT3000 manufactured by Microtrac BEL Corporation.

[0048] <Method of manufacturing sliding parts>

[0049] The above-mentioned sliding part can be produced as follows: by cold spraying, warm spraying, etc., by non-melting blowing raw material particles containing the above-mentioned matrix material particles and hard particles onto the surface of the substrate, covering the surface of the substrate with a particle aggregate, or by stamping and sintering the above-mentioned raw material particles.

[0050] Preferably, the content of hard particles in the raw material particles when the raw material particles are press-formed and sintered is 50 area % or less, and the content of hard particles in the particle assembly when the substrate surface is coated by cold spraying or the like is 20 area % or less. By taking into account hardness, strength and coolability within the above range, wear resistance can be improved.

[0051] (Cold spray)

[0052] Cold spraying is a method in which raw material particles are not melted or vaporized but collide with a substrate in a non-molten solid phase with an inert gas in a supersonic flow to form a coating layer of particle aggregates.

[0053] Unlike methods such as thermal spraying that melt and integrate raw material particles, cold spraying can prevent changes in the properties of raw material particles caused by heat, and thus can form a coating layer of the particle aggregate without changing the molybdenum silicide in the hard particles.

[0054] In addition, when the above-mentioned matrix material particles are solid solution particles, before the matrix material particles in the solid phase collide with the substrate, because the matrix material particles have not yet precipitated and solidified, the parent material (substrate) particles undergo plastic deformation and absorb the stress of the collision, thereby preventing the hard particles from breaking or rebounding.

[0055] In addition, the solid-solution components inside the matrix particles are precipitated by the energy of the collision to form crystallites with a grain size of 5 to 50 nm, and the matrix particles become precipitated and solidified copper-based alloy particles or iron-based alloy particles, thereby improving wear resistance.

[0056] Then, due to the collision of the raw material particles, part of the kinetic energy is converted into thermal energy, and the surfaces of the raw material particles are partially melted and solidified, whereby the raw material particles are bonded to each other to form a particle aggregate in which hard particles are dispersed in a group of matrix particles.

[0057] At this time, since the surface of the raw material particles is partially melted, diffusion occurs and precipitates such as intermetallic compounds are generated. However, since the temperature of the substrate and the raw material particles is below the melting point of the raw material particles, the locally melted portion is quenched, and therefore, there is no period for crystal growth of the precipitates.

[0058] Therefore, nanocrystals or amorphous materials are formed near the bonding interface between the substrate and the particles and near the bonding interface between the particles.

[0059] Whether the interface between particles is amorphous or microcrystalline can be confirmed by projecting a diffraction pattern onto a detector surface using electron backscatter diffraction (EBSD) using a scanning electron microscope (SEM) and analyzing the crystal orientation based on the projected pattern.

[0060] The speed at which the raw material particles including the substrate particles and the hard particles are blown is preferably 300 to 1200 m / s, more preferably 500 to 1200 m / s.

[0061] The pressure of the working gas for blowing the raw material particles is preferably 2 to 7 MPa, more preferably 3.5 to 7 MPa. When the pressure of the working gas is lower than 2 MPa, the particle velocity cannot be obtained and the porosity may increase.

[0062] The temperature of the working gas depends on the type and particle size of the raw material particles, but is preferably 400 to 1000°C, and more preferably 600 to 1000°C.

[0063] If the working gas temperature is lower than 400°C, the raw material particles are difficult to plastically deform, the porosity increases, and the wear resistance is sometimes reduced. On the other hand, if the working gas temperature exceeds 1000°C, it is too close to the melting point of the raw material particles and is likely to block the throat of the nozzle.

[0064] Examples of the working gas include nitrogen gas and helium gas. These gases may be used alone or in combination.

[0065] The thickness of the coating film also depends on the temperature of the part where the sliding member is used and the sliding environment, and is, for example, preferably 0.05 to 5.0 mm, more preferably 0.1 to 1.0 mm.

[0066] If it is less than 0.05 mm, the strength of the coating itself is insufficient, and plastic deformation may sometimes occur when the strength of the substrate is low. In addition, if it exceeds 5.0 mm, the coating may be easily peeled off due to the relationship between the residual stress generated when the coating is formed and the interface adhesion.

[0067] The substrate is not particularly limited, and metals currently used as sliding parts of internal combustion engines can be used. However, aluminum alloys have high thermal conductivity and can be preferably used.

[0068] Examples of the aluminum alloy include AC2A, AC8A, AC4CH, and ADC12 specified in Japanese Industrial Standards.

[0069] (sintering)

[0070] As a sintering method, the base material particles and the hard particles are press-formed and sintered at a temperature not higher than the melting point of the base material particles and the hard particles, thereby forming a sliding member.

[0071] <Particle aggregate>

[0072] The porosity of the particle assembly is preferably 20 area % or less, more preferably 4 area % or less, and further preferably 1 area % or less. The particle assembly has a small number of pores and is dense, thereby improving the strength of the particle assembly and the wear resistance of the sliding part.

[0073] The scanning electron microscope image (SEM image) is binarized by image processing, and the porosity of the particle aggregate and the area ratio of the matrix particles and the hard particles can be calculated by image analysis.

[0074] The above sliding parts are excellent in wear resistance at high temperatures and therefore can be suitably used for sliding parts such as valve seats, valve lifters, pistons, piston rings, piston pins, cylinders, crankshafts, camshafts, and connecting rods of internal combustion engines.

[0075] Example

[0076] Hereinafter, the present invention will be described in detail by way of examples, but the present invention is not limited to the following examples.

[0077] (Cold spray method)

[0078] The hard particles and matrix particles in a solid solution state shown in Table 1 below were cold sprayed under the following conditions to form a coating layer on the surface of a base material in the shape of a valve seat, and then finished to produce a sliding part.

[0079] Cold spray equipment: PCS-1000 manufactured by Plasma Technology Co., Ltd.

[0080] Working gas: Nitrogen

[0081] Working gas temperature: 600℃~1000℃

[0082] Working gas pressure: 4MPa~7MPa

[0083] Spraying distance: 20mm~35mm

[0084] (Sintering method)

[0085] The hard particles and matrix material particles in the solid solution state shown in the following Table 1 are compressed at a molding pressure of 6.5 ton / cm2 into a valve seat shape with an outer diameter of 30 mm, an inner diameter of 22 mm, and a height of 8 mm. The molded body is sintered at 1130°C in an ammonia decomposition gas for 60 minutes and then cut to make a sliding part.

[0086] <Evaluation>

[0087] The sliding components were evaluated by the following methods. The evaluation results are shown in Table 1 together with the production conditions.

[0088] (Wear test)

[0089] Test conditions

[0090] Test method: Valve seat single body knock wear test (Testing equipment: manufactured by Takachiho Seiki Co., Ltd.)

[0091] Test temperature: 300℃

[0092] Number of seats: 1.44 million times (3000cpm×8hr)

[0093] Other material (valve): JISS UH35

[0094] Evaluation items: Valve seat, valve face wear (shape measurement)

[0095] (Molybdenum silicide in hard particles)

[0096] Analysis method: The phase ratio of molybdenum silicide was determined by X-ray diffraction (XRD).

[0097] The crystal structure is identified from the distribution of the peaks of the diffraction angle, and the existence ratio (mass %, volume %) of each phase is estimated from the size of the peak. It should be noted that, needless to say, volume % is equivalent to area %.

[0098] Analysis equipment: SmartLab, a horizontal X-ray diffraction device manufactured by Rigaku Corporation

[0099] Detector: 2D detector (HyPix3000)

[0100] After measuring the ratio of each phase by the above method, the Laves phase, μ phase, R phase, other silicides, and the mother phase are identified using STEM+EDX and nano-diffraction within a radius of several nanometers to obtain the ratio of each phase.

[0101] (Porosity)

[0102] The cross-section of the particle aggregate was photographed in five fields of view using the SEM composition image with an image field range of 350 μm wide and 263 μm long, and the image was binarized using an image processing device to calculate the porosity. In addition, the area ratio of the hard particles was calculated using the image, and the area ratio of the matrix material particles was obtained as the remainder.

[0103]

[0104]

[0105]

[0106]

[0107]

[0108]

[0109] Comparison between Comparative Examples 1 to 7 and Examples 1 to 14 shows that when the hard particles contain 35 area % or more of molybdenum silicide, wear resistance is improved, and the arrangement of components containing TRIBALOY (registered trademark) T-400, a cobalt-based hard particle having a hard phase, is achieved.

[0110] Comparison of Examples 6 to 11 shows that as the Si content of the hard particles increases, the amount of molybdenum silicide increases, and the wear resistance improves.

[0111] In Comparative Example 2, the Si content was low and molybdenum silicide was not sufficiently precipitated.

[0112] Although Example 6 has less molybdenum silicide than Examples 1 and 2, it is excellent in wear resistance. Therefore, it can be seen that if the molybdenum silicide in the Laves phase is large, the wear resistance is improved.

Claims

1. A sliding part, comprising a particle assembly of matrix particles and hard particles at least on the surface, It is characterized in that The hard particles are iron-based alloy particles containing 35 area % or more and 90 area % or less of molybdenum silicide.

2. The sliding member according to claim 1, It is characterized in that The hard particles contain at least iron (Fe), molybdenum (Mo), and silicon (Si) in order of the element with the highest content by mass %. The silicon content is 2.3 mass % or more and 16 mass % or less.

3. The sliding component according to claim 1 or 2, It is characterized in that The molybdenum silicide includes a Laves phase.

4. The sliding member according to claim 3, It is characterized in that The hard particles contain 2 area % or more and 90 area % or less of the Laves phase.

5. The sliding member according to claim 3, It is characterized in that The hard particles contain 10 area % or more and 85 area % or less of the Laves phase.

6. The sliding member according to claim 3, It is characterized in that The hard particles contain 30 area % or more and 80 area % or less of the Laves phase.

7. The sliding member according to any one of claims 1 to 6, It is characterized in that The matrix material particles are copper-based alloy particles or iron-based alloy particles.

8. The sliding member according to any one of claims 1 to 7, It is characterized in that The base material particles and the hard particles are blown onto a substrate to deform and stack them.

9. The sliding member according to any one of claims 1 to 7, It is characterized in that The matrix material particles and the hard particles are sintered.

10. An internal combustion engine, It is characterized in that A sliding member according to any one of claims 1 to 9 is provided.