Conductive particles, adhesive film for circuit connection and manufacturing method therefor, and connection
By using conductive particles with low irregularity in the adhesive film and applying magnetic dispersion technology, the problem of insufficient dispersion of conductive particles is solved, an adhesive film for circuit connection with a high monodispersity rate is realized, and the insulation and insulation between electrodes are improved. Capturing properties ensure stable connection between electrodes.
Patent Information
- Application Number
- CN202380025450.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-09
- Filing Date
- 2023-03-06
- Publication Date
- 2024-10-29
AI Technical Summary
In the prior art, the conductive particles in the adhesive film have insufficient dispersion, making it difficult to cope with the narrowing of electrode intervals and the reduction of electrode area, resulting in unstable connections.
Conductive particles P are used, which have sub-particles with an irregularity of 2.0 or less. They are dispersed in the adhesive layer by applying magnetic force through a magnetic field to form an adhesive film for circuit connection with a high monodispersity rate, and the electrode is realized through thermocompression bonding technology. stable connection.
It improves the insulation between adjacent electrodes and the capture of conductive particles in circuit connection, ensuring stable connection and high reliability between electrodes.
Smart Images

Figure CN118872005A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a conductive particle, an adhesive film for circuit connection and a method for producing the same, and a connection structure and a method for producing the same. Background Art
[0002] In the past, for example, as an adhesive material for connecting a liquid crystal display to a tape carrier package (TCP), connecting a flexible printed circuit board (FPC) to a TCP, or connecting an FPC to a printed circuit board, an adhesive film for circuit connection (e.g., an anisotropic conductive adhesive film) in which conductive particles are dispersed in an adhesive is used. Furthermore, when a semiconductor silicon chip is mounted on a substrate, a so-called chip on glass (COG) is performed in which the semiconductor silicon chip is directly mounted on the substrate instead of the conventional wire bonding, and an adhesive film for circuit connection (e.g., anisotropic conductive adhesive film) is also used here. Here, "anisotropic conductivity" means that the semiconductor silicon chip is conductive in the direction of pressure application and maintains insulation in the direction of non-pressure application.
[0003] In recent years, with the development of electronic devices, the wiring density and circuit functionality are developing. As a result, a connection structure with a narrow interval between connecting electrodes is required, and the bump electrodes of the connecting components are gradually reduced in area. In order to obtain a stable electrical connection in the reduced-area bump connection, a sufficient number of conductive particles are required to be interposed between the bump electrode and the circuit electrode on the substrate side.
[0004] In this regard, a method of applying external force to the conductive particles in the adhesive film to separate the conductive particles from each other and improve the insulation between adjacent electrodes and the capture property of the conductive particles (connectivity between opposing electrodes) has been studied. For example, in Patent Document 1, the following method is proposed: a conductive particle-attached film is prepared in which a laminate having an adhesive layer provided on a biaxially stretchable film and conductive particles having an average particle size of 1 to 8 μm are densely filled on the laminate, and the conductive particles are separated from each other by biaxially stretching the conductive particle-attached film.
[0005] Previous technical literature
[0006] Patent Literature
[0007] Patent Document 1: Japanese Patent Application Publication No. 2011-091049 Summary of the invention
[0008] Technical issues to be solved by the invention
[0009] However, in the method described in Patent Document 1, the dispersion of the conductive particles in the adhesive film tends to be insufficient, making it difficult to cope with the further narrowing of the electrode interval and the further reduction of the electrode area. Therefore, it is required to develop a method for producing an adhesive film for circuit connection that can better disperse the conductive particles in the adhesive film and achieve higher conductive particle capture performance.
[0010] Therefore, the main purpose of the present invention is to provide an adhesive film for circuit connection, which contains well-dispersed conductive particles and can improve the insulation between adjacent electrodes in a connection structure and the capture property of the conductive particles, and a method for manufacturing the same, and to provide conductive particles of the conductive particles used as the adhesive film for circuit connection, and a connection structure obtained using the adhesive film for circuit connection and a method for manufacturing the same.
[0011] Means for solving technical problems
[0012] The present invention provides the following [1] to
[17] in several aspects.
[0013] [1] A conductive particle for producing an adhesive film for circuit connection having a monodispersity of 90.0% or more, the conductive particle comprising a conductive mother particle and a daughter particle covering the surface of the mother particle, wherein the particle radius and the particle diameter of the daughter particle obtained by SEM observation at a magnification of 30,000 times are respectively defined as r X and X , the particle diameter d X The average value of the sub-particles, that is, the average particle size of the sub-particles is set as d Y When the irregularity of the sub-particles is obtained by the following formula (1), it is less than 2.0.
[0014] Irregularity = D / r Y ×100(1)
[0015] [In formula (1), r Y Indicates that the diameter is equal to d Y The radius of the virtual sphere, D represents the particle radius r of the sub-particle X With the radius r of the virtual sphere Y The average of the absolute differences.]
[0016] [2] The conductive particle according to [1], wherein
[0017] The coverage rate of the surface of the mother particle by the child particles is 40.0% or more.
[0018] [3] The conductive particle according to [1] or [2], wherein
[0019] The CV value of the coverage of the surface of the mother particle by the child particles is 10.0% or less.
[0020] [4] The conductive particle according to any one of [1] to [3], wherein
[0021] The average particle size of the child particles determined by SEM observation at a magnification of 30,000 times was 200 to 400 nm.
[0022] [5] The conductive particle according to any one of [1] to [4], wherein
[0023] The ratio of the average particle size of the child particles obtained by SEM observation at a magnification of 30,000 times to the particle size of the mother particles obtained by SEM observation at a magnification of 25,000 times is 8.0 to 20.0.
[0024] [6] The conductive particle according to any one of [1] to [5], wherein
[0025] When a film composed of the conductive particles is formed, the contact angle between the surface of the film and water is 130° or more.
[0026] [7] The conductive particle according to any one of [1] to [6], wherein
[0027] The daughter particles contain a copolymer including an aromatic cross-linking monomer and a non-cross-linking monomer as monomer units.
[0028] [8] The conductive particle according to [7], wherein
[0029] The aromatic cross-linking monomer is divinylbenzene.
[0030] [9] The conductive particle according to [7] or [8], wherein
[0031] The non-crosslinking monomer is styrene.
[0032]
[10] The conductive particle according to any one of [7] to [9], wherein
[0033] The content of the polar group-containing monomer contained as a monomer unit in the copolymer is 2.0 mol% or less based on the total amount of the monomer units contained in the copolymer.
[0034]
[11] The conductive particle according to any one of [7] to
[10] , wherein
[0035] The copolymer is an emulsifying polymer.
[0036]
[12] The conductive particles according to any one of [1] to
[11] are used in a method for manufacturing an adhesive film for circuit connection, the method for manufacturing an adhesive film for circuit connection comprising a step of dispersing the conductive particles by applying an external force to the conductive particles in a film comprising an adhesive component and the conductive particles.
[0037]
[13] An adhesive film for circuit connection, comprising a conductive adhesive layer, the conductive adhesive layer comprising an adhesive component and the conductive particles described in any one of [1] to
[12] , wherein the monodispersity of the conductive particles in the conductive adhesive layer is 90.0% or more.
[0038]
[14] A method for producing an adhesive film for circuit connection, comprising the step of dispersing the conductive particles by applying external force to the conductive particles in a film comprising an adhesive component and the conductive particles described in any one of [1] to
[12] .
[0039]
[15] The method for producing an adhesive film for circuit connection according to
[14] , wherein:
[0040] In the above process, a magnetic field is applied to exert a magnetic force on the conductive particles, so that the conductive particles are dispersed.
[0041]
[16] A connection structure comprising:
[0042] A first component having a first electrode;
[0043] a second member having a second electrode; and
[0044] a connecting portion disposed between the first member and the second member and electrically connecting the first electrode and the second electrode to each other,
[0045] The connecting portion includes a cured product of the adhesive film for circuit connection described in
[13] .
[0046]
[17] A method for manufacturing a connection structure, comprising the following steps:
[0047] A first component having a first electrode and a second component having a second electrode are thermally pressed together with the circuit-connecting adhesive film described in
[13] interposed between the first component and the second component, so that the first electrode and the second electrode are electrically connected to each other.
[0048] Effects of the Invention
[0049] According to the present invention, there can be provided an adhesive film for circuit connection that contains well-dispersed conductive particles and can improve the insulation between adjacent electrodes in a connection structure and the ability to capture conductive particles, and a method for manufacturing the same. Furthermore, according to the present invention, there can be provided a conductive particle used as the conductive particle in the adhesive film for circuit connection. Furthermore, according to the present invention, there can be provided a connection structure obtained by using the adhesive film for circuit connection, and a method for manufacturing the same. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 This is a schematic cross-sectional view showing one embodiment of the conductive particles according to the present invention.
[0051] Figure 2 This is a schematic cross-sectional view showing one embodiment of the adhesive film for circuit connection according to the present invention.
[0052] Figure 3 Yes means Figure 2 Schematic diagram of the manufacturing process of the adhesive film for circuit connection shown in FIG.
[0053] Figure 4 It is a schematic diagram showing the state of the magnetic field application process.
[0054] Figure 5 This is a schematic cross-sectional view showing the state of the adhesive film for circuit connection after going through the magnetic field application step and the drying step.
[0055] Figure 6 It is a schematic cross-sectional view showing the state of the lamination process.
[0056] Figure 7 This is a microscope photograph showing the dispersion state of conductive particles in a conventional production method.
[0057] Figure 8 This is a microscope photograph showing the dispersion state of the conductive particles in the present production method.
[0058] Fig. 9 It is a schematic cross-sectional view showing one embodiment of the connection structure according to the present invention.
[0059] Fig.10 Yes means Fig. 9 Schematic cross-sectional view of the manufacturing process of the connection structure shown in FIG.
[0060] Fig.11 Yes means Fig.10 A schematic cross-sectional view of the subsequent process. DETAILED DESCRIPTION
[0061] In this specification, the numerical range represented by "~" indicates a range that includes the numerical values recorded before and after "~" as the minimum and maximum values, respectively. In the numerical range recorded in stages in this specification, the upper limit or lower limit of the numerical range of a certain stage can be replaced by the upper limit or lower limit of the numerical range of other stages. Moreover, in the numerical range recorded in this specification, the upper limit or lower limit of its numerical range can be replaced by the value shown in the embodiment. Moreover, the upper limit and lower limit recorded individually can be combined arbitrarily. Moreover, in this specification, "(meth)acrylate" refers to at least one of acrylate and its corresponding methacrylate. Other similar expressions such as "(meth)acryloyl" are also the same. Moreover, with respect to "A or B", as long as it includes any one of A and B, it can also include both. Moreover, unless otherwise specified, the materials exemplified below can be used alone or in combination of two or more. When a plurality of substances corresponding to each component are present in the composition, unless otherwise specified, the content of each component in the composition represents the total amount of the plurality of substances present in the composition.
[0062] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings as appropriate. However, the present invention is not limited to the following embodiments.
[0063] <Conductive particles>
[0064] Figure 1 Schematic cross-sectional view of a conductive particle according to an embodiment. The conductive particle P includes a conductive mother particle 31 and a daughter particle 32 covering the surface of the mother particle 31. Here, in this specification, conductivity means not insulating, and insulating means that the resistance value measured by a powder resistance measuring device is greater than 1.0E+09Ω.
[0065] In the conductive particles P of the present embodiment, the irregularity of the sub-particles 32 is 2.0 or less. Here, the irregularity is an index indicating the degree of deformation relative to a perfect sphere of the same particle size. When the particle radius and particle diameter of the sub-particles obtained by SEM observation at a magnification of 30,000 times are respectively set to r X and X , the particle diameter d X The average value of the average particle size of the daughter particles 32 is d Y When , it is obtained by the following formula (1).
[0066] Irregularity = D / r Y ×100(1)
[0067] [In formula (1), r Y Indicates that the diameter is equal to d Y The radius of the virtual sphere, D represents the particle radius r of the sub-particleX With the radius r of the virtual sphere Y The average of the absolute differences.]
[0068] Since the above-mentioned conductive particles P have sub-particles 32 with irregularities within the above-mentioned range, they can be preferably used to manufacture an adhesive film for circuit connection with a high monodispersity (for example, 90.0% or more). An adhesive film for circuit connection with a high monodispersity is usually manufactured by a method including the following steps, namely, a step (external force applying step) of dispersing the conductive particles by applying an external force (for example, a magnetic force) to the conductive particles in a film containing an adhesive component and conductive particles. Since the conductive particles P show good dispersibility in the external force applying step, they can be preferably used in the method for manufacturing the adhesive film for circuit connection including such an external force applying step. In this specification, the adhesive film for circuit connection manufactured by the method of dispersing the conductive particles using the above-mentioned external force is referred to as an "external force dispersion type adhesive film for circuit connection". The method for manufacturing the external force dispersion type adhesive film for circuit connection will be described in detail later.
[0069] When manufacturing an adhesive film for circuit connection, a coating liquid (paste) is generally used that uses an organic solvent with an SP value (Hildebrand solubility parameter) of 8.5 to 10.0 as a solvent. When an organic solvent with such an SP value (for example, acetone, methyl ethyl ketone, ethyl acetate, toluene, etc.) is used as a solvent for the coating liquid, the effect of the above-mentioned sub-particles 32 is significant, especially when the solvent is ethyl acetate.
[0070] The reasons for the above-mentioned effects are speculated as follows. First, when the sub-particles of the conductive particles have the property of being easily swollen by the solvent (organic solvent) in the above-mentioned coating liquid, it is speculated that the sub-particles swollen in the coating liquid are entangled and agglomerated when drying, and it becomes difficult to disperse even if the above-mentioned external force is applied. In addition, in general, since the organic solvent used to form the film has a high affinity for the adhesive component (resin, etc.) that forms the film, when the affinity of the sub-particles for the organic solvent is high, there is a tendency that the affinity of the sub-particles for the adhesive component is also high. Therefore, it is speculated that in the above-mentioned external force application process, when the conductive particles are dispersed by external force, the flow of the sub-particles is suppressed due to the adhesive component in the film. On the other hand, the small irregularity of the above-mentioned sub-particles 32 means that the sub-particles 32 are inorganic particles or organic particles with low polarity or organic-inorganic mixed particles. These particles have low affinity for organic solvents with SP values of 8.5 to 10.0, and it can be said that it is difficult to swell in the coating liquid. Therefore, it is presumed that the conductive particles P are less likely to be entangled with each other during drying and are less likely to be hindered in flow by the binder component, thereby exhibiting good dispersibility.
[0071] From the viewpoint of achieving higher dispersibility of the conductive particles P, the irregularity of the sub-particles 32 may be less than 1.5, less than 1.3 or less than 1.2. The lower limit of the irregularity is 0.1. The irregularity can be adjusted by the constituent material of the sub-particles, for example, by the addition amount of a monomer containing a polar group (such as an alkoxysilane having an ethylenically unsaturated group).
[0072] When the external force is a magnetic force (that is, when the external force application process is a magnetic field application process), from the perspective of implementing dispersion based on the magnetic field application process with higher efficiency, the conductive particles P preferably contain at least one selected from the group consisting of iron, cobalt and nickel, and more preferably contain nickel. In general, iron, cobalt and nickel are known to be ferromagnetic and are magnetized by an external magnetic field. Among them, when nickel is used, it is possible to take into account both conductivity and dispersibility caused by the application of a magnetic field at a higher level. The magnetism of the conductive particles P can be confirmed by saturation magnetization. Saturation magnetization can be measured, for example, by a vibrating sample magnetometer (VSM: Vibrating Sample Magnetmeter). From the perspective of better dispersing the conductive particles P by an external magnetic field, the saturation magnetization obtained by VSM measurement is preferably in the range of 5.0emu / g to 50emu / g.
[0073] According to the above-mentioned conductive particles P, the sub-particles become spacers, so that the conductive particles are not easily combined and agglomerated before and after the film is formed. In addition, when the sub-particles 32 have insulating properties, the effect of ensuring insulation can be obtained even if the conductive particles are connected to each other during connection. In addition, between the opposing electrodes, since the sub-particles 32 are separated from the surface of the mother particle 31, the connection reliability can be ensured even when the sub-particles 32 have insulating properties.
[0074] (Mother Particle)
[0075] The mother particles 31 are particles having conductivity. For example, metal particles made of a metal such as gold, silver, palladium, ruthenium, iridium, nickel, tungsten, molybdenum, copper, tin, solder, etc., and conductive carbon particles made of conductive carbon can be used as the mother particles 31. Figure 1 As shown, the mother particle 31 can be a core-shell particle having an insulating core particle 31a and a conductive coating layer (shell) 31b covering the core particle 31a. Among them, by setting the core particle 31a as an elastically deformable particle, the conductive particle can be elastically deformed during connection, thereby improving the capture of the conductive particle and reducing the load on the electrode, etc. From this point of view, the core-shell particle is preferred.
[0076] The core particle 31a of the core-shell particle can be a particle containing insulating glass, ceramics, plastics, etc. The core particle 31a is preferably an insulating organic core particle. The organic core particle is a particle composed of an organic compound (for example, plastic), usually containing more than 40% by mass of the organic compound. As the organic compound constituting the organic core particle, polymers of acrylic monomers, i.e., acrylic resins, polymers of olefin monomers, i.e., olefin resins, etc. can be cited. As acrylic monomers, for example, alkyl (meth) acrylates, alkanediol di (meth) acrylates, etc. can be cited. As olefin monomers, ethylene, propylene, isobutylene, butadiene, etc. can be cited.
[0077] The core particle 31a can be a hard particle or a soft particle. The preferred hardness (elastic modulus) of the core particle 31a varies depending on the application. The elastic modulus (compression elastic modulus, hereinafter referred to as "20% K value") when the core particle 31a is compressed at room temperature (e.g., 25°C) to deform it by 20% can be 0.5 to 40.0 GPa, or 1.0 to 10.0 GPa or 10.0 to 25.0 GPa. The 20% K value can be measured using Fisher Scope HM2000 (manufactured by FISCHER INSTRUMENTS KK) by the following method.
[0078] 1) At room temperature (20 to 27°C), place a particle sample on a slide glass and apply a weight toward the center of the particle.
[0079] 2) The compressive deformation modulus (K20, 20% K value) of the particle sample when it is deformed by 20% while a weight of 50 mN is applied for 50 seconds is measured and calculated according to the following formula.
[0080] K20 (compression deformation elastic modulus) = (3 / √2) × F20 × S20 -3 / 2 ×R -1 / 2
[0081] F20: Load required to deform the particle by 20% (N)
[0082] S20: Deformation of the particle when it is deformed by 20% (m)
[0083] The core particles 31a are preferably spherical. The average particle size of the core particles 31a is, for example, 1.5 to 10.0 μm, or may be 2.0 to 5.0 μm or 5.0 to 10.0 μm. The average particle size is measured by a wet flow particle size analyzer (FPIA-3000S manufactured by Spectris).
[0084] As the material constituting the coating layer 31b, it can be a metal or conductive carbon. The coating layer 31b is preferably a metal layer (a layer containing a metal as a constituent material). The metal layer can also be composed of materials containing metal compounds such as ITO, solder, etc., in addition to metals such as gold, silver, copper, platinum, zinc, iron, palladium, ruthenium, iridium, nickel, tin, chromium, titanium, aluminum, cobalt, germanium, cadmium, tungsten, and molybdenum. As the constituent material of the metal layer, from the viewpoints of corrosion resistance, nickel, palladium or gold is preferably used. The metal layer preferably contains more than 95.0% by mass of metal or metal compounds. From the viewpoint of imparting conductivity and hardness, the metal layer can include carbon compounds such as carbon nanotubes and carbon black. The core-shell particles having a metal layer as the coating layer 31b can be obtained by, for example, forming a metal layer on the surface of the core particle by sputtering, plating (for example, electroless plating) and other methods.
[0085] The coating layer 31b may be a single-layer structure or a laminated structure composed of a plurality of layers. In the case of a single-layer structure, the coating layer 31b preferably contains nickel from the viewpoints of cost, conductivity, and corrosion resistance.
[0086] From the viewpoint of improving the conduction reliability between the opposing electrodes, the thickness of the coating layer 31b can be 70nm or more, 100nm or more, or 150nm or more. From the viewpoint of easily obtaining the effect brought by the core particles, the thickness of the coating layer 31b can be 150nm or less, 170nm or less, or 200nm or less. The thickness of the coating layer 31b is as follows: after the injection molding sample is prepared by dispersing the conductive particles in the injection molding resin for injection molding, the surface of the injection molding sample is polished using ion milling (Ion milling) or the like to expose the cross section of the particles, and the average value of the thickness of 5 places measured by observing the cross section of the particles using SEM.
[0087] The surface of the mother particle 31 may be smooth, but preferably has concavities and convexities. In addition, the mother particle 31 is preferably spherical. The average particle size of the mother particle 31 is, for example, 1.7 to 10.5 μm, or may be 2.0 to 5.5 μm or 5.5 to 10.5 μm. The average particle size is the average particle size measured by a wet flow particle size analyzer (FPIA-3000S manufactured by Spectris).
[0088] (sub-particle)
[0089] The sub-particles 32 are, for example, microparticles containing an organic compound as a constituent material (organic microparticles), preferably microparticles containing an insulating organic compound as a constituent material. The sub-particles 32 may be microparticles containing an organic compound and an inorganic compound (organic-inorganic hybrid microparticles). The sub-particles 32 are preferably insulating microparticles, more preferably insulating organic microparticles.
[0090] The child particles 32 preferably contain a copolymer including an aromatic crosslinking monomer and a non-crosslinking monomer as monomer units. When the child particles 32 contain such a copolymer, the irregularity of the child particles 32 is likely to be within the above range.
[0091] The aromatic crosslinkable monomer refers to a monomer containing an aromatic hydrocarbon group and two or more crosslinkable groups. Examples of the crosslinkable group include groups containing ethylenically unsaturated groups such as a vinyl group and a (meth)acryloyl group.
[0092] As aromatic crosslinking monomers, divinylbenzene, divinylbiphenyl, divinylnaphthalene, ethoxylated bisphenol A di(methyl)acrylate, etc. can be cited. These monomers can be used alone or in combination of two or more. From the perspective of insulation, dispersibility of the film, ease of synthesis and cost, and reducing the irregularity of the daughter particles, aromatic crosslinking monomers are preferably divinylbenzene. In addition, in addition to aromatic crosslinking monomers, conjugated dienes (non-aromatic crosslinking monomers) such as butadiene and isoprene can also be used.
[0093] From the viewpoint of easily obtaining the above-mentioned irregularity, the content (crosslinking degree) of the aromatic crosslinking monomer contained as a monomer unit in the copolymer can be 2.0 to 10.0 mass %, 2.0 to 5.0 mass % or 5.0 to 10.0 mass % based on the total amount of the monomer units contained in the copolymer. When the content of the aromatic crosslinking monomer is 2.0 mass % or more, the sub-particles tend to have better solvent resistance and are easy to become relatively hard and restorative sub-particles. When the content of the aromatic crosslinking monomer is 10.0 mass % or less, the sub-particles tend to become softer particles, and have a tendency to further improve the conductive resistance of the resulting connected structure.
[0094] The non-crosslinkable monomer refers to a monomer containing one polymerizable group. Examples of the polymerizable group include groups containing ethylenically unsaturated groups such as a vinyl group and a (meth)acryloyl group.
[0095] Examples of the non-crosslinking monomer include (i) styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, α-methylstyrene, o-ethylstyrene, m-ethylstyrene, p-ethylstyrene, 2,4-dimethylstyrene, p-butylstyrene, p-tert-butylstyrene, p-hexylstyrene, p-octylstyrene, p-nonylstyrene, p-decylstyrene, p-dodecylstyrene, p-methoxystyrene, p-phenylstyrene, p-chlorostyrene, 3,4-dichlorostyrene and other styrene or derivatives thereof; and (ii) methyl acrylate, ethyl acrylate, propyl acrylate, n-butyl acrylate, isobutyl acrylate, hexyl acrylate, 2-ethylhexyl acrylate, n-octyl acrylate, dodecyl acrylate, lauryl acrylate, stearic acid ester, 2-chloroethyl acrylate, phenyl acrylate, α-methyl chloroacrylate, glycidyl acrylate, methyl methacrylate, ethyl methacrylate, propyl methacrylate, methacrylate. (Meth)acrylates such as n-butyl, isobutyl methacrylate, hexyl methacrylate, 2-ethylhexyl methacrylate, n-octyl methacrylate, dodecyl methacrylate, lauryl methacrylate, stearic methacrylate, glycidyl methacrylate, (iii) vinyl esters such as vinyl acetate, vinyl propionate, vinyl benzoate, vinyl butyrate, (iv) N-vinyl compounds such as N-vinylpyrrole, N-vinylcarbazole, N-vinylindole, N-vinylpyrrolidone, (v) (meth)acrylates containing fluoroalkyl groups such as vinyl fluoride, vinylidene fluoride, tetrafluoroethylene, hexafluoropropylene, trifluoroethyl acrylate, tetrafluoropropyl acrylate, (vi) alkoxysilanes having a (meth)acryloyl group such as 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, etc. These can be used individually by 1 type or in combination of 2 or more types.
[0096] As the non-crosslinking monomer, a monomer having an aromatic hydrocarbon group (aromatic non-crosslinking monomer) is preferred from the perspective of insulation, dispersibility in the film, ease of synthesis and cost, and styrene is more preferred. In addition, styrene is preferably used from the perspective of further reducing the irregularity of the daughter particles.
[0097] When two or more non-crosslinking monomers are used in combination, it is preferred to use a non-crosslinking monomer without a functional group and a monomer with a functional group in combination. As a monomer with a functional group, it is preferred to use (vi) alkoxysilanes such as styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, and 3-methacryloxypropyltriethoxysilane. Since this alkoxysilane produces silanol by hydrolysis, it has a tendency that the surface treatment agent described later improves the surface treatment property of the sub-particles. From the viewpoint of being easy to obtain the above-mentioned irregularity and the viewpoint of improving the contact angle, it is preferred to use dimethoxysilanes such as 3-methacryloxypropylmethyldimethoxysilane.
[0098] From the viewpoint of easily obtaining the above-mentioned irregularity, the content of the non-crosslinking monomer contained as a monomer unit in the copolymer can be 90.0 to 98.0 mass % based on the total amount of the monomer units contained in the copolymer. When the content of the non-crosslinking monomer is 90.0 mass % or more, the sub-particles tend to become softer particles, and there is a tendency to further improve the conductive resistance of the obtained connected structure. When the content of the non-crosslinking monomer is 98.0 mass % or less, there is a tendency for the sub-particles to have better solvent resistance, and it is easy to become relatively hard and restorative sub-particles.
[0099] The copolymer contained in the sub-particle 32 may contain a monomer containing a polar group as a monomer unit. For example, one or both of the aromatic cross-linking monomer and the non-cross-linking monomer may have a polar group. In the case where a part of the non-cross-linking monomer contained in the copolymer is a monomer containing a polar group, the sub-particle 32 can be synthesized stably, and the particle size control tends to be easy.
[0100] As polar groups, in addition to functional groups such as silanol, carboxyl, amino, hydroxyl, sulfonic acid, cyano, epoxy, and phosphoric acid, functional groups (alkoxysilyl) that generate these polar groups by hydrolysis can also be cited. Epoxy groups can be included as part of glycidyl groups. Specific examples of monomers containing polar groups include (meth) acrylic acid and salts thereof, styrene sulfonic acid and salts thereof, epoxy monomers containing (meth) acryloyl groups, carboxylates containing (meth) acryloyl groups, and the above-mentioned alkoxysilanes.
[0101] Examples of the (meth)acryloyl group-containing phosphoric acid monoester include mono(2-hydroxyethyl(meth)acrylate)phosphate, etc. Mono(2-hydroxyethyl(meth)acrylate)phosphate may be provided as a mixture with other components.
[0102] As an epoxy monomer containing a (meth)acryloyl group, glycidyl (meth)acrylate, 3, 4-epoxycyclohexyl (meth)acrylate, etc. are mentioned, for example.
[0103] Examples of the (meth)acryloyl group-containing carboxylic acid ester include (meth)acryloyloxyethyl succinate, (meth)acryloyloxyethyl phthalate, and (meth)acryloyloxypropyl phthalate.
[0104] From the viewpoint of further reducing the irregularity of the daughter particles, the fewer the units derived from the monomer containing polar groups in the above-mentioned copolymer, the better. From this viewpoint, the content of the monomer containing polar groups contained as monomer units in the above-mentioned copolymer can be 2.0 mol% or less, or 1.5 mol% or less or 1.0 mol% or less, based on the total amount of monomer units contained in the copolymer. From the viewpoint of ensuring the bonding point with the mother particle and improving the coverage of the mother particle by the daughter particles, the content of the monomer containing polar groups contained as monomer units in the above-mentioned copolymer can be 0.1 mol% or more, or 0.3 mol% or more or 1.0 mol% or more, based on the total amount of monomer units contained in the copolymer. From these viewpoints, the content of the polar group-containing monomer contained as a monomer unit in the above-mentioned copolymer can be 0.1 to 2.0 mol%, 0.3 to 2.0 mol%, 0.3 to 0.5 mol%, 0.5 to 1.0 mol%, 1.0 to 2.0 mol% or 1.0 to 1.5 mol%, based on the total amount of the monomer units contained in the copolymer.
[0105] Examples of methods for synthesizing the daughter particles 32 include precipitation polymerization and emulsion polymerization, among which emulsion polymerization is preferred from the viewpoints of control of irregularity, control of particle size, ease of synthesis, etc. That is, the daughter particles 32 are preferably emulsion polymerized.
[0106] In the emulsion polymerization method, polymerization is carried out by heating while stirring an emulsion composed of monomers and an aqueous medium. The emulsion can be obtained, for example, by a method in which the monomers are added to an aqueous medium and emulsified with a dispersant or the like, a method in which the monomers are added to an aqueous medium and dispersed mechanically (for example, by a homogenizer, an ultrasonic processor, a nanometer or other fine emulsifier), etc. The stirring speed can be in the range of 100 to 500 rpm (revolutions per minute). The polymerization temperature can be in the range of 40 to 90° C. The polymerization time can be in the range of 2 to 24 hours. The concentration of all monomers can be 1 to 30% by mass relative to the aqueous medium.
[0107] Examples of the aqueous medium used for emulsion polymerization include water, a mixed medium of water and a water-soluble solvent (eg, a lower alcohol), etc. From the viewpoint of preventing unintended monomer dissolution in the solvent, the aqueous medium may be water.
[0108] A polymerization initiator can be added to the above-mentioned emulsion as needed. The polymerization initiator and the monomer can be mixed in advance and the resulting mixture can be dispersed in an aqueous medium, or the polymerization initiator and the monomer can be dispersed in an aqueous medium separately. The polymerization initiator is, for example, a free radical polymerization initiator. Examples of free radical polymerization initiators include benzoyl peroxide, tert-butyl benzoate, potassium persulfate, 1,1-azobis(cyclohexane-1-carbonitrile), 2,2-azobisisobutyronitrile, 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine], and the like. These compounds can be used as compounds provided in the form of hydrates. The polymerization initiator can be used in a range of 0.1 to 7.0 parts by mass relative to 100 parts by mass of all monomers.
[0109] The emulsion may contain anionic, cationic, nonionic, zwitterionic or other surfactants as an emulsifier.
[0110] Examples of the anionic surfactant include fatty acid oils such as sodium oleate and potassium castor oil, alkyl sulfate ester salts such as sodium lauryl sulfate, ammonium lauryl sulfate, and triethanolamine lauryl sulfate, alkylbenzene sulfonates such as sodium dodecylbenzene sulfonate, alkylnaphthalene sulfonates, alkane sulfonates, dialkyl sulfosuccinates such as sodium dioctyl sulfosuccinate, alkenyl succinates (dipotassium salt), alkyl phosphates, naphthalenesulfonic acid formalin condensate, polyoxyethylene alkylphenyl ether sulfate ester salts, polyoxyethylene alkyl ether sulfates such as sodium polyoxyethylene lauryl ether sulfate, and polyoxyethylene alkyl sulfate ester salts.
[0111] Examples of the cationic surfactant include alkylamine salts such as laurylamine acetate and stearylamine acetate, and quaternary ammonium salts such as lauryltrimethylammonium chloride. Examples of the zwitterionic surfactant include lauryldimethylamine oxide, phosphate esters, and phosphite esters.
[0112] The above surfactants may be used alone or in combination of two or more. From the viewpoint of dispersion stability during polymerization, it is preferred to use anionic surfactants.
[0113] The shape of the sub-particle 32 may be spherical, flat, red blood cell-shaped (bowl-shaped), semicircular, etc., and a spherical shape is preferred.
[0114] The particle size of the sub-particles 32 may be smaller than the particle size of the mother particles 31. The ratio of the average particle size of the sub-particles 32 obtained by SEM at a magnification of 30,000 times to the particle size of the mother particles 31 obtained by SEM (scanning electron microscope) at a magnification of 25,000 times is preferably 8.0 to 20.0. In this case, the conductive particles P become a shape closer to a true sphere, and it becomes difficult to generate steric hindrance of the conductive particles in the external force application process. From the same point of view, the ratio of the above particle sizes can be greater than 8.0 or greater than 10.0, and can be less than 20.0 or less than 15.0. In addition, the specific measurement method of the above ratio is shown in the embodiments.
[0115] The average particle size of the sub-particles 32 obtained by SEM observation at a magnification of 30,000 times is preferably 200 to 400 nm. When the above average particle size is greater than 200 nm, the function of the sub-particles 32 as spacers is easily manifested. When the above average particle size is less than 400 nm, the sub-particles 32 become less likely to fall off from the mother particles 31. From the above viewpoints, the above average particle size can be greater than 250 nm or greater than 300 nm, and can be less than 350 nm or less than 280 nm. In addition, the specific measurement method of the above average particle size is shown in the embodiments.
[0116] The coverage of the surface of the mother particle 31 by the daughter particles 32 is preferably 40.0% or more. When the coverage is within this range, since the uncoated portion of the mother particle 31 becomes a junction and prevents or inhibits the conductive particles from combining with each other, it is less likely to cause defects caused by short circuits, and there is a tendency for the dispersibility of the conductive particles to be further improved. From the same point of view, the above-mentioned coverage can be 45.0% or more or 50.0% or more. The upper limit of the above-mentioned coverage is, for example, 75.0%. That is, the above-mentioned coverage can be 40.0-75.0%. Among them, the above-mentioned coverage is the average of the coverage of multiple conductive particles, and is the area ratio obtained by analyzing the SEM image obtained by observing the conductive particles by SEM (scanning electron microscope) at a magnification of 8000 times. The specific measurement method of the above-mentioned coverage is shown in the embodiment.
[0117] The CV (Coefficient of Variation) value of the above-mentioned coverage is preferably 10.0% or less. In the case of such a CV value, particles that are too insufficiently coated are not easy to exist, so it is difficult to produce defects caused by the above-mentioned conductive particles binding to each other. From the same point of view, the above-mentioned CV value can be 5.0% or less or 4.0% or less. The lower limit of the above-mentioned CV value is, for example, 0.5%. That is, the above-mentioned CV value can be 0.5 to 10.0%. Among them, the CV value of the coverage is the value obtained by dividing the standard deviation of the coverage by the above-mentioned coverage (average value).
[0118] The daughter particles 32 may be attached to the mother particles 31 via a polymer electrolyte. The polymer electrolyte will be described later.
[0119] The sub-particle 32 may be surface treated. For example, the surface of the sub-particle 32 may be coated with a silicone oligomer. The weight average molecular weight of the silicone oligomer is preferably 500 to 4000. The silicone oligomer preferably has a polymer electrolyte described later or a functional group that reacts with a functional group introduced into the sub-particle. Examples of such functional groups include silanol, glycidyl, carboxyl, amino, isocyanate, and the like. Among them, silanol or glycidyl are preferred. In addition, the functional group in the silicone oligomer may be in a state of reacting with a polymer electrolyte or a functional group introduced into the sub-particle.
[0120] The surface treatment method of the sub-particles 32 is not particularly limited, and a relatively simple method is to mix and stir a 5 to 100 mass % solution of a silicone oligomer while stirring a dispersion of particles (eg, microparticles) to become the sub-particles 32 in a heated nitrogen atmosphere.
[0121] The ratio of the average particle size of the sub-particle 32 in ethyl acetate to the average particle size in water (hereinafter referred to as the "swelling ratio") can be 1.20 or less. The average particle size in water and the average particle size in ethyl acetate are particle sizes at a cumulative value of 50% (volume basis) in the particle size distribution obtained by laser diffraction particle size distribution measurement. When the above-mentioned swelling ratio of the sub-particle 32 is 1.20 or less, it can be said that the sub-particle 32 is a particle that is not only not easily swollen by ethyl acetate but also not easily swollen by an organic solvent having an SP value close to that of ethyl acetate (for example, acetone, methyl ethyl ketone, toluene, etc.). From the viewpoint of easily obtaining the above-mentioned effect, the above-mentioned swelling ratio can be 1.15 or less or 1.10 or less. From the viewpoint of the manufacturing stability of the sub-particle and the adsorption stability to the mother particle, the above-mentioned swelling ratio can be 1.05 or more, or 1.10 or more or 1.15 or more. From these viewpoints, the swelling ratio may be 1.05 to 1.20, 1.05 to 1.15, 1.05 to 1.10, 1.10 to 1.15, or 1.15 to 1.20.
[0122] From the viewpoint of obtaining a connection structure with better conductive resistance and insulation resistance, the conductive particles P having the mother particles 31 and the daughter particles 32 described above preferably have a hydrophobic (water-repellent) surface. Specifically, when a film composed of conductive particles P is formed, the contact angle between the surface of the film and water is preferably 130°. The contact angle may be greater than 135° or greater than 137°. The upper limit of the contact angle is, for example, 140°. That is, the contact angle may be between 130° and 140°. Preferably, the contact angle is greater than the contact angle between the surface of the adhesive film for circuit connection using the conductive particles P (the surface of the conductive adhesive layer) and water by 20° or more. The contact angle can be measured by the method described in the embodiments.
[0123] The conductive particles P can be obtained by coating conductive particles serving as mother particles with particles serving as daughter particles (eg, fine particles). From the viewpoint of preventing particles from agglomerating with each other, the following method is preferably used as a coating method.
[0124] First, the surface of the conductive particles serving as the mother particles 31 is treated with a compound having a specific functional group.
[0125] When the conductive particles have a gold layer or a palladium layer on the surface, they can be treated with a compound having at least one group selected from the group consisting of a mercapto group, a thioether group, and a disulfide group and at least one group selected from the group consisting of a hydroxyl group, a carboxyl group, an alkoxy group, and an alkoxycarbonyl group. By using such a compound to treat the conductive particles, the mercapto group, the thioether group, or the disulfide group forms a coordination bond with gold or palladium, so that a hydroxyl group, a carboxyl group, an alkoxy group, or an alkoxycarbonyl group can be imparted to the conductive particles. As such a compound, thioglycolic acid, 2-mercaptoethanol, methyl thioglycolate, mercaptosuccinic acid, thioglycerol, cysteine, etc. can be cited.
[0126] When the conductive particles have a nickel layer on the surface, they can be treated with a compound having at least one group selected from the group consisting of a mercapto group, a sulfide group or a disulfide group, a carboxyl group, a silanol group, a hydroxyl group, and a nitrogen-containing group, and at least one group selected from the group consisting of a hydroxyl group, a carboxyl group, an alkoxy group, and an alkoxycarbonyl group. By using such a compound to treat the conductive particles, the silanol group, the hydroxyl group, or the nitrogen-containing group forms a strong bond with the nickel, so that a hydroxyl group, a carboxyl group, an alkoxy group, or an alkoxycarbonyl group can be imparted to the conductive particles. Examples of such compounds include carboxylbenzotriazole and the like.
[0127] Examples of the method for treating the conductive particles with the compound include a method of preparing a 10 to 100 mmol / l solution of a compound such as thioglycolic acid or carboxybenzotriazole in an organic solvent such as methanol or ethanol, and dispersing the conductive particles in the solution.
[0128] Next, the conductive particles after the microparticle coating treatment can be used. When the pH is in the neutral region, the surface potential (zeta potential) of the conductive particles having a hydroxyl group, a carboxyl group, an alkoxy group, an alkoxycarbonyl group, etc. is negative. On the other hand, the surface potential of the microparticles having a hydroxyl group is also generally negative. Since it is difficult to coat the surroundings of the particles having a negative surface potential with particles having a negative surface potential, it is preferred to coat the conductive particles with microparticles via a polymer electrolyte.
[0129] The method of coating conductive particles with microparticles via a polymer electrolyte includes, for example, the following steps: (1) dispersing the treated conductive particles in a polymer electrolyte solution so that the polymer electrolyte is adsorbed on the surface of the conductive particles; and (2) dispersing the conductive particles adsorbed with the polymer electrolyte in a dispersion solution of the microparticles so that the microparticles are adsorbed on the surface of the polymer electrolyte.
[0130] When implementing the above method, reference may be made to the layer-by-layer assembly method, which is a method for forming an organic thin film published by G. Decher et al. in 1992 (Thin Solid Films, 210 / 211, p831 (1992)).
[0131] After the polymer electrolyte is adsorbed on the surface of the conductive particles or after the microparticles are adsorbed on the surface of the polymer electrolyte, the excess polymer electrolyte or microparticles can be washed away by washing with a solvent. Examples of the solvent used include water, alcohol, and acetone.
[0132] As a polymer electrolyte, a polymer that is ionized in an aqueous solution and contains a functional group with a charge in the main chain or the side chain can be used. This polymer electrolyte is preferably a polycation. As a polycation, a polycation that can be positively charged like polyamines can be used. Specifically, polyethyleneimine (PEI), polyallylamine hydrochloride (PAH), polydiallyldimethylammonium chloride (PDDA), polyvinylpyridine (PVP), polylysine, polyacrylamide and copolymers containing at least one of them can be cited. In polymer electrolytes, polyethyleneimine (PEI) has a high charge density and strong bonding strength.
[0133] From the perspective of avoiding electromigration and corrosion, the polymer electrolyte can be a polymer electrolyte that does not contain alkali metal (Li, Na, K, Rb, Cs) ions, alkaline earth metal (Ca, Sr, Ba, Ra) ions and halide ions (fluoride ions, chloride ions, bromide ions, iodine ions).
[0134] The polymer electrolyte may be one that is soluble in water or an organic solvent such as alcohol. The molecular weight of the polymer electrolyte may be 1000 to 200000. When the molecular weight is 1000 or more, the conductive particles have sufficient dispersibility and tend to be less likely to aggregate.
[0135] The polymer electrolyte solution is a solution obtained by dissolving a polymer electrolyte in a mixed solvent of water and a water-soluble organic solvent. Examples of the water-soluble organic solvent include methanol, ethanol, propanol, acetone, dimethylformamide, and acetonitrile. The concentration of the polymer electrolyte in the solution may be 0.001 to 10% by mass. The pH of the polymer electrolyte solution is not particularly limited.
[0136] By using the polymer electrolyte, the coverage and the CV value of the coverage can be increased. As a result, even if the electrode spacing is narrow, it is easy to ensure insulation and further reduce the connection resistance between the electrically connected electrodes.
[0137] The above-mentioned coverage and CV value of the coverage can also be adjusted by adjusting the type, molecular weight, concentration, etc. of the polymer electrolyte. Specifically, when a polymer electrolyte with a high charge density such as polyethyleneimine is used, there is a tendency for the coverage of the sub-particles to increase, and when a polymer electrolyte with a low charge density such as polydiallyldimethylammonium chloride is used, there is a tendency for the coverage of the sub-particles to decrease. In addition, when the molecular weight of the polymer electrolyte is large, there is a tendency for the coverage of the sub-particles to increase, and when the molecular weight of the polymer electrolyte is small, there is a tendency for the coverage of the sub-particles to decrease.
[0138] After coating the conductive particles with microparticles, the bonding between the daughter particles and the mother particles can also be strengthened by heating and drying. The heating temperature can be 60 to 120°C, and the heating time can be in the range of 60 to 180 minutes. When the heating temperature is above 60°C or the heating time is above 60 minutes, it is not easy to cause the peeling of the daughter particles during heating and drying. When the heating temperature is below 120°C or the heating time is below 180 minutes, it is not easy to cause deformation of the mother particles during heating and drying.
[0139] The conductive particles P may be surface-treated with a surface treatment agent such as a silane coupling agent or silicone.
[0140] <Adhesive film for circuit connection>
[0141] Figure 21 is a schematic cross-sectional view showing an embodiment of an adhesive film for circuit connection containing the above-mentioned conductive particles P (hereinafter referred to as "conductive particles P"). As shown in the same figure, the adhesive film for circuit connection 11 is composed of a release film 12, a conductive adhesive layer 13 composed of an adhesive layer in which the conductive particles P are dispersed, and an insulating adhesive layer 14 composed of an adhesive layer in which the conductive particles P are not dispersed, which are stacked in sequence. For the sake of convenience, the layer in which the conductive particles P are dispersed is called a conductive adhesive layer, and the layer in which the conductive particles P are not dispersed is called an insulating adhesive layer, but the adhesive components constituting these two layers themselves have insulating properties. In addition, the release film 12 and the insulating adhesive layer 14 are not necessarily constituted. For the sake of convenience, the adhesive film for circuit connection without a release film is sometimes also referred to as an adhesive film for circuit connection 11.
[0142] The release film 12 is made of, for example, polyethylene terephthalate (PET), polyethylene, polypropylene, etc. The release film 12 may contain any filler. Furthermore, the surface of the release film 12 may be subjected to a release treatment, a plasma treatment, or the like.
[0143] The conductive adhesive layer 13 and the insulating adhesive layer 14 both contain an adhesive component. The adhesive component refers to a component that contributes to adhesion among the components contained in the adhesive layer. The adhesive component has, for example, thermosetting properties.
[0144] The binder component preferably mainly includes components soluble in an organic solvent having an SP value of 8.5 to 10.0. That is, preferably, among the components included as the binder component, the component having the highest content ratio is soluble in an organic solvent having the above-mentioned SP value. Specifically, it is more preferred that one or both of the monomer and the film-forming material described later are soluble in an organic solvent having the above-mentioned SP value. Here, "soluble" in an organic solvent means that 50% by mass or more is dissolved in the organic solvent at 25°C.
[0145] The adhesive component includes, for example, a monomer (polymerizable compound), a curing agent, and a film-forming material. When the adhesive component has thermosetting properties, the monomer is cured by reacting with the curing agent by heat.
[0146] The monomer can be a low molecular weight compound or a high molecular weight compound as long as it is a polymerizable compound. For example, the monomer can be an oligomer. One monomer can be used alone or two or more monomers can be mixed. As a monomer, a low molecular weight compound and a high molecular weight compound can be used in combination, or a non-polymer and a polymer can be used in combination.
[0147] The monomer may be an epoxy resin monomer. As the epoxy resin monomer, bisphenol-type epoxy resins derived from epichlorohydrin and bisphenol A, bisphenol F, bisphenol AD, etc., epoxy novolac resins derived from epichlorohydrin and phenol novolac, cresol novolac, etc., glycidylamine, glycidyl ether, biphenyl, alicyclic, etc., various epoxy compounds having two or more glycidyl groups in one molecule, etc. can be used.
[0148] The monomer may be a radical polymerizable monomer. Examples of the radical polymerizable monomer include maleimide compounds, styrene derivatives, and the like, in addition to (meth)acrylic monomers such as (meth)acrylates.
[0149] The curing agent may be any component that contributes to curing by polymerization of the monomers. The curing agent may be a component incorporated into the molecular skeleton after curing, or may be a so-called polymerization initiator.
[0150] When epoxy resin monomers are used, as curing agents, imidazoles, hydrazides, boron trifluoride-amine complexes, sulfonium salts, amine imides, salts of polyamines, dicyandiamide, etc. can be used. From the viewpoint of extending the use time, the curing agent can be coated with a polyurethane or polyester polymer compound and microencapsulated.
[0151] When using epoxy monomers, the curing agent can be appropriately selected according to the target connection temperature, connection time, storage stability, etc. From the viewpoint of high reactivity, the gel time of the curing agent and the epoxy resin composition is preferably within 10 seconds at a specified temperature, and from the viewpoint of storage stability, it is preferred that the gel time with the epoxy resin composition does not change after being stored at 40° C. in a thermostatic bath for 10 days. From this viewpoint, the curing agent is preferably a sulfonium salt.
[0152] When a radical polymerizable monomer is used, as the curing agent, a curing agent that decomposes by heating to generate free radicals, such as a peroxide or an azo compound, can be used.
[0153] When a free radical polymerizable monomer (especially a (meth) acrylic acid monomer) is used, the curing agent is appropriately selected according to the target connection temperature, connection time, storage stability, etc. From the viewpoint of high reactivity and storage stability, an organic peroxide or azo compound having a half-life of 10 hours at a temperature of 40°C or more and a half-life of 1 minute at a temperature of 180°C or less is preferably used, and an organic peroxide or azo compound having a half-life of 10 hours at a temperature of 60°C or more and a half-life of 1 minute at a temperature of 170°C or less is more preferably used. These curing agents can be used alone or in combination. The curing agent can be mixed with a decomposition accelerator, an inhibitor, etc.
[0154] When the connection time is 10 seconds or less, the amount of the curing agent may be 0.1 to 40 parts by mass, or 1 to 35 parts by mass, based on 100 parts by mass of the total of the monomer and the film-forming material described below, from the viewpoint of improving the reaction rate.
[0155] The film-forming material is a polymer that facilitates the handling of the low-viscosity composition including the curing agent and monomers. By using the film-forming material, the film can be prevented from being easily cracked, damaged, or sticky, thereby obtaining an adhesive film 11 for circuit connection that is easy to handle.
[0156] As the film-forming material, thermoplastic resins can be preferably used. As thermoplastic resins, phenoxy resins, polyvinyl formal resins, polystyrene resins, polyvinyl butyral resins, polyester resins, polyamide resins, xylene resins, polyurethane resins, polyacrylic resins, polyester urethane resins, etc. can be cited. Siloxane bonds, fluorine substituents, etc. can be included in these polymers. These resins can be used alone or in combination with two or more. Among the above-mentioned resins, from the viewpoint of bonding strength, compatibility, heat resistance and mechanical strength, phenoxy resins are preferably used.
[0157] The larger the molecular weight of the thermoplastic resin, the easier it is to obtain film formation, and the melt viscosity that affects the fluidity of the adhesive film for circuit connection can be set in a wide range. The molecular weight of the thermoplastic resin can be 5000 to 150000, or 10000 to 80000, based on the weight average molecular weight. By setting the weight average molecular weight to 5000 or more, it is easy to obtain good film formation, and by setting it to 150000 or less, it is easy to obtain good compatibility with other components. In addition, the weight average molecular weight is a value measured according to the following conditions and by a gel permeation chromatograph (GPC) using a calibration curve based on standard polystyrene.
[0158] (Measurement conditions)
[0159] Apparatus: GPC-8020 manufactured by Tosoh Corporation
[0160] Detector: RI-8020 manufactured by Tosoh Corporation
[0161] Chromatographic column: Gelpack GLA160S+GLA150S manufactured by Resonac Holdings Corporation
[0162] Sample concentration: 120mg / 3mL
[0163] Solvent: Tetrahydrofuran
[0164] Injection volume: 60μL
[0165] Pressure: 2.94×106Pa(30kgf / cm 2 )
[0166] Flow rate: 1.00mL / min
[0167] The content of the film-forming material can be 5 to 80% by mass, or 15 to 70% by mass, based on the total amount of the monomer, the curing agent, and the film-forming material. When the above content is set to 5% by mass or more, good film formation is easily obtained. In addition, when the above content is set to 80% by mass or less, there is a tendency for the curable composition to show good fluidity.
[0168] Both the conductive adhesive layer 13 and the insulating adhesive layer 14 may further contain additives such as a filler, a softener, an accelerator, an anti-aging agent, a colorant, a flame retardant, a thixotropic agent, and a coupling agent.
[0169] When the adhesive layer contains a filler, it is possible to further expect that the connection reliability will be improved. The maximum diameter of the filler is preferably smaller than the particle size of the conductive particles. The content of the filler is preferably 5 to 60 parts by volume relative to 100 parts by volume of the adhesive layer. When the content of the filler is 60 parts by volume or less, there is a tendency to obtain an effect of sufficiently improving reliability. In addition, when the content of the filler is 5 parts by volume or more, the effect brought by the filler is easily obtained.
[0170] The conductive particles P exist in a dispersed state in the conductive adhesive layer 13. The ratio (monodispersity) of the conductive particles P in a state separated from other conductive particles P is preferably 90.0% or more, and can be 93.0% or more, 95.0% or more, 98.0% or more, or 99.0% or more. The upper limit of the monodispersity is 100%. The higher the monodispersity, the easier it is to obtain a connection structure with excellent insulation reliability. This dispersed state is formed by the external force application process described later. The monodispersity can be measured by the method described in the embodiments.
[0171] From the viewpoint of achieving both higher levels of insulation between adjacent electrodes and conductive particle capturing properties, the content of the conductive particles P may be 1 to 100 parts by volume, or 10 to 50 parts by volume, based on 100 parts by volume of components other than the conductive particles P in the conductive adhesive layer.
[0172] Regarding the relationship between the average particle size of the conductive particles P and the thickness of the conductive adhesive layer 13, the thickness of the conductive adhesive layer 13 is preferably 0.6 times or more and less than 1.0 times the average particle size of the conductive particles P. When the thickness of the conductive adhesive layer 13 is 0.6 times or more relative to the average particle size of the conductive particles P, better connectivity is easily obtained. When the thickness of the conductive adhesive layer 13 is less than 1.0 times the average particle size of the conductive particles P, better insulation is easily obtained. From the same point of view, the thickness of the conductive adhesive layer 13 can be 0.7 times or more and 0.9 times or less relative to the average particle size of the conductive particles P.
[0173] When the above relationship is satisfied, a part of the conductive particles P protrudes toward the insulating adhesive layer 14, and the boundary S between the insulating adhesive layer 14 and the conductive adhesive layer 13 is located at the separation portion of the adjacent conductive particles P and P. Furthermore, the conductive particles P are not exposed on the opposite side of the insulating adhesive layer 14 in the conductive adhesive layer 13 (i.e., the side on the release film 12 side), and the opposite side is a flat surface. The shortest distance between the conductive particles P and the surface of the conductive adhesive layer 13 in the thickness direction of the conductive adhesive layer 13 can be greater than 0 μm and less than 1 μm.
[0174] The boundary S between the insulating adhesive layer 14 and the conductive adhesive layer 13 can be confirmed by observing the cross section of the circuit connection adhesive film 11. The boundary S between the insulating adhesive layer 14 and the conductive adhesive layer 13 can also be determined by the difference in observation images in a processing observation device such as FIB, SEM, or TEM caused by the difference in composition between the insulating adhesive layer 14 and the conductive adhesive layer 13.
[0175] When the insulating adhesive layer 14 and the conductive adhesive layer 13 are difficult to dissolve in each other, the boundary S can be confirmed as an interface. When the insulating adhesive layer 14 and the conductive adhesive layer 13 have similar compositions and the interface disappears in the lamination process described later, a boundary layer where the insulating adhesive layer 14 and the conductive adhesive layer 13 are mixed may be observed.
[0176] The thickness of the conductive adhesive layer 13 is, for example, 1.5 to 6.0 μm. The thickness of the insulating adhesive layer 14 can be appropriately set. The total thickness of the conductive adhesive layer 13 and the insulating adhesive layer 14 is, for example, 5 to 30 μm.
[0177] The adhesive film 11 for circuit connection described above is an adhesive film for circuit connection. The adhesive film 11 for circuit connection may have anisotropic conductivity or may not have anisotropic conductivity. That is, the adhesive film 11 for circuit connection may be an anisotropic conductive adhesive film or a non-anisotropic conductive (for example, isotropic conductive) adhesive film. The adhesive film 11 for circuit connection may be used to heat-compress a first component having a first electrode and a second component having a second electrode in a state where the adhesive film 11 for circuit connection is interposed between the first component and the second component, so as to electrically connect the first electrode and the second electrode to each other.
[0178] <Method for producing adhesive film for circuit connection>
[0179] Figure 2 The circuit connection adhesive film 11 shown in the figure may be an external force dispersion type circuit connection adhesive film. That is, the circuit connection adhesive film 11 may be manufactured by a method including the following steps, namely, a step (external force application step) of applying an external force (e.g., magnetic force) to the conductive particles P in a film containing an adhesive component and the conductive particles P to disperse the conductive particles P. Figure 2 The method for producing the adhesive film for circuit connection shown in the following is described in detail.
[0180] Figure 3 Yes means Figure 2 A schematic diagram of the manufacturing process of the adhesive film for circuit connection shown in FIG. As shown in the same figure, first, a process (coating process) of applying the adhesive paste W, which is a forming material of the conductive adhesive layer 13, to the release film 12 is implemented. In the example of the same figure, the long strip release film 12 is conveyed at a predetermined speed by the feed roller 21 and the winding roller 22. On the conveying path of the release film 12, a coater 23 for coating the adhesive paste W, which is a forming material of the conductive adhesive layer 13, is arranged, and the adhesive paste W is coated on the release film 12 by the coater 23. The thickness of the film (coating film) composed of the adhesive paste W coated on the release film 12 by the coater 23 varies in time according to the proportion of the solvent contained in the resin composition, and is preferably less than 1.6 times the average particle size of the conductive particles P.
[0181] The adhesive paste W contains an adhesive component, conductive particles P dispersed in the adhesive component, and an organic solvent. The adhesive paste W can be prepared, for example, by stirring, mixing, kneading, etc. the adhesive component (monomer, curing agent, film-forming material, etc.) and the conductive particles P in an organic solvent to dissolve or disperse them. The organic solvent can be, for example, an organic compound having an SP value of 8.5 to 10.0. Examples of such an organic solvent include acetone, methyl ethyl ketone, ethyl acetate, toluene, and the like.
[0182] The viscosity of the adhesive paste W can be adjusted according to the application, coating method, etc. The viscosity of the adhesive paste W can be 10 mPa·s to 10000 mPa·s, and can be 50 mPa·s to 5000 mPa·s from the viewpoint of suppressing the separation of the preparation in the adhesive paste W and improving the compatibility. From the viewpoint of improving the appearance of the adhesive film 11 for circuit connection, the viscosity of the adhesive paste W can be 100 mPa·s to 3000 mPa·s.
[0183] The coating method of the adhesive paste W is not limited to the above, and a known method can be used. As the coating method, spin coating, roller coating, rod coating, dip coating, micro gravure coating, curtain coating, die coating, spray coating, blade coating, kneading coating, flow coating, screen printing, casting, etc. can be cited. Among them, rod coating, die coating, micro gravure coating and other methods are suitable for the preparation of the adhesive film 11 for circuit connection. From the perspective of the accuracy of the film thickness, the micro gravure coating method is particularly preferred.
[0184] Next, a magnetic force is applied as an external force to the conductive particles P in the film (adhesive paste W) containing the adhesive component and the conductive particles to disperse the conductive particles P (magnetic field application step). Figure 4 As shown, on the downstream side of the coating machine 23, a pair of magnets 24 and 25 are arranged in a vertically opposed manner so as to sandwich the release film 12, and the magnet 24 arranged on the upper side is the N pole and the magnet 25 arranged on the lower side is the S pole, so that a magnetic field is formed in a substantially vertical direction from the magnet 24 to the magnet 25. Therefore, when the release film 12 is conveyed between the magnets 24 and 25, the conductive particles P in the film (adhesive paste W) are magnetized, and the conductive particles P and P are separated from each other in the in-plane direction of the film (adhesive paste W) by the repulsive force (magnetic field application process).
[0185] Next, while the release film 12 passes between the magnets 24 and 25, the adhesive paste W is dried by hot air or the like (drying step). As a result, the viscosity of the adhesive paste W increases and the separation state of the conductive particles P in the magnetic field application step is maintained. Figure 5 As shown, the conductive adhesive layer 13 is formed on the release film 12. In addition, the thickness of the film (adhesive paste W) is reduced by the drying process. As described above, by setting the thickness of the film (adhesive paste W) to less than 1.6 times the average particle size of the conductive particles P, the thickness of the conductive adhesive layer 13 can be set to be greater than 0.6 times and less than 1.0 times the average particle size of the conductive particles P.
[0186] The drying temperature of the adhesive paste W is, for example, 20 to 80° C. The conveying speed of the release film 12 is, for example, 30 to 160 mm / s. The thickness of the film (adhesive paste W) is, for example, 5 to 10 μm.
[0187] Next, after forming the conductive adhesive layer 13, Figure 6 As shown in FIG. 1 , the insulating adhesive layer 14 prepared separately is laminated on the conductive adhesive layer 13 (lamination step). Figure 2 The circuit connection adhesive film 11 shown in FIG. 1 can be used to laminate the insulating adhesive layer 14 using, for example, a hot roll laminator. The lamination method is not limited to lamination, and may be a method in which an adhesive paste as a material of the insulating adhesive layer 14 is applied to the conductive adhesive layer 13 and dried.
[0188] Figure 7 This is a microscope photograph showing the dispersion of conductive particles in a conventional production method. Figure 8 is a microscope photograph showing the dispersion of conductive particles in this manufacturing method. Figure 7 As shown in FIG. 1 , in the conventional manufacturing method, although there are some conductive particles in a state of being separated from each other, most of the conductive particles are in contact with other conductive particles and are in a state of being aggregated. Figure 8 As shown, in the present manufacturing method, almost all the conductive particles maintain a state of being separated from other conductive particles.
[0189] In the method for manufacturing the adhesive film for circuit connection described above, magnetic force is used as the external force, but it is not limited to magnetic force. In the method of dispersing conductive particles by centrifugal force, etc., it is also possible to obtain an adhesive film for circuit connection in which the conductive particles are well dispersed by using the conductive particles P of the above embodiment.
[0190] <Connection structure>
[0191] Fig. 9 1 is a schematic cross-sectional view showing an embodiment of a connection structure. As shown in the same figure, the connection structure 1 includes: a first component 2 having a first electrode 6; a second component 3 having a second electrode 8; and a connection portion 4, which is arranged between the first component 2 and the second component 3 and electrically connects the first electrode 6 and the second electrode 8 to each other. The first component 2 and the second component 3 are arranged so that the first electrode 6 and the second electrode 8 are opposite to each other.
[0192] The first component 2 is, for example, a circuit component, and may be a tape carrier package (TCP), a printed circuit board, a semiconductor silicon chip, or the like. A plurality of first electrodes 6 included in the first component 2 are arranged on the mounting surface 5a side of the main body 5. The first electrode 6 is, for example, a bump electrode. The first electrode 6 is, for example, rectangular in a plan view. The thickness of the first electrode 6 is, for example, not less than 3 μm and less than 18 μm. The material used to form the first electrode 6 is, for example, Au, which is easier to deform than the conductive particles P. On the mounting surface 5a, an insulating layer may be formed in a portion where the first electrode 6 is not formed.
[0193] The second component 3 is, for example, a circuit component, and may be a circuit substrate for a liquid crystal display. The second component 3 may be, for example, a glass substrate or a plastic substrate with a circuit formed of ITO, IZO, metal, etc., or a flexible printed circuit board (FPC) or a ceramic wiring board. Fig. 9 As shown, the second component 3 has a plurality of second electrodes 8 corresponding to the first electrode 6 on the mounting surface 7a side of the main body 7. The second electrode 8 is, for example, a circuit electrode. The second electrode 8 is, for example, rectangular in a plan view. The thickness of the second electrode 8 is, for example, about 100 nm. The surface of the second electrode 8 is composed of, for example, one or more materials selected from the group consisting of gold, silver, copper, tin, ruthenium, rhodium, palladium, osmium, iridium, platinum, indium tin oxide (ITO) and indium zinc oxide (IZO). On the mounting surface 7a, an insulating layer may also be formed in a portion where the second electrode 8 is not formed.
[0194] The connection portion 4 is a portion formed by curing the adhesive film 11 for circuit connection, and includes a cured product of the adhesive film 11 for circuit connection. The connection portion 4 may be composed only of a cured product of the adhesive film 11 for circuit connection. The connection portion 4 includes a first region 9 formed by curing the conductive adhesive layer 13 and a second region 10 formed by curing the insulating adhesive layer 14. The first region 9 and the second region 10 are spread in a layered manner along the mounting surface 5a of the first component 2 and the mounting surface 7a of the second component 3. In the present embodiment, the first region 9 is located on the second component 3 side, and the second region 10 is located on the first component 2 side. The boundary between the first region 9 and the second region 10 may not necessarily be clear.
[0195] The conductive particles P are biased toward the second component 3, and a portion of the conductive particles P is interposed between the first electrode 6 and the second electrode 8. The conductive particles P between the first electrode 6 and the second electrode 8 are partially separated by the pressure contact, and the mother particle 31 is deformed into a slightly flat state and contacts the first electrode 6 and the second electrode 8. Thus, the electrical connection between the first electrode 6 and the second electrode 8 is achieved. In addition, between the adjacent first electrodes 6, 6 and between the adjacent second electrodes 8, 8, the conductive particles P are separated from each other, and the electrical insulation between the adjacent first electrodes 6, 6 and between the adjacent second electrodes 8, 8 is achieved.
[0196] <Method for producing a connection structure>
[0197] The method for manufacturing the connection structure 1 includes the following steps: thermocompression bonding the first component 2 and the second component 3 with the circuit connection adhesive film 11 interposed therebetween to electrically connect the first electrode 6 and the second electrode 8 to each other. Fig.10 and Fig.11 A method for producing the connection structure 1 will be described.
[0198] Fig.10 and Fig.11 Yes means Fig. 9 Schematic cross-sectional view of the manufacturing process of the connection structure 1 shown in FIG. When manufacturing the connection structure 1, first, the release film 12 is peeled off from the circuit connection adhesive film 11, and the circuit connection adhesive film 11 is laminated on the second component 3 in such a manner that the conductive adhesive layer 13 side faces the mounting surface 7a. Then, as shown in FIG. Fig.11 As shown, the first member 2 is arranged on the second member 3 laminated with the circuit-connecting adhesive film 11 so that the first electrode 6 faces the second electrode 8. The first member 2 and the second member 3 are pressed in the thickness direction while the circuit-connecting adhesive film 11 is heated.
[0199] As a result, the adhesive component of the circuit connection adhesive film 11 flows, the distance between the first electrode 6 and the second electrode 8 is shortened, and the conductive adhesive layer 13 and the insulating adhesive layer 14 are cured in a state of biting the conductive particles P. The first electrode 6 and the second electrode 8 are electrically connected by curing the conductive adhesive layer 13 and the insulating adhesive layer 14, and the connecting portion 4 is formed in a state where the adjacent first electrodes 6, 6 are electrically insulated from each other and the adjacent second electrodes 8, 8 are electrically insulated from each other, thereby obtaining Fig. 9 In the obtained connection structure 1, the connection portion 4 can sufficiently prevent the distance between the first electrode 6 and the second electrode 8 from changing with time, and can also ensure the long-term reliability of the electrical characteristics.
[0200] The heating temperature of the circuit connection adhesive film 11 is preferably a temperature at which polymerization active species are generated in the curing agent and the polymerization of the monomer (polymerizable compound) begins. The heating temperature is, for example, 80° C. to 200° C., preferably 100° C. to 180° C. The heating time is, for example, 0.1 second to 30 seconds, preferably 1 second to 20 seconds.
[0201] Example
[0202] Hereinafter, the contents of the present invention will be described in more detail using Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0203] <Production Examples 1 to 8>
[0204] (Production of Insulating Particles 1 to 8)
[0205] The monomers shown in Tables 1 to 3 were polymerized using an emulsion polymerization method. Specifically, first, 400 g of pure water was added to a synthesis flask, and then the materials shown in Tables 1 to 3 were added to the flask at the molar amounts shown in Tables 1 to 3. These were heated at 70° C. for 8 hours while being stirred. The stirring speed was set to 300 rpm. Thus, insulating particles 1 to 8 were prepared respectively.
[0206] (SEM average particle size and irregularity measurement)
[0207] The insulating fine particles 1 to 8 were observed at a magnification of 30,000 times using a field emission scanning electron microscope (SU-8020, manufactured by Hitachi High-Tech Corporation), and the obtained SEM images were analyzed using XG VisionEditor (image analysis software manufactured by KEYENCE CORPORATION) to determine the average particle size (SEM average particle size d1) and irregularity of the insulating fine particles 1 to 8 based on SEM observation.
[0208] Specifically, first, the insulating particles were dried and an SEM image of the dried insulating particles was obtained. Then, latex particles (CLINTEX series, particle size: 0.3 μm) manufactured by JSR Corporation were used as a standard sample, and a particle similar to the standard sample was extracted from the SEM image. Then, 10 or more and up to 36 points of intersection between a straight line passing through the center point of the extracted particle and a point on the edge of the particle were detected, and 5 or more and up to 18 diameters d were obtained. X (the distance between the two intersection points on the straight line) and a maximum of 36 radii r X (The distance between the center point and the intersection point) Next, the obtained diameter d is calculated. X The average value d Y , so as to find the Y The radius r of the virtual circle (perfect circle) with diameter Y (d Y / 2) and the radius r of the above particle X The average value of the absolute difference is set as the average deformation D of the particle, and the average deformation D and the radius r of the virtual circle are used to calculate the average deformation D of the particle. Y , the particle irregularity was calculated by the following formula.
[0209] Irregularity = average deformation D / radius r of virtual circle Y ×100
[0210] The above operation is performed on 100 randomly selected particles, and the calculated d YThe average values of the irregularity are defined as the SEM average particle size d1 and the irregularity of the insulating fine particles 1 to 8. The results are shown in Tables 1 to 3.
[0211] (Measurement of swelling ratio)
[0212] After measuring the average particle size d2 of the insulating particles 1 to 8 in water, the insulating particles 1 to 8 were immersed in ethyl acetate and treated in an ultrasonic bath with an ultrasonic frequency of 40 kHz and an output power of 120 W for 5 minutes, and then the average particle size d3 of the insulating particles 1 to 8 in ethyl acetate was measured. Based on the obtained average particle sizes d2 and d3, the swelling ratio of the insulating particles 1 to 8 (the ratio d3 / d2 of the average particle size d3 to the average particle size d2) was calculated. The specific method for measuring the average particle size is shown below.
[0213] The particles of the object to be measured (any one of insulating particles 1 to 8) in the range of 0.1 to 1.0 mass % were added to a solvent (water or ethyl acetate) so that the pH of the sample solution became 7.3 to 7.8, and the particles were dispersed by vibrating a 120 W ultrasonic tank for 5.0 minutes. Next, the particle size distribution was measured at 25 to 27° C. using a laser diffraction particle size distribution analyzer Microtrac MT3300EXII (manufactured by Microtrac BEL Corp., product name). Regarding the setting of the refractive index, the refractive index of insulating particles 1 to 6 (polystyrene particles) was set to 1.59, and the refractive index of insulating particles 7 to 8 (polymethyl methacrylate particles) was set to 1.49. The particle size at the cumulative value of 50% (volume basis) in the obtained particle size distribution was set as the average particle size.
[0214] (Measurement of glass transition temperature)
[0215] The glass transition temperatures (Tg) of the insulating fine particles 1 to 8 were measured using a differential scanning calorimeter (DSC) Q1000 (manufactured by TA Instruments Japan). The results are shown in Tables 1 to 3.
[0216] [Table 1]
[0217]
[0218] [Table 2]
[0219]
[0220] [Table 3]
[0221]
[0222] The details of the materials shown in Tables 1 to 3 are as follows.
[0223] (Non-crosslinking monomer)
[0224] ·Styrene: Made by FUJIFILM Wako Pure Chemical Corporation
[0225] ·Butyl acrylate: manufactured by FUJIFILM Wako Pure Chemical Corporation ·Methyl methacrylate: manufactured by MITSUBISHI GAS CHEMICAL COMPANY, INC.
[0226] · Glycidyl methacrylate: manufactured by FUJIFILM Wako Pure Chemical Corporation
[0227] ·3-Methacryloyloxypropylmethyldimethoxysilane: manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-502
[0228] ·3-Methacryloxypropyltrimethoxysilane: manufactured by Shin-Etsu Chemical Co., Ltd., product name: KBM-503
[0229] Sodium methacrylate: manufactured by Sigma-Aldrich Co. LLC
[0230] ·Sodium styrene sulfonate: manufactured by FUJIFILM Wako Pure Chemical Corporation
[0231] ·Mono(2-hydroxyethyl methacrylate) phosphate: manufactured by JOHOKU CHEMICAL CO., LTD. Product name: JAMP-514
[0232] (Crosslinking monomer)
[0233] ·Divinylbenzene: manufactured by NIPPON STEEL Chemical & Material Co., Ltd., product name: Divinylbenzene (DVB-960)
[0234] ·Diethylene glycol dimethacrylate: manufactured by Tokyo Chemical Industry Co., Ltd.
[0235] (Free Radical Polymerization Initiator)
[0236] Potassium persulfate: manufactured by FUJIFILM Wako Pure Chemical Corporation
[0237] ·2,2'-Azobis[N-(2-carboxyethyl)-2-methylpropionamidine] tetrahydrate: manufactured by FUJIFILM Wako Pure Chemical Corporation, product name: VA-057
[0238] (Emulsifier)
[0239] · Triethanolamine lauryl sulfate 30% solution: manufactured by Kao Corporation, product name: Emar TD
[0240] <Examples 1 to 4 and Comparative Examples 1 to 4>
[0241] (Production of Conductive Particles 1 to 8)
[0242] [Preparation of Mother Particle 1]
[0243] Plastic particles with an average particle size of 3.0 μm composed of a polymer of a monomer having two acryloyl groups (a bifunctional acrylic monomer) were prepared. The hardness of the plastic particles was evaluated based on the elastic modulus when the particles were compressed at room temperature (25°C) and deformed by 20% (hereinafter referred to as "20% K value"). As a result, the 20% K value was 2.0 GPa.
[0244] On the surface of the above-mentioned plastic particles, nickel was plated using an electroless plating method to form a nickel metal layer with a thickness of 100 nm. Thus, a conductive mother particle 1 (particle size: about 3.1 μm) consisting of a plastic particle and a nickel metal layer covering the surface of the plastic particle was obtained. In addition, the thickness of the nickel metal layer is the following value: the surface of the obtained injection sample is prepared by dispersing the particles in an injection resin and performing injection molding, and the surface of the obtained injection sample is ground to expose the cross section of the particle, and the average value of the thickness of 5 places measured by observing the cross section of the particle using SEM (SU-8020 manufactured by Hitachi High-Tech Science Corporation).
[0245] [Preparation of Silicone Oligomer 1]
[0246] A solution was obtained by mixing 118 g of 3-glycidyl ether propyl trimethoxysilane and 5.9 g of methanol into a glass flask equipped with a stirring device, a capacitor and a thermometer. After further adding 5 g of activated clay and 4.8 g of distilled water to the glass flask, stirring was performed at 75°C for a certain period of time to obtain a silicone oligomer 1 with a weight average molecular weight of 1300. The obtained silicone oligomer 1 is a silicone oligomer having a methoxy group or a silanol group as a terminal functional group that reacts with a hydroxyl group. Methanol was added to the obtained solution of silicone oligomer 1 to prepare a treatment liquid with a solid content of 20% by mass. In addition, the weight average molecular weight of silicone oligomer 1 was measured by gel permeation chromatography (GPC) and calculated by conversion using a calibration curve of standard polystyrene. The conditions of GPC are shown below.
[0247] -GPC conditions
[0248] Apparatus: GPC-8020 manufactured by Tosoh Corporation
[0249] Detector: RI-8020 manufactured by Tosoh Corporation
[0250] Chromatographic column: Gelpack GL-A-160-S+GL-A150 manufactured by Showa Denko Materials co., Ltd.
[0251] Sample concentration: 120mg / 3ml
[0252] Solvent: Tetrahydrofuran
[0253] Injection volume: 60μl
[0254] Pressure: 30kgf / cm 2
[0255] Flow rate: 1.00ml / min
[0256] [Production of Conductive Particles 1 to 8]
[0257] 8 mmol of thioglycolic acid was dissolved in 200 ml of methanol to prepare a reaction solution. Next, 10 g of the mother particle 1 was added to the above reaction solution, and stirred at room temperature for 2 hours using a Sany motor and a stirring blade with a diameter of 45 mm, thereby performing surface treatment (first treatment) of the mother particle 1. Next, the treated particles were taken out from the stirred liquid, washed with methanol, and filtered using a membrane filter with a pore size of 3 μm (manufactured by Nihon Millipore KK). Thus, 10 g of particles (particle 1A) with carboxyl groups on the surface were obtained.
[0258] Next, a 30 mass % polyethyleneimine aqueous solution (manufactured by FUJIFILM Wako Pure Chemical Corporation) having a weight average molecular weight of 70,000 was diluted with pure water to obtain a 0.1 mass % polyethyleneimine aqueous solution and a 0.01 mass % polyethyleneimine aqueous solution. When preparing conductive particles 1 to 6 and 8, a 0.1 mass % polyethyleneimine aqueous solution was used, and when preparing conductive particle 7, a 0.01 mass % polyethyleneimine aqueous solution was used.
[0259] Next, 10g of the above-mentioned particles 1A were added to a 0.1% by mass polyethyleneimine aqueous solution or a 0.01% by mass polyethyleneimine aqueous solution, and stirred at room temperature for 15 minutes, thereby performing a surface treatment (the second treatment) of the particles 1A. Next, the treated particles were taken out from the stirred liquid and filtered using a membrane filter (manufactured by Nihon Millipore KK) with a pore size of 3 μm. The filtered particles were added to 200g of pure water, stirred at room temperature for 5 minutes, and then the particles were taken out from the methanol and filtered using a membrane filter (manufactured by Nihon Millipore KK) with a pore size of 3 μm. On the above-mentioned membrane filter, the particles were washed twice with 200g of pure water. Thus, the polyethyleneimine that was not adsorbed on the particles 1A was removed, and particles (particles 1B) coated with a polymer containing an amino group were obtained.
[0260] Next, insulating fine particles 1 to 8 were treated with silicone oligomer 1 to prepare ethyl acetate dispersions of fine particles (fine particles 1A to 8A) having oligomers containing glycidyl groups on their surfaces.
[0261] Next, after immersing the particle 1B in ethyl acetate, an ethyl acetate dispersion of the particles 1A to 8A is added to the liquid, thereby obtaining a conductive particle having any of the insulating particles 1 to 8 as a daughter particle. At this time, the amount of the ethyl acetate dispersion added is set to a sufficient amount required for the surface of the mother particle to be completely covered with the daughter particles (including the unadsorbed daughter particles).
[0262] Next, the conductive particles were treated with 315 g of a solution (solid content concentration: 1.9 mass %) of poly(dimethyldimethoxysilane) (weight average molecular weight Mw: 800-1200) dissolved in IPA (isopropyl alcohol) and washed, thereby hydrophobizing the surface of the conductive particles. Thereafter, the conductive particles were dried by heating at 100° C. for 90 minutes in a vacuum state, thereby producing conductive particles 1 to 8.
[0263] (Evaluation 1)
[0264] [Measurement of coverage and its CV value]
[0265] The coverage of conductive particles 1 to 8 and their CV values were measured by the following method. First, a field emission scanning electron microscope (SU-8020, manufactured by Hitachi High-Tech Corporation) was used to observe the conductive particles at a magnification of 8000 times to obtain a SEM image. Next, the SEM image was binarized using XG VisionEditor (image analysis software manufactured by KEYENCE CORPORATION). Next, one conductive particle was extracted from the binarized SEM image, and a circle with a radius of the outer circle of the conductive particle as its diameter (a circle concentric with the outer circle) was used as the measuring circle. The area S1 of the measuring circle and the total area S2 of the portion of the insulating fine particles present in the measuring circle were calculated, and the coverage of the extracted particles (the coverage of the daughter particles on the mother particles) was calculated by the following formula.
[0266] Coverage (%) = S2 / S1×100
[0267] This operation was performed on 100 randomly selected conductive particles, and the calculated coverage of the 100 conductive particles was averaged to obtain the coverage of conductive particle 1. The CV value of the coverage was obtained by dividing the standard deviation of the coverage calculated by the above formula by the average value. The results are shown in Table 4.
[0268] [Measurement of particle size]
[0269] The average particle size of the child particles in conductive particles 1 to 8 and the ratio of the average particle size of the child particles to the particle size of the mother particles were determined by the following method. First, a carbon tape was attached to the SEM sample stage, and conductive particles (conductive particles 1 to 8) were scattered thereon. The scattered conductive particles were observed by SEM, the conductive particles to be measured were determined, and the particle size of the mother particles in the conductive particles was measured at a magnification of 25,000 times. Next, in order to measure the particle size of the child particles, the SEM magnification was changed to 30,000 times, and the particle size of the child particles in the conductive particles whose particle size of the mother particles was measured was measured. In one conductive particle, the particle sizes of 5 child particles were measured, and their average was taken as the average particle size of the child particles in the conductive particle. And, based on the obtained measurement values, the ratio of the average particle size of the child particles to the particle size of the mother particles was determined. The above measurement was repeated for 25 conductive particles, and the average particle size of the child particles and the average particle size ratio of the child particles to the particle size of the mother particles were calculated (25 average values), and these were used as the average particle size of the child particles and the average particle size ratio of the child particles to the particle size of the mother particles in the conductive particles 1 to 8. The results are shown in Table 4.
[0270] [Contact angle measurement]
[0271] The contact angle of conductive particles 1 to 8 with water was measured by the following method. First, a double-sided tape (product name: Hibon 11-583 (manufactured by Resonac Holdings Corporation), width 10.0 mm, length 76.0 mm, thickness 0.14 mm) was attached to the surface of a glass plate. Next, 1.0 g of conductive particles were placed on the double-sided tape, and the conductive particles were spread on the double-sided tape in such a way that the entire surface of the double-sided tape was covered with the conductive particles (in such a way that no gaps were created between the conductive particles as much as possible). Next, by blowing air (product name: Air Duster AHSze300, manufactured by AIR WATER SOL INC.), the spraying time was set to 30 seconds to remove the excess conductive particles accumulated on the double-sided tape. Thus, a laminate consisting of glass, double-sided tape and a film formed by conductive particles was obtained. The laminate was used as a test piece for contact angle measurement.
[0272] Next, using the above-mentioned test piece, the contact angle with water was measured according to the static method described in Item 6 of JIS R 3257 (1999) "Test method for wettability of substrate glass surface". Specifically, using the contact angle meter "DM-701" manufactured by Kyowa Interface Science Co., Ltd., 6 μL of pure water was dripped on the film formed by conductive particles on the sample piece. The contact angle after 2000 ms after the dripping was measured. The above operation was performed a total of 10 times (10 places) at intervals of 7 to 10 mm, and the average value of the obtained values was calculated. This average value is used as the contact angle of the conductive particles. The results are shown in Table 4. In addition, the above-mentioned contact angle measurement was carried out at room temperature (25°C).
[0273] [Table 4]
[0274]
[0275] (Manufacturing of adhesive films for circuit connection)
[0276] 45 g of 4,4'-(9-fluorenylene)-diphenol (manufactured by Sigma-Aldrich Japan) and 50 g of 3,3',5,5'-tetramethylbiphenyl diglycidyl ether (manufactured by Mitsubishi Chemical Co., Ltd.: YX-4000H) were dissolved in 1000 mL of N-methylpyrrolidone in a 3000 mL three-necked flask equipped with a Dimroth condenser, a calcium chloride tube, and a Teflon stirring rod ("Teflon" is a registered trademark) connected to a stirring motor as a reaction solution. 21 g of potassium carbonate was added thereto, and the mixture was stirred while being heated to 110° C. with a mantle heater. After stirring for 3 hours, the reaction solution was dripped into a flask containing 1000 mL of methanol, and the precipitate generated was filtered by suction filtration. The filtered precipitate was further washed three times with 300 mL of methanol to obtain 75 g of phenoxy resin a.
[0277] Thereafter, the molecular weight of phenoxy resin a was measured using a high performance liquid chromatograph GP8020 manufactured by Tosoh Corporation (chromatographic column: Gelpak GLA150S and GLA160S manufactured by Showa Denko Materials Co., Ltd., solvent: tetrahydrofuran, flow rate: 1.0 mL / min). As a result, in terms of polystyrene, Mn (number average molecular weight) = 15769, Mw (weight average molecular weight) = 38045, and Mw / Mn = 2.413.
[0278] Next, 50 parts by mass of bisphenol A epoxy resin (Mitsubishi Chemical Co., Ltd.: jER828) as an epoxy compound, 5 parts by mass of 4-hydroxyphenylmethylbenzylsulfonium hexafluoroantimonate as a curing agent, 50 parts by mass of the above-mentioned phenoxy resin a as a film-forming material, and 80 parts by mass of conductive particles were blended to obtain conductive adhesive compositions (adhesive pastes) 1 to 8. At this time, the above-mentioned conductive particles 1 to 8 were used as conductive particles, respectively. In addition, ethyl acetate was used as a solvent.
[0279] Next, the above-mentioned conductive adhesive compositions 1 to 8 were used to obtain conductive adhesive layers 1 to 8 with a thickness of 2.7 μm on a PET resin film. Specifically, first, the conductive adhesive composition was applied to a PET resin film with a thickness of 50 μm using a coater to form a coating film, and then the coating film was dried and a magnetic field was applied. The thickness of the conductive adhesive layers 1 to 8 was adjusted by the amount of the conductive adhesive composition applied.
[0280] Next, 45 parts by mass of a bisphenol F epoxy resin (Mitsubishi Chemical Co., Ltd., jER807) as an epoxy compound, 5 parts by mass of 4-hydroxyphenylmethylbenzylsulfonium hexafluoroantimonate as a curing agent, and 55 parts by mass of a phenoxy resin b having a Mw (weight average molecular weight) of 50,000 and a Tg (glass transition temperature) of 70° C. as a film-forming material were blended to obtain an insulating adhesive composition.
[0281] Next, the insulating adhesive composition was applied to a PET resin film having a thickness of 50 μm using a coater to form a coating film, and then the coating film was dried with hot air at 70° C. for 5 minutes to obtain an insulating adhesive layer having a thickness of 16 μm.
[0282] Next, each of the conductive adhesive layers 1 to 8 and the insulating adhesive layer was heated to 40° C. and laminated with a hot roll laminator to obtain adhesive films for circuit connection of Examples 1 to 4 and Comparative Examples 1 to 4.
[0283] (Rating 2)
[0284] [Monodispersity of conductive particles]
[0285] The circuit connection adhesive films of Examples 1 to 4 and Comparative Examples 1 to 4 were observed from the conductive adhesive layer side at a magnification of 200 times using a metal microscope, and the number of conductive particles in the conductive adhesive layer was measured to determine the monodispersity of the conductive particles. The results are shown in Table 5. The monodispersity is the ratio of conductive particles that exist in a state separated from other conductive particles (monodispersed state), and is determined using the following formula.
[0286] Monodispersity (%) = (2500 μm 2 Number of monodisperse conductive particles in 2500 μm 2 The number of conductive particles in the
[0287] [Evaluation of Conductive Particle Capture and Insulation Properties]
[0288] (1) Fabrication of the connection structure
[0289] First, as the first component, an IC chip is prepared having a structure with two rows of bump electrodes arranged in a straight line (outer shape: 0.9 mm×20.3 mm, thickness: 0.3 mm, size of bump electrode: 75 μm×12 μm (for particle capture number evaluation) or 100 μm×12 μm (for insulation evaluation), distance between bump electrodes: 24 μm, thickness of bump electrode: 8 μm, bump electrode configuration: the bump electrodes in the second row are configured at a position deviated by 12 μm from the center of the bump electrodes in the first row along the length direction of the IC chip, and the interval between the bump electrodes in the first row and the bump electrodes in the second row is 25 μm). As a second member, a wiring board was prepared in which an ITO wiring pattern (pattern width: 19 μm, inter-electrode interval: 5 μm) was formed on the surface of a glass substrate (manufactured by Corning Incorporated Co., Ltd.: #1737, outer shape: 38 mm×28 mm, thickness: 0.3 mm).
[0290] Using the adhesive films for circuit connection of Examples 1 to 4 and Comparative Examples 1 to 4, the first component (IC chip) and the second component (wiring substrate) were connected according to the following steps to obtain a plurality of connection structures of Examples 1 to 4 and Comparative Examples 1 to 4. A workbench (150 mm × 150 mm) composed of a ceramic heater and a thermocompression bonding device composed of a tool (3 mm × 20 mm) were used for connection.
[0291] First, the PET resin film on the conductive adhesive layer of the circuit connection adhesive film (outer shape: 2.5 mm×25 mm) was peeled off, and the surface on the conductive adhesive layer side was passed through a 80°C·0.98 MPa (10 kgf / cm 2 ) for 2 seconds under heating and pressurization conditions to adhere to the surface of the second component (wiring substrate) on which the wiring pattern is formed.
[0292] Next, the PET resin film on the insulating adhesive layer of the circuit connection adhesive film is peeled off, and after the position of the bump electrode of the first component (IC chip) is aligned with the circuit electrode of the second component (wiring substrate), heating and pressurization are performed for 5 seconds under the conditions of the measured maximum reached temperature of the circuit connection adhesive film of 170°C and the area conversion pressure at the bump electrode of 70 MPa to attach the insulating adhesive layer to the first component (IC chip), thereby obtaining a connection structure.
[0293] (2) Evaluation of conductive particle capture performance
[0294] The number of conductive particles captured between the bump electrodes and the circuit electrodes in the connection structures of Examples 1 to 4 and Comparative Examples 1 to 4 (particle capture number) was measured using an optical microscope, and the conductive particle capture property was evaluated based on the particle capture number per bump electrode (particle capture number / bump electrode number) and its CV value. The results are shown in Table 5.
[0295] (3) Evaluation of insulation properties
[0296] The insulation performance was evaluated based on the proportion of connection structures judged as having poor insulation resistance based on the insulation resistance value (insulation resistance defect rate). The connection resistance value was measured as follows: the terminal of the insulation resistance measuring device was connected to the terminal provided at the end of the connection structure, and a voltage of 50V was applied to the connection structure to measure the insulation resistance. The insulation resistance value displayed by the insulation resistance measuring instrument was judged to be poor insulation resistance when it was less than 1.0E+09Ω. Examples 1 to 4 and Comparative Examples 1 to 4 were all evaluated with N (the number of connection structures evaluated) = 10 for the above-mentioned judgment and evaluation, and the connection structures with poor insulation resistance were counted to calculate the insulation resistance defect rate. The results are shown in Table 5.
[0297] [Table 5]
[0298]
[0299] Explanation of symbols
[0300] 1-connecting structure, 2-first component, 3-second component, 4-connecting portion, 6-first electrode (bump electrode), 8-second electrode (circuit electrode), 11-adhesive film for circuit connection, 13-conductive adhesive layer, 14-insulating adhesive layer, 31-mother particle, 32-daughter particle, P-conductive particle.
Claims
1. A conductive particle for producing an adhesive film for circuit connection having a monodispersity of 90.0% or more, The conductive particles include conductive mother particles and daughter particles covering the surface of the mother particles. When the particle radius and particle diameter of the child particles obtained by SEM observation at a magnification of 30,000 times are respectively defined as r X and X , the particle diameter d X The average value of the sub-particles, that is, the average particle size of the sub-particles is set as d Y When the irregularity of the sub-particles obtained by the following formula (1) is less than 2.0, Irregularity = D / r Y ×100(1) In formula (1), r Y Indicates that the diameter is equal to d Y The radius of the virtual sphere, D represents the particle radius r of the sub-particle X With the radius r of the virtual sphere Y The average of the absolute differences.
2. The conductive particle according to claim 1, wherein The coverage rate of the surface of the mother particle by the child particles is 40.0% or more.
3. The conductive particle according to claim 1 or 2, wherein: The CV value of the coverage of the surface of the mother particle by the child particles is 10.0% or less.
4. The conductive particle according to any one of claims 1 to 3, wherein The average particle size of the child particles determined by SEM observation at a magnification of 30,000 times was 200 to 400 nm.
5. The conductive particle according to any one of claims 1 to 4, wherein The ratio of the average particle size of the child particles obtained by SEM observation at a magnification of 30,000 times to the particle size of the mother particles obtained by SEM observation at a magnification of 25,000 times is 8.0 to 20.
0.
6. The conductive particle according to any one of claims 1 to 5, wherein When a film composed of the conductive particles is formed, the contact angle between the surface of the film and water is 130° or more.
7. The conductive particle according to any one of claims 1 to 6, wherein The daughter particles contain a copolymer including an aromatic cross-linking monomer and a non-cross-linking monomer as monomer units.
8. The conductive particle according to claim 7, wherein The aromatic cross-linking monomer is divinylbenzene.
9. The conductive particle according to claim 7 or 8, wherein The non-crosslinking monomer is styrene.
10. The conductive particle according to any one of claims 7 to 9, wherein The content of the polar group-containing monomer contained as a monomer unit in the copolymer is 2.0 mol% or less based on the total amount of the monomer units contained in the copolymer.
11. The conductive particle according to any one of claims 7 to 10, wherein The copolymer is an emulsifying polymer.
12. The conductive particles according to any one of claims 1 to 11, used in a method for manufacturing an adhesive film for circuit connection, the method for manufacturing an adhesive film for circuit connection comprising a step of dispersing the conductive particles by applying an external force to the conductive particles in a film containing an adhesive component and the conductive particles.
13. An adhesive film for circuit connection, comprising a conductive adhesive layer, wherein the conductive adhesive layer comprises an adhesive component and the conductive particles according to any one of claims 1 to 12, The monodispersity rate of the conductive particles in the conductive adhesive layer is 90.0% or more. 14 . A method for producing an adhesive film for circuit connection, comprising the step of dispersing the conductive particles by applying external force to the conductive particles in a film comprising an adhesive component and the conductive particles according to claim 1 .
15. The method for producing an adhesive film for circuit connection according to claim 14, wherein: In the above process, a magnetic field is applied to exert a magnetic force on the conductive particles, so that the conductive particles are dispersed.
16. A connection structure comprising: A first component having a first electrode; a second member having a second electrode; and a connecting portion disposed between the first member and the second member and electrically connecting the first electrode and the second electrode to each other, The connecting portion includes a cured product of the adhesive film for circuit connection according to claim 13 .
17. A method for manufacturing a connection structure, comprising the following steps: A first member having a first electrode and a second member having a second electrode are thermocompression bonded with the adhesive film for circuit connection according to claim 13 interposed therebetween, so that the first electrode and the second electrode are electrically connected to each other.