Composite positive electrode comprising coated carbon fiber and all-solid-state battery comprising same

By using carbon fibers coated with oxide materials in the positive electrode layer of all-solid-state batteries, the problem of capacity fading caused by the degradation of sulfide electrolytes is solved, the cycle stability and initial capacity of the battery are improved, and efficient Li+ migration and battery are achieved Long term maintenance of performance.

CN118872092APending Publication Date: 2024-10-29FACTORIAL INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027443.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-07-15
Filing Date
2023-05-24
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The thermodynamic stability, chemical-mechanical coupling and interfacial dynamics problems of the thiophosphate electrolyte in all-solid-state batteries lead to the capacity fading of the positive electrode composite layer, especially the accelerated deterioration of the sulfide electrolyte at high potentials, affecting Li+ mobility and battery Cycling stability.

Method used

Adding carbon fiber coated with oxide materials, such as Li3B11O18 coating, to the positive electrode layer reduces the deterioration at the interface between the sulfide electrolyte and carbon fiber through pressure electrical contact between the CAM particles and the carbon fiber during the manufacturing process, and improves the electrical connection path and electrical insulation. sex.

Benefits of technology

It significantly reduces the degradation of sulfide electrolytes, improves the cycle stability and initial capacity of all-solid-state batteries, achieves close to 100% CAM utilization and high initial specific capacity, and extends the cycle life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872092A_ABST
    Figure CN118872092A_ABST
Patent Text Reader

Abstract

Disclosed is a positive electrode composite layer for an all-solid-state battery comprising particles of a positive electrode active material (CAM), a solid electrolyte (SE), a conductive carbon fiber coated with an oxide material. In one embodiment, the present disclosure provides an all-solid-state battery comprising the positive electrode composite layer, where the battery has improved capacity and cycling stability due to reduced SE degradation.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Cross-references

[0002] This application claims the benefit of U.S. Serial No. 63 / 389,383, filed on July 15, 2022, and Serial No. 63 / 350,665, filed on June 9, 2022, the entire contents of each of which are incorporated herein by reference in their entirety. Technical Field

[0003] The present disclosure relates to a positive electrode layer or a positive electrode composite layer for an all-solid-state battery. Background Art

[0004] All-solid-state batteries (ASSBs) are considered to be ideal candidates for future energy storage devices because they can use lithium metal as the anode material and bring higher specific energy compared to traditional lithium-ion batteries based on organic liquid electrolytes. Thiophosphate-based solid electrolytes (SEs) appear particularly promising due to their high ionic conductivity, good mechanical compatibility, and relatively low cost. In general, poor thermodynamic stability, chemical-mechanical coupling, and interfacial dynamics of SEs are the main remaining challenges. In the positive electrode composite, side reactions include: a) decomposition at the collector / SE interface at high potentials, b) reactions between the positive active material (CAM) and SE resulting in a resistive interfacial layer, and c) decomposition reactions at the carbon / SE interface when carbon conductive additives are used. Excessive degradation of SE can reduce Li + The mobility in the positive electrode layer causes the capacity to decay over time.

[0005] Compared to the corresponding ASSB without carbon fiber (CF), the composite cathode containing carbon fiber (CF) such as vapor grown carbon fiber (VGCF) produces higher initial capacity because more CAM particles are electrically connected, resulting in higher utilization of CAM. However, the initial capacity is not constant, and due to the accelerated degradation of SE (from both CAM / SE and carbon / SE interfaces), the capacity decay is observed during battery cycling. When the potential is outside the potential stability window of SE, such as for LPS (Li7P3S 11 ) When the electrolyte is above 2.1 V, the sulfide SE will degrade at the CAM / SE and CF / SE interfaces.

[0006] To minimize the impact from SE degradation, it is very important to reduce the degradation of SE in the positive composite layers, especially those with high percentage (eg not less than 86 wt %) of CAM and low percentage (eg not more than 14 wt %) of SE.

[0007] U.S. Patent No. 7150911B2 describes vapor grown carbon fiber (VGCF) coated with an electrical insulating material such as boron nitride as a filler for thermal conductivity and electrical insulation. However, the resistivity of the coated VGCF disclosed therein is 10×10 3 Ω.cm or more, which may block the electrical connection paths required for the electrode layers.

[0008] US20150228966 A1 discloses an all-solid-state battery using carbon fiber as a conductive agent in the CAM layer, thereby improving the initial capacity due to higher utilization of the CAM by increasing the electron conduction pathway. US 9219271 B2 discloses an all-solid-state battery using a conductive carbon additive in the positive electrode layer. However, neither discloses any coated carbon material. The SE degradation problem still exists. Summary of the invention

[0009] In one embodiment, the present disclosure provides a positive electrode layer comprising CAM particles, a sulfide solid electrolyte, and a sulfide solid electrolyte coated with an oxide material (e.g., Li3B 11 O 18 ) of carbon fiber (CF), wherein the CAM particles are in electrical contact with the CF (e.g., under pressure during manufacturing). In one embodiment, the present disclosure provides an all-solid-state battery comprising a cathode layer. In one embodiment, the ASSB has increased capacity and cycle stability due to reduced SE degradation at the VGCF / SE interface. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] Figure 1 A representative structure of an ASSB with a positive electrode layer comprising CAM particles (1), sulfide SE (2), and VGCF (3) coated with an oxide material (4), wherein the CAM particles are in electrical contact with the VGCF.

[0011] Figure 2 The coating is shown to be Li3B with a thickness of about 1-2 nm. 11 O 18 TEM (transmission electron microscope) image of carbon fibers of a layer of (LBO).

[0012] Figure 3 A graph showing the specific capacity versus cycle of a half-cell consisting of a Li metal anode, an LPS SE, and NCA88 (LiNi 0.88 Co 0.09 Al 0.03Figure 2 shows the composition of the positive electrode layer of particles of LBO (O2) and VGCF (uncoated or coated). At 45°C, cycles 1 and 2 were cycled at 0.1C charge / discharge; cycles 3 and 4 were cycled at 0.33C charge / discharge; cycle 5 was cycled at 1.0C charge / discharge; and cycles 6-25 were cycled at 0.5C charge / discharge. The cycle graph compares uncoated VGCF with 2, 20, 50, and 100nm LBO coated VGCF.

[0013] Figure 4 Figure 2 shows the specific capacity versus cycle of a half-cell consisting of a Li metal anode, LPS as the SE, and NCA88 (LiNi 0.88 Co 0.09 Al 0.03 O2) particles and the cathode layer composition of VGCF (uncoated or coated). Cycles 1 and 2 were cycled at 0.1C charge / discharge; cycles 3 and 4 were cycled at 0.33C charge / discharge; cycle 5 was cycled at 1.0C charge / discharge; cycles 6-25 were cycled at 0.5C charge / discharge. The cycle diagram compares the uncoated VGCF with 20nm B2O3, LBO (Li3B 11 O 18 ), Li3BO3, and 10nm LiNbO3. DETAILED DESCRIPTION

[0014] In one embodiment, the present disclosure provides a positive electrode composite layer, the positive electrode composite layer comprising particles (1) of a positive electrode active material (CAM), a sulfide-based solid electrolyte (2), and carbon fibers (3) coated with an oxide material (4). In one embodiment, a representative structure is shown in Figure 1 middle.

[0015] In one embodiment, the sulfide solid electrolyte used in the present disclosure can be any sulfide solid electrolyte as long as it contains Li and S and has the required lithium ion conductivity. The sulfide solid electrolyte can be any one of a crystalline material, a glass ceramic, and a glass. Examples of sulfide solid electrolytes include Li2S-P2S5, Li2S-P2S5-LiHa ("Ha" is one or more halogen elements), Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4、Li7P3S 11 , Li 3.25 P 0.95 S4, and Li7-x PS 6-x Ha x (Argyrodite-type solid electrolyte, "Ha" is one or more halogen elements, where 0.2 < x < 1.8). The concentration of the sulfide solid electrolyte in the positive electrode layer is between 1 wt% and 30 wt%.

[0016] In one embodiment, the conductive carbon fiber includes but is not limited to vapor-grown carbon fiber (VGCF), carbon nanotube (CNT), multi-walled carbon nanotube (MWCNT), carbon nanofiber, and graphite fiber. The BET measured specific surface area of the CF is between 1 - 600 m 2 / g, and the resistance is not greater than 0.5 Ω·cm. In one embodiment, the concentration of the fiber in the positive electrode layer is between 0.01 wt% and 5 wt%.

[0017] In one embodiment, the oxide material is an electrically insulating material. In one embodiment, the oxide material is an inorganic oxide material. In one embodiment, the oxide material contains Li, a second element, and a third element. In one embodiment, the second element is one or more elements from Groups 15 and 16 of the periodic table (e.g., O, N, S, P). In one embodiment, the third element is a transition metal or one or more elements from Groups 13 and 14 of the periodic table (e.g., B, C, Al, Si, Ga, and Ge). In one embodiment, the oxide material is an oxide containing Li, B, and one or more elements selected from the group consisting of B, Nb, Ti, Zr, Ta, Zn, W, and Al. In one embodiment, the oxide material is an inorganic oxide material including but not limited to lithium borate, alumina, lithium zirconate (Li2ZrO3), LiNbO3, Li4SiO4, Li3PO4, Li2SiO3, LiPO3, Li2SO4, Li2WO4, Li2MoO4, LiAlO2, Li2TiO3, Li4Ti5O 12 、or their composite oxides. In one embodiment, the lithium borate includes but is not limited to Li3B 11 O 18 、Li3BO3、Li4B2O5、Li6B4O9、LiBO2、Li2B4O7、Li3B7O 12 ,and LiB3O5. In one embodiment, the inorganic oxide is any other material having a wide stability potential window such as from 1.9 V to 5.0 V. For example, the stable potential window of the inorganic oxide material is at least 1.5 V with reference to Li / Li + In one embodiment, the stable potential window of the inorganic oxide material is at least 1.5 V with reference to Li / Li +is at least 2.0 V. In one embodiment, the stable potential window of the inorganic oxide material is Li / Li + is at least 2.5 V. In one embodiment, the stable potential window of the inorganic oxide material is Li / Li + is at least 3.0 V. In one embodiment, the stable potential window of the inorganic oxide material is Li / Li + is at least 4.0 V. In one embodiment, the stable potential window of the inorganic oxide material is Li / Li + is at least 4.5 V. In one embodiment, the stable potential window of the inorganic oxide material is Li / Li + is at least 5.1V.

[0018] In one embodiment, the positive electrode composite layer is sandwiched between the positive electrode current collector and the solid electrolyte layer. In one embodiment, the positive electrode composite layer includes lithium ions (Li + ) and electron (e-) connectivity of positive electrode active materials (CAM). Li + The connectivity is mainly provided by the small particles of sulfide-based SE in the cathode composite mixture, and the e-connectivity is mainly provided by CF. Sulfide-based SE (such as LPS) has high Li + conductivity. However, they are usually + When the potential is lower than 1.7 V or higher than 2.1 V, it degrades at the CAM / SE, CF / SE, and collector / SE interfaces. The degraded byproducts usually have lower Li + The degradation of the electrolyte reduces the conductivity, which in turn requires a higher proportion of SE in the cathode composite layer, leading to a lower proportion of CAM. As a result, the degradation narrows the battery operating voltage window, hindering the ability to manufacture high energy density batteries.

[0019] In one embodiment, the present disclosure discloses a carbon fiber coated with an oxide material layer or coating for a positive electrode composite layer. In one embodiment, the coating is a carbon fiber having a relative Li / Li + Li3B with a wide voltage stability window of 1.9-4.7 V 11 O 18. The present disclosure finds that the thickness of the oxide material layer is critical. A coating with a large thickness may completely block the electron conduction pathway, which is necessary for the operation of the all-solid-state battery. A coating with a small thickness may be indistinguishable when compared to uncoated carbon fiber and may not reduce degradation. On the one hand, the coating has a certain thickness to provide a certain electrical insulation, thereby reducing SE degradation at the CF / SE interface. In one embodiment, the thickness is not less than 1 nm. In one embodiment, the thickness is not less than 2 nm. In one embodiment, the thickness is not less than 5 nm. In one embodiment, the thickness is not less than 10 nm. In one embodiment, the minimum thickness varies depending on several factors such as coating composition, inherent properties, and coating-CF interface. On the other hand, the coating should not be too thick and be thin enough to be penetrated by hard CAM particles during battery formation (5000 lbs / in 2 Pressure) to provide a thickness t of electrical contact with the CAM particles and VGCF. In one embodiment, the thickness does not exceed 200nm. In one embodiment, the thickness does not exceed 150nm. In one embodiment, the thickness does not exceed 100nm. In one embodiment, the thickness does not exceed 80nm. In one embodiment, the thickness does not exceed 50nm. In one embodiment, the thickness does not exceed 30nm. In one embodiment, the maximum thickness varies depending on several factors such as coating composition, inherent properties, and coating-CF interface. In one embodiment, the positive composite layer disclosed in the present disclosure significantly reduces the degradation of SE, thereby improving the stability of cycle life, while achieving a high initial specific capacity close to 100% CAM utilization. In one embodiment, the thickness of the coating is 1-5nm. In one embodiment, the thickness of the coating is 1-20nm. In one embodiment, the thickness of the coating is 1-50nm. In one embodiment, the thickness of the coating is 1-80nm. In one embodiment, the thickness of the coating is 1-100nm. The present disclosure will be better understood by reference to the experimental details below, but it is easy for those skilled in the art to understand that the specific experiments described in detail are only illustrative and are not meant to limit the disclosure described herein, which is defined by the claims.

[0020] In one embodiment, the oxide material can transport lithium ions in the positive electrode composite layer. Without being bound by any theory, the lithium ion conductivity is attributed to defects in the crystal structure of the inorganic oxide and the relatively small activation energy required for the ion migration process. Islam, M. et al 2012 J. Phys.: Condens. Matter 24 203201.

[0021] In one embodiment, the present disclosure provides a composite layer as a positive electrode for an all-solid-state battery, wherein the composite layer comprises particles of a positive electrode active material (CAM), a solid electrolyte, and carbon fibers coated with an oxide material. In one embodiment, the oxide material is an electrically insulating material.

[0022] In one embodiment, the thickness of the oxide material coated on the carbon fiber is 1-80 nm.

[0023] In one embodiment, the thickness of the oxide material coated on the carbon fiber is 2-50 nm. In some embodiments, the thickness of the oxide material coated on the carbon fiber ranges from 1 nm to 100 nm, 1 nm to 90 nm, 1 nm to 80 nm, 1 nm to 70 nm, 1 nm to 60 nm, 1 nm to 50 nm, 1 nm to 40 nm, 1 nm to 30 nm, 1 nm to 25 nm, 1 nm to 20 nm, 1 nm to 15 nm, 1 nm to 10 nm, 2 nm to 100 nm, 2 nm to 90 nm, 2 nm to 80 nm, 2 nm to 70 nm, 2 nm to 60 nm, 2 nm to 50 nm, 2 nm to 40 nm, 2 nm to 30 nm, 2 nm to 25 nm, 2 nm to 20 nm, 2 nm to 15 nm, 2 nm to 1 In some embodiments, the thickness is measured by observing a cross section of the dissected particles using a scanning electron microscope (SEM). In some embodiments, the thickness is measured on a transmission electron microscope (TEM).

[0024] In one embodiment, the weight percentage of CAM particles in the composite layer is not less than 65%.

[0025] In one embodiment, the weight percentage of the carbon fibers coated with the oxide material in the composite layer is between 0.01 wt % and 5.0 wt %.

[0026] In one embodiment, the weight percentage of the carbon fibers coated with the oxide material in the composite layer is between 1.0 wt % and 3.0 wt %.

[0027] In one embodiment, the oxide material is an inorganic oxide material having a wide voltage stability window.

[0028] In one embodiment, the inorganic oxide material is selected from B2O3, Li3B 11 O 18 , Li3BO3, Li4B2O5, Li6B4O9, LiBO2, Li2B4O7, Li3B7O 12 , LiB3O5, LiNbO3, Li4SiO4, Li3PO4, Li2SiO3, LiPO3, Li2SO4, Li2WO4, Li2MoO4, Li2ZrO3, LiAlO2, Li2TiO3, Li4Ti5O 12 , and a group consisting of composite oxides thereof.

[0029] In one embodiment, the inorganic oxide material is stable within a voltage range of 1.9V to 5.0V.

[0030] In some embodiments, the inorganic oxide material is Li2CO3-doped Li3BO3 (LCBO), wherein the ratio of Li2CO3-Li3BO3 is expressed as Li 2+x C 1-x B xIn some embodiments, 0 <x<1、0<x≤0.90、0<x≤0.80、0<x≤0.70、0<x≤0.60、0<x≤0.50、0<x≤0.45、0<x≤0.40、0<x≤0.35、0<x≤0.30、0<x≤0.25、0<x≤0.20、0<x≤0.15、0<x≤0.10、0.10≤x<1、0.10≤x≤0.90、0.10≤x≤0.80、0.10≤x≤0.70、0.10≤x≤0.60、0.10≤x≤0.50、0.10≤x≤0.45、0.10≤x≤0.40、0.10≤x≤0.35、0.10≤x≤0.30、0.10≤x≤0.25、0.10≤x≤0.20、0.15≤x<1、0.15≤x≤0.90、0.15≤x≤0.80、0.15≤x≤0.70、0.15≤x≤0.60、0.15≤x≤0.50、0.15≤x≤0.45、0.15≤x≤0.40、0.15≤x≤0.35、0.15≤x≤0.30、0.15≤x≤0.25、0.20≤x<1、0.20≤x≤0.90、0.20≤x≤0.80、0.20≤x≤0.70、0.20≤x≤0.60、0.20≤x≤0.50、0.20≤x≤0.45、0.20≤x≤0.40、0.20≤x≤0.35、0.20≤x≤0.30、0.25≤x<1、0.25≤x≤0.90、0.25≤x≤0.80、0.25≤x≤0.70、0.25≤x≤0.60、0.25≤x≤0.50、0.25≤x≤0.45、0.25≤x≤0.40、0.25≤x≤0.35、0.30≤x<1、0.30≤x≤0.90、0.30≤x≤0.80、0.30≤x≤0.70、0.30≤x≤0.60、0.30≤x≤0.50、0.30≤x≤0.45、0.30≤x≤0.40、0.35≤x<1、0.35≤x≤0.90、0.35≤x≤0.80、0.35≤x≤0.70、0.35≤x≤0.60、0.35≤x≤0.50、0.35≤x≤0.45、0.40≤x<1、0.40≤x≤0.90、0.40≤x≤0.80、0.40≤x≤0.70、0.40≤x≤0.60、0.40≤x≤0.50、0.45≤x<1、0.45≤x≤0.90、0.45≤x≤0.80、0.45≤x≤0.70、0.45≤x≤0.60、0.50≤x<1、0.50≤x≤0.90、0.50≤x≤0.80、0.50≤x≤0.70、0.50≤x≤0.60、0.70≤x<1、0.70≤x≤0.90, 0.70≤x≤0.80, and all ranges and subranges therein. .

[0031] In one embodiment, the solid electrolyte is a sulfur-containing inorganic electrolyte.

[0032] In one embodiment, the solid electrolyte is selected from Li2S-P2S5, Li2S-P2S5-LiHa, Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P 0.75 S4、Li7P3S 11 , Li 3.25 P 0.95 S4, and Li 7-x PS 6-x Ha x The group consisting of, wherein "Ha" is one or more halogen elements, and 0.2 <x<1.8。

[0033] In one embodiment, the weight percentage of the solid electrolyte in the composite layer is between 1 wt% and 35 wt%. In some embodiments, the concentration range of the solid electrolyte in the composite layer can be 1 wt% to 35 wt%, 1 wt% to 30 wt%, 1 wt% to 25 wt%, 1 wt% to 20 wt%, 1 wt% to 15 wt%, 1 wt% to 10 wt%, 5 wt% to 35 wt%, 5 wt% to 30 wt%, 5 wt% to 25 wt%, 5 wt% to 20 wt%, 5 wt% to 15 wt%, 10 wt% to 35 wt%, 10 wt% to 30 wt%, 10 wt% to 25 wt%, 10 wt% to 20 wt%, 15 wt% to 35 wt%, 15 wt% to 30 wt%, 15 wt% to 25 wt%, 20 wt% to 30 wt%, or any and all ranges and subranges therein.

[0034] In one embodiment, CAM is selected from Li x Mn 1-y M y A2.Li x Mn 1-y M y O 2-z X z , Li x Mn2O 4-z X z , Li x Mn 2- y My A4, Li x Co 1-y M y A2.Li x Co 1-y M y O 2-z X z , Li x Ni 1-y M y A2.Li x Ni 1-y M y O 2-z X z , Li x Ni 1-y Co y O 2-z X z , Li x Ni 1-y-z Co y M z A a , Li x Ni 1-y-z Co y M z O 2-a X a , Li x Ni 1-y-z Mn y M z A a , Li x Ni 1-y-z Mn y M z O 2-a X a The group consisting of: 0.95≤x≤1.1, 0≤y≤0.5, 0≤z≤0.5, 0≤a≤2; M is selected from the group consisting of Al, Ni, Co, Mn, Cr, Fe, Mg, Sr, V and rare earth elements; A is selected from the group consisting of O, F, S and P; X is selected from the group consisting of F, S and P.

[0035] In some embodiments, CAM is selected from Li x MO2、Li x Ni 1-y-z Co y M1 z O2 and Li x Ni 1-y-z Mn y M2 zO2, wherein M is selected from Ni, Co, Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn and at least one of the group consisting of rare earth elements, wherein M1 is selected from Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr , Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn and at least one of the group consisting of rare earth elements, wherein M2 is at least one of the group consisting of Co, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn and rare earth elements, and wherein 0.95≤x≤1.1, 1-yz>0, 0 <y≤0.5,0≤z≤0.5。

[0036] In some embodiments, CAM is selected from Li x MO2、Li x Ni 1-y-z Co y M1 z O2 and Li x Ni 1-y-z Mn y M2 z O2, wherein M is at least one selected from the group consisting of Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn and rare earth elements, wherein M1 is at least one selected from the group consisting of Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn and rare earth elements, wherein M2 is at least one selected from the group consisting of Co, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn and rare earth elements, and wherein 0.95≤x≤1.1, 1-yz>0, 0 <y≤0.5,0≤z≤0.5。

[0037] In some embodiments, the CAM is surface doped with a doping element, wherein the doping element is at least one selected from the group consisting of Ni, Co, Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn, Si, Ge, S, P and rare earth elements.

[0038] In some embodiments, the CAM is in the form of particles having an average diameter in the range of about 1 μm to about 15 μm, about 1 μm to about 12 μm, about 1 μm to about 10 μm, about 1 μm to about 7 μm, about 1 μm to about 6 μm, about 3 μm to about 15 μm, about 3 μm to about 12 μm, about 3 μm to about 10 μm, about 3 μm to about 7 μm, about 3 μm to about 6 μm, about 5 μm to about 15 μm, about 5 μm to about 12 μm, about 5 μm to about 10 μm, and all ranges and sub-ranges therein. In some embodiments, the concentration of the coated CAM in the positive electrode layer can range from about 50 wt % to about 99 wt %, about 50 wt % to about 95 wt %, about 50 wt % to about 90 wt %, about 50 wt % to about 85 wt %, about 50 wt % to about 80 wt %, about 55 wt % to about 99 wt %, about 55 wt % to about 95 wt %, about 55 wt % to about 90 wt %, about 55 wt % to about 85 wt %, about 55 wt % to about 80 wt %, about 60 wt % to about 99 wt %, about 60 wt % to about 95 wt %, about % to about 90 wt%, about 60 wt% to about 85 wt%, about 60 wt% to about 80 wt%, about 65 wt% to about 99 wt%, about 65 wt% to about 95 wt%, about 65 wt% to about 90 wt%, about 65 wt% to about 85 wt%, about 65 wt% to about 80 wt%, about 70 wt% to about 99 wt%, about 70 wt% to about 95 wt%, about 70 wt% to about 90 wt%, about 70 wt% to about 85 wt%, about 70 wt% to about 80 wt%, and all ranges and subranges therein. In some embodiments, the CAM particles can be polycrystalline or single crystalline. In some embodiments, the CAM particles can have a single size distribution or multiple size distributions.

[0039] In some embodiments, the CAM contains elemental Ni in a molar fraction of at least 50%, at least 55%, at least 60%, at least 65%, at least 70%, at least 75%, at least 80%, or at least 85% of all metal elements except lithium.

[0040] In one embodiment, the particles have an average diameter of 1-15 μm.

[0041] In one embodiment, the present disclosure provides an all-solid-state battery (ASSB) comprising:

[0042] a) as a composite layer of the positive electrode, and

[0043] b) A solid electrolyte layer between the positive and negative electrodes.

[0044] In one embodiment, the solid electrolyte layer is made of a second solid electrolyte that is the same as or different from the solid electrolyte in the positive electrode composite layer.

[0045] In one embodiment, the composite layer comprises at least 65 wt% CAM particles.

[0046] In one embodiment, the ASSB has an initial discharge specific capacity of at least 180 mAh / g at a discharge rate of 0.5C.

[0047] In one embodiment, the ASSB has an initial discharge specific capacity of at least 200 mAh / g at a discharge rate of 0.1C.

[0048] In one embodiment, the ASSB has a specific capacity of at least 180 mAh / g and a capacity retention of at least 95% after 20 cycles of discharge at a discharge rate of 0.5C.

[0049] The present disclosure will be better understood by referring to the experimental details that follow, but those skilled in the art will readily appreciate that the specific experiments described in detail are only illustrative and are not meant to limit the disclosure described herein, which is defined by the claims.

[0050] It should be noted that the transitional term "comprising" is synonymous with "including", "containing" or "characterized by", which are inclusive or open and do not exclude other unrecited elements or method steps.

[0051] Example 1

[0052] Carbon fibers coated with oxide materials were prepared using a conventional sol-gel method. 11 O 18 Coating, dissolving stoichiometric amounts of Li precursor (such as lithium acetate or lithium metal) and B precursor (such as triisopropyl borate) in a dry solvent (such as ethanol) to form a coating solution containing a lithium precursor and a borate precursor. The coating solution is added to a predetermined amount of CF (VGCF-H, fiber diameter 150nm, fiber length 10-20μm, BET surface area 13m 2 / g, aspect ratio 10-500, true density 2.0g / cm 3, apparent density VGCF(R) (standard type) 0.04g / cm, single fiber resistivity 1×10 -4 Ωcm). Based on the CFBET surface area and coating phase (for Li3B 11 O 18 , 2.16g / cm 3 ) volume density to calculate the predetermined amount of CF to obtain the desired coating thickness. The mixture was stirred for 30 minutes, and then the solvent was removed by vacuum while ultrasonicating to obtain a CF gel coated with Li precursor and B precursor. The CF gel was then annealed at 300°C under an oxygen flow for 1 hour to form a Li3B-coated 11 O 18 layer of carbon fiber. Table 1 summarizes the specific discharge capacity and cycle life retention of various positive electrode layers with coated and uncoated CF. The positive electrode layer consists of 65wt% CAM (NCA88), 5wt% CF (coated or uncoated), and 30wt% LPS. The positive electrode layer was electrochemically evaluated in a torque-cell using Li metal as the negative electrode and LPS as the SE on copper. The battery was cycled at 45°C from 2.8V to 4.25V, charged / discharged at 0.1C for cycles 1 and 2, charged / discharged at 0.33C for cycles 3 and 4, charged / discharged at 1.0C for cycle 5, and charged / discharged at 0.5C for cycles 6 to 25.

[0053] Carbon fiber or other electronically conductive materials are necessary to electrically connect all CAM particles in the positive electrode layer to achieve a high initial discharge capacity. However, the decomposition of SE in contact with CF leads to significant attenuation. In the present disclosure, an oxide material (e.g., LBO (Li3B4)) with a thickness of 2-50 nm on CF is used. 11 O 18 )) solved this problem. The coating thickness was calculated stoichiometrically using the BET surface area of ​​the CF, the bulk density of the coating composition, and the mass / moles of reagents in the coating solution (assuming 100% reagent utilization). The coating thickness was confirmed by TEM analysis. Representative TEM images are shown in Figure 2 middle.

[0054] The coated CF reduces the decay of discharge capacity while maintaining the initial cell performance at a high level. For example, for the half-cell containing uncoated VGCF, the initial discharge capacity at 0.1C discharge rate is 205.33 mAh / g. In the case of 2nm, 20nm and 50nm LBO coating on VGCF, the initial discharge capacities are 203.91 mAh / g, 206.76 mAh / g and 219.23 mAh / g, respectively. When the thickness of LBO is 100nm, the initial discharge capacity drops to 178.73 mAh / g. The coated CF effectively reduces cell decomposition, as shown by Table 1 and Figure 3 The coated CF is critical for achieving high capacity SSBs, as evidenced by the cycle-life capacity retention after 20 cycles at 0.5C in NCA88-LiNi 0.88 Co 0.09 Al 0.03 This is demonstrated by the increase in the initial discharge capacity at 0.1C rate for O2 (219.8 mAh / g).

[0055] Table 1 Initial discharge (dChg.) capacity (Cap.) at different C-rates for half-cells using uncoated VGCF and LBO coated VGCF with different coating thicknesses

[0056]

[0057] a: Cycle life 0.5C dChg. capacity retention rate is calculated by dividing the 20th cycle 0.5C dChg. capacity by the initial 0.5C dChg. capacity and multiplying by 100%.

[0058] VGCF coatings are not limited to Li-containing oxides or lithium borates. Figure 4 Uncoated VGCF with 20nm B2O3, 20nm Li3B 11 O 18 , 20nm Li3BO3, and 10nm LiNbO3. The positive electrode layer consisted of 65wt% CAM (NCA88), 5wt% CF (coated or uncoated), and 30wt% LPS. The positive electrode layer was electrochemically evaluated in a torque-cell using Li metal as the negative electrode and LPS as the SE on copper. The battery was cycled from 2.8V to 4.25V, charged / discharged at 0.1C for cycles 1 and 2, charged / discharged at 0.33C for cycles 3 and 4, charged / discharged at 1.0C for cycle 5, and charged / discharged at 0.5C for cycles 6 to 25. All coating compositions except Li3BO3 showed improved discharge capacity and 25th cycle capacity retention compared to uncoated VGCF.

[0059] Table 2 For the use of uncoated VGCF and 20nm B2O3, Li3B 11 O 18 Initial discharge (dChg.) and capacity (Cap.) of half-cells of VGCF coated with 10 nm Li3BO3 and 10 nm LiNbO3 at different C-rates.

[0060]

[0061] a: Cycle life 0.5C dChg. capacity retention rate is calculated by dividing the 20th cycle 0.5C dChg. capacity by the initial 0.5C dChg. capacity and multiplying by 100%.

Claims

1. A composite layer comprising: Particles of positive active material (CAM); solid electrolyte, and Carbon fibers coated with oxide materials.

2. The composite layer according to claim 1, wherein the thickness of the oxide material coated on the carbon fiber is 1-70 nm.

3. The composite layer according to claim 1, wherein the oxide material coated on the carbon fibers has a thickness of 2-50 nm. The composite layer according to claim 1 , wherein the weight percentage of the CAM particles in the composite layer is not less than 65%.

5. The composite layer of claim 1, wherein the weight percentage of the carbon fibers coated with oxide material in the composite layer is between 0.01 wt% and 5.0 wt%.

6. The composite layer of claim 1, wherein the weight percentage of the carbon fibers coated with oxide material in the composite layer is between 1.0 wt% and 3.0 wt%. The composite layer according to claim 1 , wherein the oxide material is an inorganic oxide material.

8. The composite layer according to claim 7, wherein the inorganic oxide material is selected from B2O3, Li3B 11 O 18 , Li4B2O5, Li6B4O9, LiBO2, Li2B4O7, Li3B7O 12 , LiB3O5, LiNbO3, Li4SiO4, Li3PO4, Li2SiO3, LiPO3, Li2SO4, Li2WO4, Li2MoO4, Li2ZrO3, LiAlO2, Li2TiO3, Li4Ti5O 12 , and a group consisting of composite oxides thereof.

9. The composite layer of claim 7, wherein the inorganic oxide is stable in a voltage range of 1.9V to 5.0V.

10. The composite layer of claim 1, wherein the solid electrolyte is a sulfur-containing inorganic electrolyte.

11. The composite layer according to claim 1, wherein the solid electrolyte is selected from the group consisting of Li2S-P2S5, Li2S-P2S5-LiHa, Li2S-P2S5-P2O5, Li2S-Li3PO4-P2S5, Li3PS4, Li4P2S6, Li 10 GeP2S 12 , Li 3.25 Ge 0.25 P0.75 S4、Li7P3S 11 , Li 3.25 P 0.95 S4 and Li 7-x PS 6-x Ha x The group consisting of, wherein Ha is one or more halogen elements, and 0.2 <x<1.8。 12. The composite layer of claim 1, wherein the weight percentage of the solid electrolyte in the composite layer is between 1 wt% and 35 wt%.

13. The composite layer according to claim 1, wherein the CAM is selected from Li x MO2、Li x Ni 1-y-z Co y M1 z O2 and Li x Ni 1-y-z Mn y M2 z O2, wherein M is selected from the group consisting of Ni, Co, Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn and rare earth elements, wherein M1 is selected from the group consisting of Mn, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr , Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn and rare earth elements, wherein M2 is at least one selected from the group consisting of Co, Al, B, Fe, Mg, Ca, Sr, Sc, Y, Ti, Zr, V, Nb, Ta, Cr, Mo, W, Rh, Pd, Cu, Zn, Cd, Ga, In, Sn and rare earth elements, and wherein 0.95≤x≤1.1, 1-yz>0, 0 <y≤0.5,0≤z≤0.5。 14. The composite layer of claim 1, wherein the particles have an average diameter of 1-15 μm.

15. An all-solid-state battery (ASSB), comprising: a) The composite layer according to claim 1 as a positive electrode; b) a negative electrode; and c) a solid electrolyte layer between the positive electrode and the negative electrode.

16. The ASSB of claim 15, wherein the solid electrolyte layer is the same as or different from the solid electrolyte in the positive electrode composite layer.

17. The ASSB of claim 15, wherein the composite layer comprises at least 65 wt% of particles of the CAM.

18. The ASSB of claim 17, wherein the ASSB has an initial discharge specific capacity of at least 180 mAh / g at a discharge rate of 0.5C.

19. The ASSB of claim 17, wherein the ASSB has an initial discharge specific capacity of at least 200 mAh / g at a discharge rate of 0.1C.

20. The ASSB of claim 17, wherein: When the ASSB is charged to 4.25V and discharged to 2.8V for 20 cycles at 45°C, at 0.1C for cycles 1 and 2, at 0.33C for cycles 3 and 4, at 1.0C for cycle 5, and at 0.5C for cycles 6 to 20, the ASSB shows a specific capacity of at least 180 mAh / g, and a cycle life retention rate of at least 95% at the 20th cycle, wherein the cycle life retention rate is the ratio of the discharge specific capacity at the 20th cycle at 45°C to the initial discharge specific capacity at 0.5C.