By using a specific carbon material composition, including a carbon material with a moderate pore size and a carbon material coated with an organic compound, the problem of difficulty in densifying the anode material of the lithium ion secondary battery during pressurization is solved, and the initial efficiency of the battery is improved. Rate characteristics and high temperature capacity maintenance rate.

CN118872094APending Publication Date: 2024-10-29MITSUBISHI CHEM CORP
0 Cites 0 Cited by

Patent Information

Application Number
CN202380026900.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-03-09
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing lithium-ion secondary battery anode materials are difficult to achieve high density during pressure processing, resulting in poor initial efficiency, rate characteristics, and residual capacity maintenance after high-temperature storage.

Method used

A specific carbon material composition is used, including a carbon material (A) and an organic compound-coated carbon material (B). The carbon material (A) has a pore diameter of 0.01 μm or more and 1 μm or less and a moderate cumulative pore volume. The carbon material (B) The organic compounds are coated to maintain flexibility and mixed to achieve high density of the negative electrode plate.

Benefits of technology

It achieves high density of the negative electrode plate, improves the initial efficiency, rate characteristics and residual capacity maintenance rate after high-temperature storage, and avoids the damage of carbon materials during pressure treatment and the problem of electrolyte flow path clogging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005037785410000471
    Figure BDA0005037785410000471
  • Figure BDA0005037785410000491
    Figure BDA0005037785410000491
Patent Text Reader

Abstract

The present invention addresses the problem of providing a carbon material composition capable of easily increasing the density of a negative electrode plate and providing a secondary battery having excellent initial efficiency, rate characteristics, and residual capacity retention rate after high-temperature storage, and as a result, providing a high-performance secondary battery. The present invention pertains to a carbon material composition containing a carbon material (A) having a cumulative pore volume in the range of 0.01 [mu] m to 1 [mu] m (inclusive) of 0.02 mL / g or more and a ratio (PD / d50 (%)) of the pore diameter to the volume-based average particle diameter represented by formula (1) of 1.8 or less, and a carbon material (B) that is an organic compound-coated carbon material. Formula (1): PD / d50 (%) = ([the mode pore diameter (PD) in the pore distribution determined by mercury intrusion method in the range of 0.01 [mu] m to 1 [mu] m (inclusive)] / [the volume-based average particle diameter (d50)]) * 100.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a carbon material composition and a method for producing the same, as well as a negative electrode and a secondary battery. Background Art

[0002] In recent years, as electronic devices have become smaller, the demand for high-capacity secondary batteries has increased. In particular, lithium-ion secondary batteries, which have higher energy density and excellent large-current charge and discharge characteristics than nickel-cadmium batteries and nickel-metal hydride batteries, have attracted attention.

[0003] Conventionally, extensive research has been conducted on increasing the capacity of lithium ion secondary batteries. In recent years, demands for higher performance of lithium ion secondary batteries have been increasing, and further higher capacity, higher input and output, longer life, and improved other characteristics are sought.

[0004] In Patent Document 1, as a negative electrode material for a non-aqueous secondary battery having high capacity and excellent cycle characteristics, a negative electrode material for a non-aqueous secondary battery is proposed, which comprises carbonaceous particles (A) and silicon oxide particles (B), wherein the cumulative pore volume of the carbonaceous particles (A) within the range of pore diameter of 0.01 μm or more and 1 μm or less is 0.08 mL / g or more, the ratio of the pore diameter to the volume-based average particle diameter (PD / d50(%)) shown in the following formula is 1.8 or less, and the particle size (d10) of the silicon oxide particles (B) from the small particle side to the 10% cumulative portion is 0.001 μm or more and 6 μm or less.

[0005] PD / d50 (%) = ([mode pore diameter in the range of 0.01 μm to 1 μm in pore diameter distribution determined by mercury porosimetry (PD)] / [volume-based average particle diameter (d50)]) × 100

[0006] In Patent Document 2, as a negative electrode material for non-aqueous secondary batteries with high capacity and good charge and discharge load characteristics, a non-aqueous secondary battery carbon material (C) is proposed, which is obtained by adding a water-soluble polymer (B) to a carbon material (A) having a surface functional group amount O / C value of more than 1% and less than 4%.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application Publication No. 2018-88406

[0010] Patent Document 2: Japanese Patent Application Publication No. 2011-198710 Summary of the invention

[0011] Problem that the invention aims to solve

[0012] The negative electrode material disclosed in Patent Document 1 does not contain a carbon material equivalent to the carbon material (B) used in the present invention, and therefore has a high hardness. It is difficult to densify the negative electrode plate using this carbon material through pressurization. If the pressurization is performed with excessive pressure, the negative electrode material particles will be destroyed and new active surfaces will be generated. Therefore, the initial efficiency, rate characteristics, and residual capacity maintenance rate after high-temperature storage are poor.

[0013] The carbon material disclosed in Patent Document 2 does not include a carbon material equivalent to the carbon material (A) used in the present invention, and is therefore easily deformed by pressurization. When a negative electrode plate using this carbon material is pressurized for high density, the negative electrode material particles are deformed and block the flow path of the electrolyte in the plate, resulting in poor initial efficiency, rate characteristics, and residual capacity after high-temperature storage.

[0014] The present invention aims to provide a carbon material composition that can easily increase the density of negative electrode plates and provide a secondary battery having excellent initial efficiency, rate characteristics, and residual capacity retention after high-temperature storage, and as a result, provide a high-performance secondary battery.

[0015] Solutions for solving problems

[0016] The inventors of the present invention have discovered that a carbon material composition can solve the above-mentioned problem. The carbon material composition comprises a carbon material (A) and a carbon material (B) which is a carbon material coated with an organic compound. The cumulative pore volume of the carbon material (A) within the range of pore diameters of greater than 0.01 μm and less than 1 μm is greater than 0.02 mL / g, and the ratio of the specified pore diameter to the volume-based average particle diameter (PD / d50(%)) is less than 1.8.

[0017] The reason why the carbon material composition of the present invention exerts the above-mentioned effects is considered to be as follows.

[0018] The carbon material (A) having a cumulative pore volume of 0.02 mL / g or more in the range of pore diameter of 0.01 μm or more and 1 μm or less and a PD / d50 (%) of 1.8 or less forms a moderately dense intra-particle void structure and appropriately ensures the inter-particle voids, so the electrolyte immersion is good, and the original initial efficiency and rate characteristics are good. It is believed that the carbon material (A) can also deform to follow the expansion of the active material particles in the electrode during charging, and has the effect of suppressing the irreversible expansion accompanying charging and discharging. On the other hand, the hardness of the negative electrode plate using only the carbon material (A) is high. If the pressure treatment is performed with excessive pressure, the negative electrode material particles will be destroyed and new active surfaces will be generated, so as a result, the initial efficiency and rate characteristics will be impaired.

[0019] The carbon material (B) as an organic compound coated carbon material maintains flexibility by being coated with an organic compound, and can be mixed with the carbon material (A) to deform flexibly during the pressurization process, thereby preventing the carbon material (A) from being crushed. In addition, the coating of the organic compound can inhibit the side reaction of the electrolyte by preventing the direct contact between the electrolyte and the carbon material, thereby improving the initial efficiency, rate characteristics, and the residual capacity maintenance rate after high temperature storage.

[0020] Therefore, the carbon material composition of the present invention comprising such carbon material (A) and carbon material (B) can be used as a negative electrode material for a secondary battery, which can easily achieve high density of the negative electrode plate and can realize a secondary battery with excellent initial efficiency, rate characteristics, and residual capacity retention rate after high-temperature storage.

[0021] The gist of the present invention is as follows.

[0022] [1] A carbon material composition comprising a carbon material (A) and a carbon material (B),

[0023] The carbon material (A) has a cumulative pore volume within a range of pore diameters of 0.01 μm or more and 1 μm or less of 0.02 mL / g or more, and a ratio of the pore diameter to the volume-based average particle diameter (PD / d50(%)) represented by the following formula (1) is 1.8 or less,

[0024] The carbon material (B) is an organic compound-coated carbon material.

[0025] Formula (1): PD / d50 (%) = ([mode pore diameter (PD) in the range of pore diameters of 0.01 μm or more and 1 μm or less in the pore distribution determined by mercury intrusion porosimetry] / [volume-based average particle diameter (d50)]) × 100

[0026] [2] The carbon material composition according to [1], wherein the circularity of the carbon material (A) determined by flow cytometry particle image analysis is 0.88 or more.

[0027] [3] The carbon material composition according to [1] or [2], wherein the carbon material (A) is derived from natural graphite.

[0028] [4] The carbon material composition according to any one of [1] to [3], wherein the carbon material (A) is a composite carbon material of spheroidized graphite and a carbonaceous material.

[0029] [5] The carbon material composition according to any one of [1] to [4], wherein the carbon material (B) is derived from natural graphite.

[0030] [6] The carbon material composition according to any one of [1] to [5], wherein the organic compound covers the basal surface of the carbon material (B).

[0031] [7] The carbon material composition according to any one of [1] to [6], wherein the organic compound is a compound derived from a polyvinyl alcohol resin.

[0032] [8] A carbon material composition according to any one of [1] to [7], wherein the carbon material (A) and the carbon material (B) account for 20% to 80% by mass and 20% to 80% by mass, respectively, out of a total of 100% by mass of the carbon material (A) and the carbon material (B).

[0033] [9] The carbon material composition according to any one of [1] to [8], wherein the mass reduction rate from 200° C. to 700° C. measured by TG-DTA is 0.04% by mass to 0.48% by mass.

[0034]

[10] A method for producing a carbon material composition, comprising the step of mixing a carbon material (A) and a carbon material (B),

[0035] The cumulative pore volume of the carbon material (A) within the range of pore diameter of 0.01 μm or more and 1 μm or less is 0.02 mL / g or more, and the ratio of the pore diameter to the volume-based average particle diameter (PD / d50(%)) represented by the following formula (1) is 1.8 or less,

[0036] The carbon material (B) is an organic compound-coated carbon material.

[0037] Formula (1): PD / d50 (%) = ([mode pore diameter (PD) in the range of pore diameters of 0.01 μm or more and 1 μm or less in the pore distribution determined by mercury intrusion porosimetry] / [volume-based average particle diameter (d50)]) × 100

[0038]

[11] A negative electrode comprising a current collector and an active material layer formed on the current collector,

[0039] The active material layer includes the carbon material composition described in any one of [1] to [9].

[0040]

[12] A secondary battery comprising a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode is the negative electrode described in

[11] .

[0041] Effects of the Invention

[0042] According to the present invention, a secondary battery having excellent initial efficiency, rate characteristics, and residual capacity maintenance rate after high-temperature storage can be provided. DETAILED DESCRIPTION

[0043] The content of the present invention will be described in detail below. The description of the inventive constituent elements described below is an example (representative example) of the embodiment of the present invention, and the present invention is not limited to these embodiments unless it exceeds the gist of the present invention.

[0044] [Carbon material composition]

[0045] The carbon material composition of the present invention comprises a specific carbon material (A) (hereinafter sometimes referred to as "the carbon material (A) of the present invention") and a carbon material (B) (hereinafter sometimes referred to as "the carbon material (B) of the present invention").

[0046] The carbon material composition of the present invention may contain only one carbon material (A) of the present invention, or may contain two or more carbon materials having different physical properties, raw carbon materials, etc. In addition, the carbon material (B) of the present invention may contain only one carbon material, or may contain two or more carbon materials having different types, physical properties, etc. of organic compounds.

[0047] [Carbon material (A)]

[0048] The carbon material (A) of the present invention has a cumulative pore volume within the range of pore diameters of 0.01 μm to 1 μm of 0.02 mL / g or more, and a ratio of the pore diameter to the volume-based average particle diameter (PD / d50(%)) represented by the following formula (1) of 1.8 or less.

[0049] Formula (1): PD / d50 (%) = ([mode pore diameter (PD) in the range of pore diameters of 0.01 μm or more and 1 μm or less in the pore distribution determined by mercury intrusion porosimetry] / [volume-based average particle diameter (d50)]) × 100

[0050] The carbon material (A) of the present invention is not particularly limited as long as the cumulative pore volume in the pore diameter range of 0.01 μm to 1 μm is 0.02 mL / g or more and PD / d50 (%) is 1.8 or less, and examples thereof include graphite, amorphous carbon, and carbonaceous materials with a low degree of graphitization.

[0051] Wherein, graphite is commercially available, has a high charge-discharge capacity of 372mAh / g in theory, and then compared with the case of using other negative electrode active materials, the improvement effect of the charge-discharge characteristics under high current density is large, so it is preferred. As graphite, natural graphite, artificial graphite, etc. can be listed, and natural graphite is more preferred from the aspect that the charge-discharge characteristics under high capacity and high current density are good.

[0052] Furthermore, those obtained by coating them with a carbonaceous material such as amorphous carbon or graphitized material may also be used.

[0053] In the present invention, these can be used alone or in combination of two or more.

[0054] Examples of the amorphous carbon used in the carbon material (A) of the present invention include particles obtained by calcining a bulk mesophase and particles obtained by subjecting a carbon precursor to an infusibility treatment and then calcining.

[0055] As carbonaceous materials with a low degree of graphitization used in the carbon material (A) of the present invention, particles obtained by calcining organic matter at a temperature usually lower than 2500° C. are listed. As organic matter, coal-based heavy oils such as coal tar pitch and dry distillation liquefied oil; straight-run heavy oils such as atmospheric residual oil and vacuum residual oil; petroleum-based heavy oils such as ethylene tar produced as a by-product during thermal cracking of crude oil, naphtha, etc.; aromatic hydrocarbons such as acenaphthylene, decacyclene, anthracene; nitrogen-containing cyclic compounds such as phenazine and acridine; sulfur-containing cyclic compounds such as thiophene; aliphatic cyclic compounds such as adamantane; polyphenyls such as biphenyl and terphenyl, polyvinyl esters such as polyvinyl chloride, polyvinyl acetate, and polyvinyl butyral, thermoplastic polymers such as polyvinyl alcohol, etc. are listed.

[0056] Examples of artificial graphite include: those obtained by heating organic substances such as coal tar pitch, coal-based heavy oil, atmospheric residual oil, petroleum-based heavy oil, aromatic hydrocarbons, nitrogen-containing cyclic compounds, sulfur-containing cyclic compounds, polyphenylene, polyvinyl chloride, polyvinyl alcohol, polyacrylonitrile, polyvinyl butyral, natural polymers, polyphenylene sulfide, polyphenylene ether, furfuryl alcohol resin, phenol-formaldehyde resin, and imide resin to 2500° C. or above to graphitize them.

[0057] Examples of natural graphite include earthy graphite, scaly graphite, and flaky graphite. Among these natural graphites, scaly graphite and flaky graphite are preferred, and flaky graphite is more preferred, from the viewpoint of high graphitization degree and small amount of impurities.

[0058] Among natural graphites, spheroidized natural graphites are most preferred from the viewpoints of forming appropriate dense pores inside the carbon material and exhibiting excellent particle packing properties and charge and discharge load characteristics.

[0059] As the carbon material (A) of the present invention, particles obtained by coating the above-mentioned artificial graphite or natural graphite with amorphous carbon and / or a carbonaceous material with a low degree of graphitization can also be used. The carbon material (A) can also contain oxides and other metals. Examples of other metals include metals that can be alloyed with Li, such as Sn, Si, Al, and Bi.

[0060] <Method for producing carbon material (A)>

[0061] The method for manufacturing the carbon material (A) of the present invention is not particularly limited as long as it can be manufactured to have a cumulative pore volume of 0.02 mL / g or more within a range of pore diameters of 0.01 μm or more and PD / d50 (%) of 1.8 or less. As one of the means for achieving this, the following method can be cited: fine powder produced when spheroidizing (granulating) flaky natural graphite whose particle size is adjusted so that d50 becomes 80 μm or less is attached to a base material of graphite (hereinafter sometimes referred to as spheroidized graphite) after spheroidization, and / or particles encapsulated in spheroidized graphite are spheroidized.

[0062] Specifically, there may be a granulation step of granulating the raw carbon material by imparting at least one mechanical energy of impact, compression, friction, and shear force, and the granulation step is carried out in the presence of a granulating agent that satisfies the following conditions 1) and 2):

[0063] 1) The raw carbon material is in liquid state during the granulation step.

[0064] 2) The granulating agent does not contain an organic solvent, or, if it contains an organic solvent, at least one of the organic solvents does not have a flash point or, if it has a flash point, the flash point is 5° C. or higher.

[0065] If the granulation step is provided, other steps may be provided as needed. Other steps may be implemented individually or in multiple steps simultaneously. As one embodiment, an embodiment including the following steps 1 to 6 may be provided.

[0066] (Step 1) Step of adjusting the particle size of the raw carbon material

[0067] (Second step) Step of mixing raw carbon material with granulating agent

[0068] (Step 3) Step of granulating the raw carbon material

[0069] (Step 4) Step of removing granulating agent

[0070] (Step 5) Step of purifying the granulated carbon material

[0071] (Sixth step) A step of further adding a carbonaceous material having a lower crystallinity than the raw carbon material to the granulated carbon material

[0072] (Step 1) Step of adjusting the particle size of the raw carbon material

[0073] The raw carbon material used in the manufacture of the carbon material (A) of the present invention is not particularly limited, and the above-mentioned artificial graphite and natural graphite can be used. Among them, natural graphite is preferably used from the aspect of high crystallinity and high capacity. As natural graphite, for example, scaly, flaky, blocky or plate-like natural graphite can be listed, among which flaky graphite is preferred.

[0074] The volume-based average particle size d50 (hereinafter sometimes referred to as "d50") of the raw carbon material obtained in the first step is preferably greater than 1 μm, more preferably greater than 2 μm, further preferably greater than 3 μm, and preferably less than 80 μm, more preferably less than 50 μm, further preferably less than 35 μm, particularly preferably less than 20 μm, especially preferably less than 10 μm, and most preferably less than 8 μm.

[0075] When d50 is in the above range, the increase of irreversible capacity and the decrease of cycle characteristics can be prevented. In addition, the intra-particle void structure of spheroidized graphite can be densely controlled, and PD / d50(%) can be easily made less than 1.8. Therefore, the electrolyte can be efficiently distributed throughout the intra-particle voids, so that the Li ion embedding and de-embedding sites in the particles can be efficiently utilized, so there is a tendency for low-temperature output characteristics and cycle characteristics to improve. Furthermore, the circularity of spheroidized graphite can be adjusted to be high, so the curvature of Li ion diffusion will not increase and the electrolyte can be smoothly moved in the inter-particle voids, and the rapid charge and discharge characteristics are improved.

[0076] When d50 is within the above range, the fine powder produced in the granulation process can be attached to the base material of the graphite after granulation (hereinafter referred to as granulated carbon material) or be enclosed in the base material and granulated, so that a granulated carbon material with high sphericity and less fine powder can be obtained.

[0077] In this specification, the volume-based average particle diameter d50 is a value of a volume-based median particle diameter measured by a laser diffraction / scattering particle size distribution analyzer.

[0078] Specifically, 0.01 g of a sample was suspended in 10 mL of a 0.2% by mass aqueous solution of polyoxyethylene sorbitan monolaurate as a surfactant, and introduced into a laser diffraction / scattering particle size distribution measuring device. After irradiation with 28 kHz ultrasonic waves at a power of 60 W for 1 minute, the volume-based median particle size in the above measuring device was measured.

[0079] As a method for adjusting d50 of the raw carbon material to the above range, for example, there is a method of pulverizing and / or classifying (natural) graphite particles.

[0080] The aspect ratio of the raw carbon material is preferably 3 or more, more preferably 5 or more, further preferably 10 or more, particularly preferably 15 or more, and is preferably 1000 or less, more preferably 500 or less, further preferably 100 or less, particularly preferably 50 or less.

[0081] When the aspect ratio is at least the lower limit, strong granules are easily formed, while when the aspect ratio is at most the upper limit, particles having an appropriate particle size are easily formed.

[0082] In this specification, the aspect ratio is calculated from the longest diameter A of the particles and the shortest diameter B among the diameters perpendicular thereto when three-dimensionally observed using a scanning electron microscope, and is the average value of the aspect ratios of 50 random particles.

[0083] From the viewpoint that graphite is highly crystalline and has sufficient charge and discharge capacity, the d002 value of the raw carbon material is preferably The following are more preferably The following is further preferably the following.

[0084] From the viewpoint that graphite is highly crystalline and has sufficient charge and discharge capacity, the Lc of the raw carbon material is preferably More preferably above.

[0085] In this specification, d002 is the distance between lattice planes (002 planes) measured by X-ray diffraction of Gakushin Method, and Lc is the size of a crystallite measured by X-ray diffraction of Gakushin Method. The measurement conditions of X-ray diffraction are as follows.

[0086] Sample: A mixture of approximately 15% by mass of X-ray standard high-purity silicon powder added to the object to be measured.

[0087] X-ray: CuKα ray

[0088] Measuring range: 20°≤2θ≤30°

[0089] Step angle: 0.013°

[0090] Sample adjustment: Fill the concave part of the sample plate with a depth of 0.2mm with powder sample to make a flat sample surface

[0091] The filling structure of raw carbon material depends on the size, shape, degree of particle interaction force of particles, etc., and in this specification, tap density can also be used as one of the indicators for quantitatively discussing the filling structure. In the research of the present inventors, it is confirmed that in the graphite particles with roughly equal true density and volume reference average particle diameter, the more spherical the shape and smooth the particle surface, the higher the value of tap density display. That is, in order to improve the tap density, it is important to make the shape of the particle with curvature close to spherical, and remove the burrs and defects on the particle surface and keep it smooth. If the particle shape is close to spherical and the particle surface is smooth, the filling property of the powder is also greatly improved.

[0092] The tap density of the raw carbon material is preferably 0.1 g / cm 3 More preferably 0.15 g / cm 3 More preferably, 0.2 g / cm 3 Above, particularly preferably 0.3 g / cm 3 above.

[0093] In this specification, the tap density is the following value: using a powder density measuring instrument, the sample is passed through a sieve with a mesh size of 300 μm and falls to a diameter of 1.6 cm and a volume capacity of 20 cm 3 The sample is dropped into a cylindrical vibration container to fill the container, and then the container is vibrated 1000 times with a stroke length of 10 mm. The density value is calculated based on the volume and mass of the sample at this time.

[0094] The Raman R value of the raw carbon material is usually 0.1 or more, preferably 0.15 or more, more preferably 0.2 or more, and is usually 0.6 or less, preferably 0.5 or less, more preferably 0.4 or less.

[0095] If the Raman R value is above the lower limit, there is a tendency that the crystallinity of the particle surface is not easy to increase, and in the case of high density, the crystals are difficult to orient in a direction parallel to the negative electrode plate, avoiding a decrease in load characteristics. If the Raman R value is below the upper limit, there is a tendency that the crystallinity of the particle surface is not easy to change, the reactivity with the electrolyte can be suppressed, and a decrease in charge and discharge efficiency and an increase in gas generation can be avoided.

[0096] In this specification, the Raman R value is the following value: the Raman spectrum obtained by Raman spectroscopy is measured at 1580 cm -1 Nearby peaks P A Strength I A , and 1360cm -1 Nearby peaks P B Strength I B , calculate its intensity ratio (I B / I A ) is the value obtained.

[0097] In this manual, "1580cm -1 "Nearby" refers to 1580~1620cm -1 Range, "1360cm -1 "Nearby" refers to 1350-1370cm -1 range.

[0098] The Raman spectrum was measured using a Raman spectrometer. Specifically, the measurement container was filled by allowing the carbon material to fall naturally into the measurement container, and the measurement container was rotated in a plane perpendicular to the laser while irradiating the measurement container with an argon ion laser. The measurement conditions were as follows.

[0099] Wavelength of argon ion laser: 514.5nm

[0100] Laser power on sample: 25mW

[0101] Resolution: 4cm -1

[0102] Measuring range: 1100cm -1 ~1730cm -1

[0103] Peak intensity measurement, peak half-value width measurement: background processing, smoothing processing (5-point convolution operation based on simple average)

[0104] The specific surface area (SA) of the raw carbon material is preferably 0.3 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 2m 2 / g or more, most preferably 5m 2 / g or more, and preferably 30 m 2 / g or less, more preferably 20m 2 / g or less, more preferably 15m 2 / g or less.

[0105] When the specific surface area is within the above range, the acceptability of Li ions becomes good, and a decrease in battery capacity due to an increase in irreversible capacity can be prevented.

[0106] In this specification, the specific surface area (SA) is a value measured by the BET method.

[0107] Specifically, the sample was preliminarily dried under reduced pressure at 100° C. for 30 minutes under a nitrogen flow using a specific surface area measuring device, then cooled to liquid nitrogen temperature, and measured using nitrogen by the BET single point method.

[0108] The surface functional group amount O / C value of the raw carbon material is preferably greater than 0.01%, more preferably greater than 0.1%, further preferably greater than 0.3%, particularly preferably greater than 0.5%, and preferably less than 5%, more preferably less than 3%, further preferably less than 2.5%, particularly preferably less than 2%, and most preferably less than 1.5%.

[0109] If the surface functional group amount O / C value is within the above range, the hygroscopicity is suppressed and the particles are easily kept in a dry state. The electrostatic attraction between the particles becomes larger during the spheroidization treatment, so the adhesion between the particles increases, and it is easy for the fine powder to adhere to the base material and be enclosed in the spheroidized particles. Therefore, it is preferred.

[0110] In this specification, the surface functional group amount O / C value is a value measured using X-ray photoelectron spectroscopy (XPS).

[0111] Specifically, an X-ray photoelectron spectrometer is used to place the object to be measured on a sample stand with its surface flat. The Kα ray of aluminum is used as the X-ray source. The spectra of C1s (280-300 eV) and O1s (525-545 eV) are measured by multi-task measurement. The peak top of the obtained C1s is set to 284.3 eV for charge correction, and the peak areas of the spectra of C1s and O1s are calculated, and then multiplied by the device sensitivity coefficient to calculate the surface atomic concentrations of C and O, respectively. The obtained atomic concentration ratio of O to C O / C (O atomic concentration / C atomic concentration) is 100% as the surface functional group amount O / C value (%).

[0112] (Second step) Step of mixing raw carbon material with granulating agent

[0113] The granulating agent used in the embodiment of the present invention satisfies the following conditions 1) and 2).

[0114] 1) The raw carbon material is in liquid state during the granulation step.

[0115] 2) The granulating agent does not contain an organic solvent, or, if it contains an organic solvent, at least one of the organic solvents does not have a flash point or, if it has a flash point, the flash point is 5° C. or higher.

[0116] By including a granulating agent that meets the above requirements, when the raw carbon material is granulated in the subsequent third step, the granulating agent generates liquid bridging between the raw carbon materials, whereby the gravitational force generated by the capillary negative pressure in the liquid bridging between the raw carbon materials and the surface tension of the liquid acts as a liquid bridging adhesion force between the particles, thereby increasing the liquid bridging adhesion force between the raw carbon materials and allowing the raw carbon materials to be more firmly attached.

[0117] The granulating agent is preferably one having the following properties: it can be removed efficiently in the following step of removing the granulating agent (step 4) and will not adversely affect the battery characteristics such as capacity, output characteristics, storage, and cycle characteristics. Specifically, a granulating agent that generally reduces its mass by 50% or more, preferably 80% or more, more preferably 95% or more, further preferably 99% or more, and particularly preferably 99.9% or more when heated to 700° C. in an inert atmosphere can be appropriately selected.

[0118] As a method for mixing the raw carbon material with the granulating agent, for example, there can be listed: a method of mixing the raw carbon material with the granulating agent using a mixer or a kneader, a method of mixing the granulating agent obtained by dissolving an organic compound in a low-viscosity diluent solvent (organic solvent) with the raw carbon material and then removing the diluent solvent (organic solvent), etc. In addition, the following method can also be listed: when the raw carbon material is granulated in the subsequent third step, the granulating agent and the raw carbon material are added to the granulating device, and the step of mixing the raw carbon material with the granulating agent and the step of granulating are performed simultaneously.

[0119] The amount of the granulating agent added is preferably 0.1 parts by mass or more, more preferably 1 part by mass or more, further preferably 5 parts by mass or more, particularly preferably 10 parts by mass or more, and preferably 1000 parts by mass or less, more preferably 100 parts by mass or less, further preferably 80 parts by mass or less, particularly preferably 50 parts by mass or less, relative to 100 parts by mass of the raw carbon material. If it is within the above range, it is not easy to produce problems such as a decrease in sphericity due to a decrease in adhesion between particles and a decrease in productivity due to adhesion of the raw carbon material to the device.

[0120] (Step 3) Step of granulating the raw carbon material (step of spheroidizing the raw carbon material)

[0121] The carbon material is preferably subjected to spheroidization (hereinafter also referred to as granulation) by applying mechanical effects such as impact compression, friction, and shear force to the raw carbon material. In addition, the spheroidized graphite is preferably composed of a plurality of flaky or scale-like graphites and ground graphite powders, and is particularly preferably composed of a plurality of scale-like graphites.

[0122] The embodiment of the present invention preferably includes a granulation step of granulating the raw carbon material by applying any one of mechanical energy of impact, compression, friction, and shearing force.

[0123] As an apparatus used in this step, for example, an apparatus that repeatedly applies mechanical action such as compression, friction, shearing force, etc., mainly including impact force and also including interaction with the raw carbon material, can be used.

[0124] Specifically, the following device is preferred: a rotor having a plurality of blades disposed inside a housing, which is rotated at high speed to impart mechanical effects such as impact, compression, friction, shearing force, etc. to the raw carbon material introduced inside. In addition, it is preferred to have a mechanism for repeatedly imparting mechanical effects by circulating the raw carbon material.

[0125] In the step of granulating the raw carbon material, the raw carbon material can be granulated in the presence of other substances. As other substances, for example, metals or oxides thereof that can be alloyed with lithium, flaky graphite, flaky graphite, ground graphite powder, amorphous carbon, and green coke can be listed. By granulating with substances other than the raw carbon material, various types of carbon materials (A) with particle structures can be produced.

[0126] When the spheroidization treatment of the carbon material is carried out, it is more preferred that the micropowder produced in the spheroidization treatment is attached to the parent material and / or is encapsulated in the spheroidized particles and is spheroidized. By making the micropowder produced in the spheroidization treatment attached to the parent material and / or is encapsulated in the spheroidized particles and is spheroidized, the intra-particle void structure can be made more compact. Therefore, the electrolyte is effectively and efficiently distributed throughout the intra-particle voids, and the Li ion embedding and de-embedding sites in the particles can be efficiently utilized. Therefore, there is a tendency to show good low-temperature output characteristics and cycle characteristics. The micropowder attached to the parent material is not limited to the micropowder produced in the spheroidization treatment, and it can also be adjusted to include micropowder when adjusting the flaky graphite particle size, and it can also be added and mixed at an appropriate time.

[0127] In order to make the fine powder adhere to the matrix and be enclosed in the spherical particles, it is preferred to enhance the adhesion between flaky graphite particles and flaky graphite particles, between flaky graphite particles and fine powder particles, and between fine powder particles and fine powder particles. Specific examples of the adhesion between particles include van der Waals forces that are not through interparticle inclusions, electrostatic attraction, and physical and / or chemical crosslinking forces through interparticle inclusions.

[0128] The van der Waals force is bounded by a volume-based average particle size (d50) of 100 μm. The smaller the volume-based average particle size (d50), the more "self-weight < adhesion" is expressed. Therefore, the smaller the volume-based average particle size (d50) of the spherical graphite (raw carbon material) is, the greater the adhesion between particles, and the easier it is for the fine powder to adhere to the base material and be enclosed in the spherical particles, so it is preferred.

[0129] (Step 4) Step of removing granulating agent

[0130] In an embodiment of the present invention, a step of removing the granulating agent may be included. Examples of methods for removing the granulating agent include a method of washing with a solvent and a method of volatilizing and decomposing the granulating agent by heat treatment.

[0131] The granulated carbon material from which the granulating agent has been removed can also be subjected to isotropic pressure treatment.

[0132] By isotropically pressurizing the granulated carbon material, the internal voids of the granulated carbon material are compressed. As a result, the density of the crushed granulated carbon material after the pressurization treatment increases, and the high-speed charging characteristics can be improved. In addition, by isotropically pressurizing, it is not easy to cause the particles to flatten, and the spherical shape can be maintained, and the fluidity can be prevented from decreasing when slurrying.

[0133] The pressurizing means may be a roller compactor, a roller press, a briquetting machine, a cold isostatic press (CIP), a uniaxial molding machine, a tablet press, etc. Among these pressurizing means, a cold isostatic press is preferred because it can reduce internal pores while maintaining the particle shape.

[0134] (Step 5) Step of purifying the granulated carbon material

[0135] In the present invention, there may be a step of purifying the granulated carbon material. As a method for purifying the granulated carbon material, there may be a method of performing an acid treatment containing nitric acid or hydrochloric acid. The acid treatment containing nitric acid or hydrochloric acid is preferred because it can remove impurities such as metals, metal compounds, and inorganic compounds in graphite without introducing sulfates that may become highly active sulfur sources into the system.

[0136] (Sixth step) A step of further adding a carbonaceous material having a lower crystallinity than the raw carbon material to the granulated carbon material

[0137] In an embodiment of the present invention, there may also be a step of further adding a carbonaceous material having lower crystallinity than the raw carbon material to the granulated carbon material. That is, the carbonaceous material may be composited in the above-mentioned carbon material. Through this step, a carbon material (A) capable of suppressing side reactions with the electrolyte and improving rapid charge and discharge properties may be obtained.

[0138] A material obtained by further adding and adhering a carbonaceous material having a lower crystallinity than the raw carbon material to a granulated carbon material is sometimes referred to as a "carbonaceous material composite carbon material" or a "composite carbon material".

[0139] The treatment for adding and attaching (compounding) a carbonaceous substance to a granulated carbon material is as follows: an organic compound as a carbonaceous substance is mixed with the granulated carbon material, and heated in a non-oxidizing atmosphere, preferably with the flow of nitrogen, argon, carbon dioxide, etc., to carbonize or graphitize the organic compound.

[0140] As specific organic compounds of carbonaceous materials, various substances that can be used include soft or hard various coal tar pitches, carbonaceous heavy oils such as coal liquefied oil, petroleum heavy oils such as atmospheric or vacuum distillation residues of crude oil, and cracking heavy oils produced as a by-product of ethylene production by cracking naphtha.

[0141] The heating temperature (calcination temperature) varies depending on the organic compound used when preparing the mixture, and is usually heated to 800° C. or higher, preferably 900° C. or higher, and more preferably 950° C. or higher to fully perform carbonization or graphitization. The upper limit of the heating temperature is a temperature at which the carbide of the organic compound does not reach the same crystal structure as the crystal structure of the flaky graphite in the mixture, and is usually 3500° C. or lower. The upper limit of the heating temperature is preferably 3000° C., preferably 2000° C., and more preferably 1500° C. or lower.

[0142] After the above-mentioned treatment, crushing and / or pulverization are then performed to produce a carbonaceous composite carbon material.

[0143] Unless the effects of the present embodiment are impaired, other steps may be added and control conditions not described above may be added.

[0144] Relative to the granulated carbon material as a raw material, the content of the carbonaceous material in the carbonaceous composite carbon material is usually 0.01% by mass or more, preferably 0.1% by mass or more, more preferably 0.3% or more, further preferably 0.7% by mass or more, particularly preferably 1% by mass or more, and most preferably 1.5% by mass or more. In addition, the above content is usually 30% by mass or less, preferably 20% by mass or less, further preferably 15% by mass or less, and particularly preferably 10% by mass or less.

[0145] If the content of the carbonaceous material in the carbonaceous material composite carbon material is above the lower limit, there is a tendency that the effect achieved by coating is easily obtained, such as an increase in initial efficiency, an increase in residual capacity during high-temperature storage, etc. If the content of the carbonaceous material in the carbonaceous material composite carbon material is below the upper limit, there is a tendency that the capacity reduction can be suppressed, and in the case of pressurization treatment with sufficient pressure to achieve high capacity in a non-aqueous secondary battery, the material destruction of the carbon material can be suppressed, and the increase in irreversible capacity of charge and discharge during the initial cycle and the reduction in initial efficiency can be suppressed.

[0146] Carbonaceous Material The content of carbonaceous material in the composite carbon material can be calculated from the sample mass before and after the material is calcined by the following formula (2). In this case, the calculation is performed assuming that there is no mass change in the granulated carbon material before and after the calcination.

[0147] Formula (2): Carbonaceous matter content (mass %) = [(w2-w1) / w1] × 100

[0148] (w1 is the mass of the granulated carbon material (kg), w2 is the mass of the carbonaceous composite carbon material (kg))

[0149] In order to improve the orientation of the electrode plate, the permeability of the electrolyte, the conductivity, etc., and to improve the cycle characteristics and electrode plate swelling, a carbon material different from the above-mentioned granulated carbon material may be mixed.

[0150] <Preferred embodiment of carbon material (A)>

[0151] From the viewpoint of suppressing side reactions with the electrolyte and improving rapid charge and discharge properties, the carbon material (A) of the present invention is preferably a composite carbon material of spheroidized graphite, especially spheroidized graphite derived from natural graphite, and a carbonaceous material (amorphous carbon).

[0152] In the composite carbon material, the mass ratio of spheroidized graphite to amorphous carbon is preferably spheroidized graphite: amorphous carbon = 100: 0.1 to 20, and particularly preferably 100: 1.5 to 10. If the mass ratio of amorphous carbon to spheroidized graphite is above the lower limit of the above range, the side reaction with the electrolyte is reduced. If the mass ratio is below the upper limit, the crushing during the pressurized treatment can be suppressed, and the initial efficiency and the residual capacity maintenance rate during high temperature storage can be suppressed.

[0153] <Physical properties of carbon material (A)>

[0154] The mode pore diameter (PD) within the range of pore diameter of 0.01 μm or more and 1 μm or less of the carbon material (A) of the present invention is preferably 0.01 μm or more, more preferably 0.03 μm or more, further preferably 0.05 μm or more, particularly preferably 0.06 μm or more, most preferably 0.07 μm or more, and preferably 1 μm or less, more preferably 0.65 μm or less, further preferably 0.5 μm or less, further more preferably 0.4 μm or less, particularly preferably 0.3 μm or less, and most preferably 0.2 μm or less.

[0155] If the mode pore diameter (PD) in the range of pore diameters of 0.01 μm or more and 1 μm or less is within the above range, there is a tendency that the electrolyte efficiently spreads throughout the voids within the particles, the Li ion insertion and extraction sites within the particles can be efficiently utilized, and the low-temperature output characteristics and cycle characteristics are improved.

[0156] The cumulative pore volume of the carbon material (A) of the present invention within the range of pore diameters of 0.01 μm or more and 1 μm or less is preferably 0.02 mL / g or more, more preferably 0.03 mL / g or more, and preferably 0.30 mL / g or less, more preferably 0.25 mL / g or less, further preferably 0.20 mL / g or less, and particularly preferably 0.18 mL / g or less.

[0157] If the cumulative pore volume within the range of pore diameters of 0.01 μm or more and 1 μm or less is within the above range, the electrolyte can be smoothly and efficiently distributed throughout the particles. Therefore, there is a tendency that the Li ion embedding and de-embedding sites not only present in the periphery of the particles but also in the particles can be effectively and efficiently utilized during charge and discharge, showing good low-temperature output characteristics.

[0158] The total pore volume of the carbon material (A) of the present invention is preferably 0.1 mL / g or more, more preferably 0.3 mL / g or more, further preferably 0.5 mL / g or more, and preferably 10 mL / g or less, more preferably 5 mL / g or less, further preferably 2 mL / g or less, and particularly preferably 1 mL / g or less.

[0159] When the total pore volume is within the above range, the thickener and binder can be easily dispersed without excessive amount of binder during plate formation, that is, during production of the negative electrode plate.

[0160] The average pore diameter of the carbon material (A) of the present invention is preferably 0.1 μm or more, more preferably 0.5 μm or more, further preferably 1.0 μm or more, particularly preferably 2.0 μm or more, and is preferably 80 μm or less, more preferably 50 μm or less, further preferably 20 μm or less.

[0161] When the average pore diameter is within the above range, there is a tendency that the amount of binder does not need to be excessive when forming an electrode plate, thereby being able to avoid a decrease in the high current density charge and discharge characteristics of the battery.

[0162] In this specification, the mode pore diameter (PD) within the range of pore diameters of 0.01 μm to 1 μm, the cumulative pore volume within the range of pore diameters of 0.01 μm to 1 μm, the total pore volume and the average pore diameter are values ​​measured by mercury intrusion porosimetry.

[0163] Specifically, a mercury intrusion meter is used to weigh about 0.2 g of carbon material, and it is sealed in a powder container, and pre-treated by degassing at 25°C and below 50 μmHg for 10 minutes. Next, the pressure is reduced to 4 psia and mercury is introduced into the above container, and the pressure is increased from 4 psia to 40,000 psia in stages, and then reduced to 25 psia. The number of stages during the pressure increase is set to 80 points or more, and after maintaining a balance time of 10 seconds in each stage, the amount of mercury intrusion is measured. Based on the mercury intrusion curve obtained in this way, the pore distribution is calculated using the Washburn formula. The surface tension (γ) of mercury is set to 485 dyne / cm, and the contact angle (ψ) is set to 140° for calculation. From the obtained pore distribution, the mode pore diameter (PD) within the pore diameter range of 0.01 μm to 1 μm, the cumulative pore volume within the pore diameter range of 0.01 μm to 1 μm, the total pore volume, and the average pore diameter were calculated.

[0164] The volume-based average particle size d50 of the carbon material (A) of the present invention is preferably 3 μm or more, more preferably 4 μm or more, further preferably 5 μm or more, particularly preferably 8 μm or more, especially preferably 10 μm or more, most preferably 12 μm or more, and preferably 30 μm or less, more preferably 25 μm or less, further preferably 23 μm or less, particularly preferably 20 μm or less, and particularly preferably 17 μm or less.

[0165] If d50 is above the lower limit, there is a tendency that the increase in irreversible capacity and the initial battery capacity loss of the non-aqueous secondary battery obtained using the carbon material (A) can be suppressed. If d50 is below the upper limit, there is a tendency that the occurrence of process defects such as streaks in slurry coating, the decrease in high current density charge and discharge characteristics, and the decrease in low temperature output characteristics can be suppressed.

[0166] The carbon material (A) of the present invention has d10 of preferably 20 μm or less, more preferably 17 μm or less, further preferably 15 μm or less, particularly preferably 13 μm or less, and preferably 1 μm or more, more preferably 3 μm or more, further preferably 5 μm or more.

[0167] If d10 is within the above range, the aggregation tendency of the particles will not become too strong, which can avoid the occurrence of process defects such as increased slurry viscosity, reduced electrode strength in non-aqueous secondary batteries, and reduced initial charge and discharge efficiency. In addition, there is also a tendency to avoid a decrease in high current density charge and discharge characteristics and a decrease in low temperature output characteristics.

[0168] In this specification, d10 is a value obtained by measuring the volume-based average particle diameter d50, and the frequency % of particles in the particle size distribution is accumulated to 10% from the smallest particle diameter.

[0169] The d90 of the carbon material (A) of the present invention is preferably less than 100 μm, more preferably less than 70 μm, further preferably less than 60 μm, further more preferably less than 50 μm, particularly preferably less than 45 μm, most preferably less than 42 μm, and preferably greater than 10 μm, more preferably greater than 15 μm, further preferably greater than 17 μm, and particularly preferably greater than 20 μm.

[0170] If d90 is within the above range, there is a tendency to avoid a decrease in electrode strength and initial charge and discharge efficiency in the non-aqueous secondary battery, and to avoid the occurrence of process defects such as streaks during slurry coating, a decrease in high current density charge and discharge characteristics, and a decrease in low temperature output characteristics.

[0171] In this specification, d90 is a value at which the frequency % of particles in the particle size distribution obtained when the volume-based average particle diameter d50 is measured reaches 90% cumulatively from the smallest particle diameter.

[0172] The dmax of the carbon material (A) of the present invention is preferably 200 μm or less, more preferably 150 μm or less, further preferably 120 μm or less, particularly preferably 100 μm or less, and most preferably 80 μm or less.

[0173] When dmax is within the above range, the occurrence of process defects such as streaks tends to be suppressed.

[0174] In this specification, dmax is a value of the maximum particle size of particles measured in a particle size distribution obtained when the volume-based average particle size d50 is measured.

[0175] The PD / d50 (%) of the carbon material (A) of the present invention is represented by the following formula (1), which is 1.8 or less, preferably 1.7 or less, more preferably 1.5 or less, further preferably 1.4 or less, particularly preferably 1.3 or less, most preferably 1.2 or less, and preferably 0.01 or more, more preferably 0.1 or more, further preferably 0.2 or more.

[0176] Formula (1): PD / d50 (%) = ([mode pore diameter (PD) in the range of pore diameters of 0.01 μm or more and 1 μm or less in the pore distribution determined by mercury intrusion porosimetry] / [volume-based average particle diameter (d50)]) × 100

[0177] When PD / d50(%) is within the above range, the electrolyte efficiently spreads throughout the voids in the particles, and the Li ion insertion and extraction sites in the particles can be efficiently utilized, thereby tending to improve low-temperature output characteristics and cycle characteristics.

[0178] The frequency of the number of particles with a particle size of less than 3 μm in the carbon material (A) of the present invention is preferably greater than 1%, more preferably greater than 10%, and preferably less than 60%, more preferably less than 55%, further preferably less than 50%, particularly preferably less than 40%, and most preferably less than 30%.

[0179] When the particle number frequency is within the above range, particle disintegration and powder separation are less likely to occur during slurry kneading, electrode rolling, charge and discharge, and the like, and low-temperature output characteristics and cycle characteristics tend to be good.

[0180] In this specification, the number frequency of particles having a particle diameter of 3 μm or less is set to a value measured by a flow-type particle image analyzer.

[0181] Specifically, 0.2 g of the sample was suspended in 50 mL of a 0.2% by mass aqueous solution of polyoxyethylene sorbitan monolaurate as a surfactant, and introduced into a flow particle image analyzer. After irradiation with 28 kHz ultrasonic waves at a power of 60 W for 5 minutes, the detection range was designated as 0.6 to 400 μm, the number of particles was measured, and the frequency of the number of particles with a particle size of less than 3 μm was calculated.

[0182] The circularity of the carbon material (A) of the present invention is usually 0.88 or more, preferably 0.90 or more, more preferably 0.91 or more, and preferably 1 or less, more preferably 0.98 or less, and further preferably 0.97 or less. A circularity of 1 is a theoretically perfect sphere.

[0183] When the circularity is within the above range, the curvature of Li ion diffusion decreases, the electrolyte moves smoothly in the gaps between particles, and the carbon materials can be appropriately contacted with each other, so there is a tendency to show good rapid charge and discharge characteristics and cycle characteristics.

[0184] In this specification, the circularity is calculated by measuring the particle size distribution of the circle equivalent diameter by flow particle image analysis and using the following formula (3).

[0185] Specifically, ion exchange water is used as a dispersion medium, polyoxyethylene sorbitan monolaurate is used as a surfactant, and dispersion is performed by ultrasonic dispersion to obtain a dispersion liquid. Then, a flow image analyzer is used to photograph the shape of the particles. From the images obtained by photographing at least 1,000 particles, the circularity of particles with a circle equivalent diameter in the range of 1.5 μm to 40 μm is averaged and set as the circularity.

[0186] Formula (3): [Circularity] = [Circumference of an equivalent circle having the same area as the particle's projected shape] / [Actual circumference of the particle's projected shape]

[0187] The tap density of the carbon material (A) of the present invention is usually 0.7 g / cm 3 Above, preferably 0.75 g / cm 3 More preferably, 0.8 g / cm 3 More preferably, 0.83 g / cm 3 Above, particularly preferably 0.85 g / cm 3 Above, particularly preferably 0.88 g / cm 3 More preferably, 0.9 g / cm 3 Above, most preferably 0.95 g / cm 3 Above, and preferably 1.3 g / cm 3 Below, more preferably 1.25g / cm 3 Below, more preferably 1.2 g / cm 3 the following.

[0188] If the tap density is within the above range, defects such as streaks when making the plate are reduced, and the high-speed charge and discharge characteristics are excellent. In addition, there is a tendency that the carbon density in the plate is not easy to increase, so the calendering property is also good and it is easy to form a high-density negative electrode sheet.

[0189] From the viewpoint that graphite is highly crystalline and has sufficient charge and discharge capacity, the d002 value of the carbon material (A) of the present invention is preferably The following are more preferably The following is further preferably the following.

[0190] From the viewpoint that graphite is highly crystalline and has sufficient charge and discharge capacity, the Lc of the carbon material (A) of the present invention is preferably More preferably above.

[0191] The ash content of the carbon material (A) of the present invention is preferably 0.0001 mass% or more and preferably 1 mass% or less, more preferably 0.5 mass% or less, and further preferably 0.1 mass% or less in 100 mass% of the carbon material (A).

[0192] If the ash content is within the above range, when a secondary battery is made, the battery performance degradation caused by the reaction between the carbon material composition of the present invention and the electrolyte containing the carbon material (A) as the negative electrode material during charge and discharge can be suppressed to a negligible degree. In addition, when manufacturing the negative electrode material, a large amount of time, energy and equipment for preventing pollution are not required, so the cost increase can also be suppressed.

[0193] The specific surface area (SA) of the carbon material (A) of the present invention is preferably 0.5 m 2 / g or more, more preferably 0.8m2 / g or more, more preferably 1m 2 / g or more, and preferably 30 m 2 / g or less, more preferably 25m 2 / g or less, more preferably 20m 2 / g or less, particularly preferably 18m 2 / g or less, particularly preferably 17m 2 / g or less, and most preferably 15m 2 / g or less.

[0194] If the specific surface area is within the above range, the position for Li to enter and exit can be fully ensured, so the high-speed charge and discharge characteristics and output characteristics are excellent, and the activity of the active material to the electrolyte can be appropriately suppressed. Therefore, there is a tendency that a high-capacity battery can be manufactured without increasing the initial irreversible capacity and suppressing gas generation.

[0195] The surface functional group amount O / C value of the carbon material (A) of the present invention is preferably 0.01% or more, more preferably 0.1% or more, further preferably 0.2% or more, particularly preferably 1% or more, especially preferably 1.5% or more, most preferably 2% or more, and preferably 8% or less, more preferably 4% or less, further preferably 3.5% or less, particularly preferably 3% or less, and most preferably 2.5% or less.

[0196] If the surface functional group amount O / C value is within the above range, the reactivity of the desolvation of Li ions on the surface of the negative electrode active material with the electrolyte solvent is promoted, and the rapid charge and discharge characteristics become good. As a result, there is a tendency that the reactivity with the electrolyte is suppressed and the charge and discharge efficiency becomes good.

[0197] The true density of the carbon material (A) of the present invention is preferably 1.9 g / cm 3 More preferably, 2 g / cm 3 More preferably, 2.1 g / cm 3 Above, particularly preferably 2.2 g / cm 3 The upper limit of true density is 2.26 g / cm, which is the theoretical value of graphite. 3 .

[0198] When the true density is within the above range, the crystallinity of carbon will not be too low, and when a secondary battery is produced, an increase in the initial irreversible capacity of the secondary battery can be suppressed.

[0199] In this specification, the true density is a value measured by a liquid phase replacement method (pycnometer method) using butanol. The true density was measured five times, and the average value was used.

[0200] The aspect ratio of the carbon material (A) of the present invention is preferably 1.1 or more, more preferably 1.2 or more, and is preferably 10 or less, more preferably 8 or less, and further preferably 5 or less.

[0201] When the aspect ratio is within the above range, streaks of the slurry containing the carbon material composition of the present invention including the carbon material (A) are less likely to occur during plate formation, and a uniform coating surface can be obtained. As a result, there is a tendency to avoid a decrease in the high current density charge and discharge characteristics of the secondary battery.

[0202] The Raman R value of the carbon material (A) of the present invention is preferably 0.01 or more, more preferably 0.05 or more, further preferably 0.1 or more, particularly preferably 0.2 or more, and is preferably 1 or less, more preferably 0.8 or less, further preferably 0.6 or less, particularly preferably 0.5 or less.

[0203] If the Raman R value is within the above range, there is a tendency that the crystallinity of the carbon material (A) surface is not easy to increase, and the crystals are not easy to be oriented in a direction parallel to the negative electrode plate in the case of high density, thereby avoiding a decrease in load characteristics. In addition, there is a tendency that the crystals on the particle surface are not easy to become disordered, which can suppress the reactivity with the electrolyte, and can avoid a decrease in charge and discharge efficiency and an increase in gas generation.

[0204] The DBP (dibutyl phthalate) oil absorption of the carbon material (A) of the present invention is preferably 85 mL / 100 g or less, more preferably 70 mL / 100 g or less, further preferably 65 mL / 100 g or less, particularly preferably 60 mL / 100 g or less, and preferably 30 mL / 100 g or more, more preferably 40 mL / 100 g or more.

[0205] If the DBP oil absorption is within the above range, it means that the spheroidization of the carbon material has progressed sufficiently, and there is a tendency that streaks are less likely to occur when applying a slurry containing the carbon material. In addition, since there is a pore structure in the particles, there is a tendency to avoid a reduction in the reaction surface.

[0206] In this specification, the DBP oil absorption is a value measured in accordance with ISO 4546.

[0207] Specifically, it is a value when 40 g of a sample is added and the measurement is performed at a dropping speed of 4 mL / min, a rotation speed of 125 rpm, and a set torque of 500 N·m. Examples of the measuring apparatus include a carbon ink absorber E model manufactured by Brabender.

[0208] [Carbon material (B)]

[0209] The carbon material (B) of the present invention is an organic compound-coated carbon material.

[0210] From the viewpoint of suppressing the increase of resistance, the carbon material (B) of the present invention is preferably a carbon material with a base surface coated with an organic compound. If it is an organic compound-coated carbon material obtained by coating the base surface of the carbon material with an organic compound, it can suppress the increase of resistance and improve the initial efficiency, so it is preferred.

[0211] The basal plane refers to a benzene-fused plane of a carbon material, and as described later, refers to a surface of a carbon material having a high affinity for toluene.

[0212] The organic compound-coated carbon material obtained by coating the basal surface of the organic compound-coated carbon material can be produced by the method for producing the carbon material (B) of the present invention described below.

[0213] Whether the basal surface of the carbon material is coated with an organic compound can be confirmed by simultaneously measuring the adsorption isotherm and the adsorption heat using toluene gas. Specifically, the surface of the carbon material with a high affinity for toluene of 67 kJ / mol or more is defined as the basal surface, and the amount of toluene adsorbed in this area is reduced compared to the carbon material before coating, thereby confirming that the basal surface is coated with an organic compound.

[0214] In the carbon material (B) of the present invention, the raw carbon material is preferably natural graphite, and the organic compound coating the raw carbon material is preferably a cross-linked polyvinyl alcohol-based resin.

[0215] Such a carbon material (B) of the present invention can be produced by mixing a raw carbon material and an organic compound raw material, and allowing the organic compound raw material to be preferentially adsorbed on the basal surface of the raw carbon material.

[0216] <Raw carbon material of carbon material (B)>

[0217] The raw carbon material of the carbon material (B) is not particularly limited, and examples thereof include the following.

[0218] (Types of raw carbon materials)

[0219] Examples of the raw carbon material include carbon materials having various degrees of graphitization, ranging from graphite to amorphous carbon materials.

[0220] From the viewpoint of being easily obtained by commercial means, graphite or carbon (amorphous carbon) materials with a small degree of graphitization are particularly preferred. If such graphite or graphite (amorphous carbon) with a small degree of graphitization is used as the raw carbon material, the charge and discharge characteristics at high current density are significantly greater than when other negative electrode active materials are used, so it is preferred.

[0221] The graphite may be either natural graphite or artificial graphite, and natural graphite is preferred from the viewpoint of large specific surface area and large initial efficiency improvement effect obtained by coating with organic compounds. As graphite, graphite with few impurities is preferred, and various refining treatments are applied as needed before use.

[0222] As natural graphite, for example, earthy graphite, scaly graphite, flaky graphite, etc. can be cited. Among these natural graphites, scaly graphite and flaky graphite are preferred from the perspective of high graphitization degree and few impurities, and flaky graphite is more preferred. Among natural graphites, spherical natural graphite is most preferred from the perspective of being able to form suitable dense pores inside the carbon material, exerting excellent particle packing properties, and charge and discharge load characteristics.

[0223] Examples of artificial graphite include: graphitized materials obtained by heating organic substances such as coal tar pitch, coal-based heavy oil, atmospheric residual oil, petroleum-based heavy oil, aromatic hydrocarbons, nitrogen-containing cyclic compounds, sulfur-containing cyclic compounds, polyphenylene, polyvinyl chloride, polyvinyl alcohol, polyacrylonitrile, polyvinyl butyral, natural polymers, polyphenylene sulfide, polyphenylene ether, furfuryl alcohol resin, phenol-formaldehyde resin, and imide resin to 2500° C. or higher.

[0224] The raw carbon material can also be used by appropriately mixing particles such as metal particles and metal oxide particles in the carbon material in any combination. In addition, the raw carbon material can also be a substance in which a variety of materials are mixed in each particle. For example, the raw carbon material can be a carbonaceous particle having a structure formed by coating the surface of graphite with a carbon material with a small degree of graphitization, or a particle obtained by aggregating the carbon material through a suitable organic substance and then graphitizing it. Furthermore, the raw carbon material can also include metals such as Sn, Si, Al, and Bi that can be alloyed with Li in the above-mentioned composite particles.

[0225] (Physical Properties of Raw Carbon Material of Carbon Material (B))

[0226] From the viewpoint that graphite is highly crystalline and has sufficient charge and discharge capacity, the d002 value of the raw carbon material is preferably The following are more preferably The following is further preferably the following.

[0227] From the viewpoint that graphite is highly crystalline and has sufficient charge and discharge capacity, the Lc of the raw carbon material is preferably More preferably above.

[0228] The surface functional group amount O / C value of the raw carbon material is preferably 0.01% or more, more preferably 0.1% or more, further preferably 0.3% or more, particularly preferably 0.5% or more, and preferably 4% or less, more preferably 3.6% or less, further preferably 3% or less.

[0229] If the surface functional group amount O / C value is above the lower limit, there is a tendency that the interaction between the raw carbon material surface and the organic compound is enhanced, and the organic compound is not easy to peel off. If the surface functional group amount O / C value is below the upper limit, it is easy to adjust the O / C value by oxidation treatment, etc., and the manufacturing process can be suppressed in a short time without increasing the number of steps, so that productivity is improved and cost is reduced.

[0230] The volume-based average particle size d50 of the raw carbon material is usually 1 μm or more, preferably 4 μm or more, more preferably 6 μm or more, and is usually 50 μm or less, preferably 30 μm or less, more preferably 25 μm or less.

[0231] When d50 is equal to or greater than the lower limit, the surface area does not become too large, thereby suppressing the activity to the electrolyte. When d50 is equal to or less than the upper limit, there is a tendency to suppress process defects such as streaks during plate formation.

[0232] The specific surface area (SA) of raw carbon materials is usually 0.3 m 2 / g or more, preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, more preferably 2m 2 / g or more, particularly preferably 5 m 2 / g or more, and usually 30m 2 / g or less, preferably 20m 2 / g or less, more preferably 15m 2 / g or less.

[0233] If the specific surface area is above the lower limit, the position for Li to enter and exit can be fully ensured, so the high-speed charge and discharge characteristics and output characteristics are excellent. If the specific surface area is below the upper limit, there is a tendency that the activity of the active material to the electrolyte can be appropriately suppressed, and the increase in the initial irreversible capacity can be suppressed, and a high-capacity battery can be manufactured.

[0234] The tap density of raw carbon materials is usually 0.1 g / cm 3 Above, preferably 0.15 g / cm 3 More preferably 0.2 g / cm 3 More preferably, 0.3 g / cm 3 Above, and usually 1.3g / cm 3 Below, preferably 1.2 g / cm3 Below, more preferably 1.1 g / cm 3 the following.

[0235] When the tap density is greater than or equal to the lower limit, the high-rate charge and discharge characteristics are excellent. When the tap density is less than or equal to the upper limit, there is a tendency that an increase in the carbon density in the electrode plate is suppressed, a decrease in the rolling properties is suppressed, and a high-density negative electrode sheet is easily formed.

[0236] The Raman R value of the raw carbon material is usually 0.1 or more, preferably 0.15 or more, more preferably 0.2 or more, and is usually 0.6 or less, preferably 0.5 or less, more preferably 0.4 or less.

[0237] If the Raman R value is above the lower limit, there is a tendency that the crystallinity of the particle surface is not easy to increase, and the crystals are not easy to be oriented in a direction parallel to the negative electrode plate in the case of high density, thereby avoiding a decrease in load characteristics. If the Raman R value is above the upper limit, there is a tendency that the crystallinity of the particle surface is not easy to be disordered, thereby suppressing the reactivity with the electrolyte, and avoiding a decrease in charge and discharge efficiency and an increase in gas generation.

[0238] (Method for producing raw carbon material)

[0239] The raw material of the raw carbon material is not particularly limited as long as it is graphitized carbon particles. As mentioned above, natural graphite, artificial graphite, and powders of graphitized materials such as coke powder, needle coke powder, and resin can be used. Among them, natural graphite is preferred, and spheroidized natural graphite that has been spheroidized is particularly preferred from the viewpoint of easily showing the effect of organic compound coating treatment. Below, the manufacturing method of spheroidized natural graphite is described as an example.

[0240] In the spheroidization treatment, for example, the following apparatus can be used: an apparatus that repeatedly applies mechanical effects such as compression, friction, and shearing force, which are mainly impact force and also include interaction between particles, to the carbon particles to perform spheroidization. Specifically, the following apparatus is preferably an apparatus that has a rotor with a plurality of blades disposed inside a housing, and by rotating the rotor at high speed, applies mechanical effects such as impact compression, friction, and shearing force to the raw carbon material introduced inside.

[0241] When the raw carbon material is flaky graphite, by implementing the above-mentioned spheroidization process, the flaky natural graphite is folded into a spherical shape, or the peripheral edge portion of the raw carbon material is spherically crushed into a spherical shape, and fine powder mainly below 5 μm produced by crushing is further attached to its mother particles.

[0242] In the method for producing an organic compound-coated carbon material of the present invention, the raw carbon material may be isotropically pressurized before mixing the raw carbon material with the organic compound raw material.

[0243] By isotropically pressurizing the raw carbon material, the internal voids of the raw carbon material are compressed. As a result, the density of the crushed raw carbon material after the pressurization treatment increases, which can improve the high-speed charging characteristics, and the organic compound raw material efficiently covers the raw carbon material without being excessively absorbed into the internal pores of the raw carbon material. In addition, by isotropically pressurizing, it is not easy to cause flattening of the particles, the spherical shape can be maintained, and the fluidity can be prevented from decreasing when slurrying.

[0244] The pressurizing means may be a roller compactor, a roller press, a briquetting machine, a cold isostatic press (CIP), a uniaxial molding machine, a tablet press, etc. Among these pressurizing means, a cold isostatic press is preferred because it can reduce the internal pores while maintaining the particle shape.

[0245] <Organic compound raw materials>

[0246] From the viewpoint of forming a strong coating, the organic compound raw material to be mixed with the raw carbon material preferably has a group in the molecule that can be self-crosslinked by a plurality of hydroxyl groups or by heat or light.

[0247] As the organic compound raw material, for example, polyol resins such as polyvinyl alcohol resins, acrylic polyol resins, polyester polyol resins, polyether polyol resins, silicone resins, epoxy resins, acrylic resins with hydrolyzable silyl groups, and polyester resins can be cited as preferred organic compound raw materials. As the organic compound raw material, polyvinyl alcohol resins, acrylic polyol resins, polyester polyol resins, acrylic resins with hydrolyzable silyl groups, and polyester resins are more preferred. Polyvinyl alcohol resins, acrylic polyol resins, and polyester polyol resins are further preferred. From the viewpoint of excellent solvent resistance of the active material layer formed by using an organic compound coated carbon material, polyvinyl alcohol resins are particularly preferred.

[0248] The specific structure of the polyvinyl alcohol resin is not particularly limited as long as it is a resin having a vinyl alcohol structural unit. The polyvinyl alcohol resin is typically obtained by saponifying polyvinyl carboxylate obtained by polymerizing vinyl carboxylate monomers such as vinyl acetate, but is not limited thereto.

[0249] <Mixing of raw carbon materials and organic compound raw materials>

[0250] When the organic compound raw material and the raw coke material are mixed, it is preferred that a solution obtained by dissolving the organic compound raw material in a solvent is prepared and the solution is mixed with the raw coke material.

[0251] The solvent is not particularly limited as long as it dissolves the organic compound raw material. The solvent is preferably water, ethyl methyl ketone, toluene, acetone, methyl isobutyl ketone, ethanol, and methanol, more preferably water, ethyl methyl ketone, acetone, methyl isobutyl ketone, ethanol, and methanol, and even more preferably water.

[0252] Additives may be further added to the solution. Examples of additives include: crosslinking agents that help crosslink organic compound raw materials; surfactants and silane coupling agents that help impart wettability and adhesion to negative electrode active materials and binder resins; inorganic oxide particles that help reduce the resistance of the coating; lithium compound particles; conductive polymers such as polyaniline sulfonic acid; and compounds that form complex ions with lithium ions, such as polyethylene oxide and complex hydride.

[0253] As a method for mixing the raw coke material with the organic compound raw material, a method for mixing the raw coke material with a solution of the organic compound raw material is preferred from the perspective of being able to uniformly cover the base surface of the raw coke material with the organic compound raw material to suppress the initial gas amount and the retained gas amount.

[0254] As the mixing method, there can be mentioned: a method of stirring with a stirring blade in a fixed container, a method of rotating the container itself to rotate the contents for mixing, and a method of fluidizing the contents by airflow for mixing. Among them, from the viewpoint of mixing uniformity, the method of stirring with a stirring blade in a fixed container is preferred.

[0255] During the mixing of the raw carbon material and the organic compound raw material, heating may be performed in order to efficiently impregnate the organic compound raw material into the internal pores of the raw carbon material. The heating temperature is preferably 80°C to 180°C, more preferably 100°C to 150°C.

[0256] In the mixing of the raw carbon material and the organic compound raw material, isotropic pressure treatment can be performed from the aspect of efficiently impregnating the organic compound raw material into the internal pores of the raw carbon material. In addition, a method of mixing the raw carbon material and the organic compound raw material under reduced pressure, a method of pre-ozone treatment of the raw carbon material, etc. can also be used to efficiently impregnate the organic compound raw material into the internal pores of the raw carbon material.

[0257] The concentration of the organic compound raw material in the solution of the organic compound raw material is preferably 0.01% by mass or more, more preferably 0.03% by mass or more, further preferably 0.05% by mass or more, and is preferably 20% by mass or less, more preferably 15% by mass or less, further preferably 10% by mass or less, in 100% by mass of the solution of the organic compound raw material.

[0258] When the concentration is within the above range, the organic compound raw material can be uniformly adsorbed on the basal surface of the raw carbon material, and the effect of the present invention can be efficiently obtained.

[0259] The mixing amount of the organic compound raw material is usually 0.05 mass parts or more, preferably 0.1 mass parts or more, more preferably 0.15 mass parts or more, relative to 100 mass parts of raw carbon material, and is usually 2 mass parts or less, preferably 1.5 mass parts or less, more preferably 0.8 mass parts or less.

[0260] If the mixed amount is above the lower limit, the organic compound coated on the carbon material can be uniformly coated, thereby improving the initial efficiency of the battery. If the mixed amount is below the upper limit, there is a tendency that the organic compound coated on the carbon material will not be excessive, and the reversible capacity of the battery will not decrease.

[0261] The mixing amount of the solution of the organic compound raw material can be appropriately set according to the concentration of the solution of the above-mentioned organic compound raw material and the mixing amount of the above-mentioned organic compound raw material. It is preferably 1 mass part or more, more preferably 5 mass parts or more, and preferably 300 mass parts or less, more preferably 250 mass parts or less, relative to 100 mass parts of raw carbon material.

[0262] When the mixing amount is within the above range, uniform mixing can be performed and the drying time in the subsequent step can be shortened.

[0263] A solution of an organic compound raw material may be added to a slurry in which a raw carbon material is dispersed, and a binder may be added as needed to use the slurry as a slurry to be applied to a current collector as described below. This method can also simplify the battery manufacturing process.

[0264] After the raw carbon material and the organic compound raw material are mixed, it is preferred to dry them. From the viewpoint of forming a strong coating, the organic compound raw material may be cross-linked while drying.

[0265] The heating temperature for drying is usually not less than the boiling point of the solvent and not more than the decomposition temperature of the organic compound raw material, preferably 50 to 300°C, more preferably 100 to 250°C.

[0266] The drying heating temperature is within the above range, the drying efficiency is sufficient, the battery performance degradation caused by solvent residue can be avoided, and it is easy to prevent the decomposition of organic compound raw materials and the weakening of the interaction between the raw carbon material and the organic compound.

[0267] When drying is performed under reduced pressure, the pressure is expressed as a gauge pressure (difference from atmospheric pressure) and is usually -0.1 MPa or more, preferably -0.08 MPa or more, and is usually 0 MPa or less, preferably -0.03 MPa or less.

[0268] When the pressure is within the above range, drying can be performed relatively efficiently.

[0269] From the viewpoint of suppressing the amount of initial gas generated when manufacturing a non-aqueous secondary battery and suppressing the amount of storage gas generated in storing a non-aqueous secondary battery, the method of drying the mixture of the raw carbon material and the organic compound raw material preferably forms a uniform coating. By uniformly coating, the organic compound can be efficiently adsorbed on the specific mesopore surface. Therefore, by suppressing the side reaction of the electrolyte caused by the mesopore, it is easy to obtain the effect of suppressing gas generation.

[0270] Before drying, the process may include filtering the mixture of the raw carbon material and the organic compound raw material and washing the obtained residue with water. This process can remove the excess organic compound raw material that is not directly attached to the raw carbon material, and can suppress the reduction of battery capacity and increase of battery resistance caused by the attachment of the excess organic compound raw material.

[0271] When the carbon material (B) of the present invention contains other components, it is preferred to prepare a solution in which the other components are dissolved in a solvent, similarly to the organic compound raw material, mix the solution with the raw carbon material, and then dry the mixture by heating and / or reducing pressure.

[0272] When other components are added, a solution of the other components may be prepared separately from the organic compound raw material solution, or may be added to the same solvent as the organic compound raw material solution to prepare a solution.

[0273] The organic compound-coated carbon material obtained through the above steps may be subjected to powder processing such as pulverization, crushing, and classification as necessary.

[0274] The device used for pulverizing and crushing is not particularly limited. Examples of coarse pulverizers include shear mills, jaw crushers, impact crushers, cone crushers, etc. Examples of intermediate pulverizers include roll crushers, hammer mills, etc. Examples of fine pulverizers include ball mills, vibration mills, pin mills, stirred mills, jet mills, etc.

[0275] The device used for the classification process is not particularly limited. In the case of dry screening, for example, rotary screen, shaking screen, rotating screen, vibrating screen, etc. can be listed. In the case of dry airflow classification, for example, gravity classifier, inertial force classifier, centrifugal force classifier (classifier, cyclone separator, etc.) can be listed. Wet screening, mechanical wet classifier, hydraulic classifier, sedimentation classifier, centrifugal wet classifier, etc. can also be used.

[0276] <Physical properties of carbon material (B)>

[0277] The cumulative pore volume of the carbon material (B) of the present invention within the range of pore diameters of 0.01 μm or more and 1 μm or less is preferably 0.01 mL / g or more, more preferably 0.02 mL / g or more, further preferably 0.03 mL / g or more, and preferably 0.30 mL / g or less, more preferably 0.20 mL / g or less, further preferably 0.15 mL / g.

[0278] If the cumulative pore volume within the range of pore diameters of 0.01 μm or more and 1 μm or less is within the above range, the electrolyte can be smoothly and efficiently distributed throughout the particles, so that during charge and discharge, not only the Li ion insertion and extraction sites present in the outer periphery of the particles but also the Li ion insertion and extraction sites inside the particles can be effectively and efficiently utilized. Therefore, there is a tendency to show good low-temperature output characteristics.

[0279] The DBP (dibutyl phthalate) oil absorption of the carbon material (B) of the present invention is preferably 85 mL / 100 g or less, more preferably 70 mL / 100 g or less, further preferably 65 mL / 100 g or less, particularly preferably 60 mL / 100 g or less, and preferably 30 mL / 100 g or more, more preferably 40 mL / 100 g or more.

[0280] If the DBP oil absorption is below the upper limit, it means that the internal pores can be reduced while maintaining the particle shape, and the high-speed charging characteristics are excellent. If the DBP oil absorption is above the lower limit, there is a pore structure inside the particle, so there is a tendency to reduce the degree of Li ion insertion and extraction reactions.

[0281] In the carbon material (B) of the present invention, the carbon material is coated with an organic compound. In 100% by mass of the carbon material (B), the coating amount of the carbon material (B) of the present invention is preferably 0.05% by mass or more, more preferably 0.10% by mass or more, further preferably 0.15% by mass or more, and preferably 2.00% by mass or less, preferably 1.50% by mass or less, further preferably 0.80% by mass or less.

[0282] If the coating amount is above the lower limit, the organic compound coated on the carbon material (B) is uniformly coated, and the initial efficiency of the battery tends to be improved. If the coating amount is below the upper limit, there is a tendency that the organic compound coated on the carbon material (B) is not excessive, and the reduction in the reversible capacity of the battery and the increase in resistance can be suppressed.

[0283] In this specification, the coating amount of the carbon material (B) of the present invention with the organic compound is defined as the mass reduction rate at 200° C. to 700° C. when the carbon material (B) of the present invention is heated in nitrogen using a TG-DTA apparatus.

[0284] The volume-based average particle size d50 of the carbon material (B) of the present invention is preferably greater than 1 μm, more preferably greater than 3 μm, further preferably greater than 5 μm, particularly preferably greater than 10 μm, most preferably greater than 15 μm, and preferably less than 50 μm, more preferably less than 45 μm, further preferably less than 40 μm, particularly preferably less than 35 μm, and most preferably less than 30 μm.

[0285] If d50 is in the above-mentioned range, there is a tendency to suppress the irreversible capacity increase and initial battery capacity loss of the secondary battery obtained by using the organic compound coated carbon material as the negative electrode material. In addition, the generation of process defects such as streaks in the slurry coating, the decline in high current density charge-discharge characteristics, and the decline in low temperature input-output characteristics can also be suppressed.

[0286] The circularity of the carbon material (B) of the present invention is preferably 0.88 or more, more preferably 0.90 or more, and even more preferably 0.91 or more, and is preferably 1 or less, more preferably 0.98 or less, and even more preferably 0.97 or less.

[0287] When the circularity is within the above range, there is a tendency to suppress a decrease in the high current density charge and discharge characteristics of a secondary battery obtained by using the carbon material (B) of the present invention as a negative electrode material.

[0288] From the viewpoint of the shape of the inter-particle gaps when the negative electrode is made, the method for improving the circularity is preferably a method of implementing a spherical treatment to make the carbon material (B) spherical. As the spherical treatment, for example, there can be listed: a method of mechanically approaching a sphere by applying a shear force or a compressive force, a mechanical or physical treatment method of granulating a plurality of carbon materials by the adhesive force of the binder or the particles themselves, etc.

[0289] The tap density of the carbon material (B) of the present invention is preferably 0.7 g / cm 3 More preferably, 0.8 g / cm 3 More preferably, 0.85 g / cm 3 Above, particularly preferably 0.9 g / cm 3 Above, most preferably 0.95 g / cm 3 Above, and preferably 1.3 g / cm 3 Below, more preferably 1.2 g / cm 3 Below, more preferably 1.1 g / cm 3 the following.

[0290] If the tap density is within the above range, the defects in the process such as streaks are suppressed during the plate formation, and the high-speed charge and discharge characteristics are excellent. In addition, there is a tendency to suppress the increase of carbon density in the plate, suppress the decrease of calenderability, and easily form a high-density negative electrode sheet.

[0291] From the viewpoint that graphite is highly crystalline and has sufficient charge and discharge capacity, the d002 value of the carbon material (B) of the present invention is preferably The following are more preferably The following is further preferably the following.

[0292] Since graphite is highly crystalline and has sufficient charge and discharge capacity, the Lc of the carbon material (B) of the present invention is preferably More preferably above.

[0293] The ash content of the carbon material (B) of the present invention is preferably 0.0001 mass % or more and preferably 1 mass % or less, more preferably 0.5 mass % or less, and further preferably 0.1 mass % or less in 100 mass % of the carbon material (B).

[0294] If the ash content is within the above range, when a secondary battery is made, the battery performance degradation caused by the reaction between the carbon material composition of the present invention containing the carbon material (B) as the negative electrode material during charge and discharge and the electrolyte can be suppressed to a negligible degree. In addition, when manufacturing the negative electrode material, a large amount of time, energy and equipment for preventing pollution are not required, so the cost increase can also be suppressed.

[0295] The specific surface area (SA) of the carbon material (B) of the present invention is preferably 1 m 2 / g or more, more preferably 2m 2 / g or more, more preferably 2.5m 2 / g or more, and preferably 11 m 2 / g or less, more preferably 9m 2 / g or less, more preferably 8m 2 / g or less, particularly preferably 7m 2 / g or less, and most preferably 6m 2 / g or less.

[0296] If the specific surface area is within the above range, the area for Li insertion and extraction can be fully ensured during charge and discharge. Therefore, the high-speed charge and discharge characteristics and output characteristics are excellent, and the activity of the active material to the electrolyte can also be appropriately suppressed. Therefore, there is a tendency as follows: the initial irreversible capacity increase can be suppressed, and a high-capacity battery can be manufactured. In addition, when the carbon material composition of the present invention comprising the carbon material (B) is used as a negative electrode material to form a negative electrode, the reactivity with the electrolyte can be suppressed and gas generation can be suppressed. Therefore, a preferred non-aqueous secondary battery can be provided.

[0297] The total pore volume of the carbon material (B) of the present invention is preferably 0.1 mL / g or more, more preferably 0.2 mL / g or more, further preferably 0.25 mL / g or more, particularly preferably 0.5 mL / g or more, and preferably 10 mL / g or less, more preferably 5 mL / g or less, further preferably 2 mL / g or less, and particularly preferably 1 mL / g or less.

[0298] When the total pore volume is within the above range, the dispersion effect of the thickener and the binder can be easily obtained without making the amount of the binder excessive during the electrode plate formation.

[0299] The average pore diameter of the carbon material (B) of the present invention is preferably 0.1 μm or more, more preferably 0.5 μm or more, further preferably 1.0 μm or more, particularly preferably 2.0 μm or more, and is preferably 80 μm or less, more preferably 50 μm or less, further preferably 20 μm or less.

[0300] When the average pore diameter is within the above range, there is a tendency that the amount of binder does not need to be excessive when forming an electrode plate, thereby being able to avoid a decrease in the high current density charge and discharge characteristics of the battery.

[0301] The true density of the carbon material (B) of the present invention is preferably 1.9 g / cm 3 More preferably, 2 g / cm 3 More preferably, 2.1 g / cm 3 Above, particularly preferably 2.2 g / cm 3 The upper limit of true density is 2.26 g / cm, which is the theoretical value of graphite. 3 .

[0302] When the true density is within the above range, the crystallinity of carbon will not be too low, and when a secondary battery is produced, an increase in the initial irreversible capacity of the secondary battery can be suppressed.

[0303] The aspect ratio of the carbon material (B) of the present invention is preferably 1.1 or more, more preferably 1.2 or more, and is preferably 10 or less, more preferably 8 or less, further preferably 5 or less, and particularly preferably 3 or less.

[0304] If the aspect ratio is within the above range, streaks of the slurry containing the carbon material composition of the present invention including the carbon material (B) are less likely to occur during plate formation, and a uniform coating surface can be obtained. As a result, there is a tendency to avoid a decrease in the high current density charge and discharge characteristics of the secondary battery.

[0305] The Raman R value of the carbon material (B) of the present invention is preferably 0.1 or more, more preferably 0.15 or more, and even more preferably 0.2 or more, and is preferably 0.6 or less, more preferably 0.5 or less, and even more preferably 0.4 or less.

[0306] If the Raman R value is within the above range, there is a tendency that the crystallinity of the carbon material (B) surface is not easy to increase, and the crystals are not easy to be oriented in a direction parallel to the negative electrode plate in the case of high density, thereby avoiding a decrease in load characteristics. In addition, there is a tendency that the crystallinity of the particle surface is not easy to change, which can suppress the reactivity with the electrolyte, and can avoid a decrease in charge and discharge efficiency and an increase in gas generation.

[0307] The dmax of the carbon material (B) of the present invention is preferably 200 μm or less, more preferably 150 μm or less, further preferably 120 μm or less, particularly preferably 100 μm or less.

[0308] When dmax is within the above range, there is a tendency to suppress process defects such as streaks during electrode formation.

[0309] The d10 of the carbon material (B) of the present invention is preferably 1 μm or more, more preferably 2 μm or more, further preferably 3 μm or more, particularly preferably 5 μm or more, most preferably 7 μm or more, and preferably 30 μm or less, more preferably 20 μm or less, further preferably 17 μm or less.

[0310] If d10 is within the above range, the aggregation tendency of the particles will not become too strong, which can avoid the occurrence of adverse conditions in the process such as increased slurry viscosity, reduced electrode strength in the secondary battery, and reduced initial charge and discharge efficiency. In addition, there is also a tendency to avoid a decrease in high current density charge and discharge characteristics and a decrease in low temperature input and output characteristics.

[0311] The d90 of the carbon material (B) of the present invention is preferably 15 μm or more, more preferably 18 μm or more, further preferably 20 μm or more, particularly preferably 25 μm or more, and preferably 100 μm or less, more preferably 70 μm or less, further preferably 60 μm or less, particularly preferably 50 μm or less, and most preferably 45 μm or less.

[0312] If d90 is within the above range, there is a tendency to avoid a decrease in electrode strength and initial charge and discharge efficiency in the secondary battery, and to avoid the occurrence of undesirable conditions in the process such as streaks during slurry coating, a decrease in high current density charge and discharge characteristics, and a decrease in low temperature input and output characteristics.

[0313] The frequency of the number of particles with a particle size of less than 3 μm in the carbon material (B) of the present invention is preferably greater than 1%, more preferably greater than 10%, and preferably less than 60%, more preferably less than 55%, further preferably less than 50%, particularly preferably less than 40%, and most preferably less than 30%.

[0314] When the particle number frequency is within the above range, particle disintegration and powder separation are less likely to occur during slurry kneading, electrode rolling, charge and discharge, and the like, and low-temperature output characteristics and cycle characteristics tend to be good.

[0315] The elution amount of the organic compound of the carbon material (B) of the present invention is preferably 20 mass % or less, more preferably 15 mass % or less, further preferably 10 mass % or less, and particularly preferably 5 mass % or less, per 100 mass % of the organic compound contained in the carbon material (B).

[0316] When the elution amount is within the above range, the organic compound is less likely to be peeled off during high-temperature storage and charge-discharge cycles, and the degradation of storage characteristics and charge-discharge cycle characteristics can be effectively suppressed.

[0317] In this specification, the elution amount of organic compounds refers to: after impregnating the organic compound-coated carbon material in a salt-free mixed solvent of ethylene carbonate and ethyl methyl carbonate (volume ratio = 30:70) at 25°C for 5 hours, the supernatant is recovered and the value is calculated by the ratio of the peak intensity of the eluted component in GPC to the peak intensity in the case of 100% elution.

[0318] [Content ratio of carbon material (A) and carbon material (B)]

[0319] The carbon material composition of the present invention preferably contains 20 to 80 mass % of the carbon material (A) and 20 to 80 mass % of the carbon material (B) based on 100 mass % of the total of the carbon material (A) and the carbon material (B).

[0320] If the content ratio of the carbon material (A) in the carbon material composition of the present invention is above the above lower limit, and the content ratio of the carbon material (B) is below the above upper limit, when the pressure treatment is performed for high density, the blockage of the flow path of the electrolyte in the plate can be suppressed, and the negative electrode plate has excellent liquid immersion and excellent rate characteristics. If the content ratio of the carbon material (A) in the carbon material composition of the present invention is below the above upper limit, and the content ratio of the carbon material (B) is above the above lower limit, the negative electrode plate can be made high-densified with a relatively weak pressure, the capacity of the secondary battery can be increased, and the carbon material is not easily crushed to produce a new surface that is easy to react with the electrolyte, and the initial efficiency and the residual capacity maintenance rate after high temperature storage are excellent.

[0321] The content ratio of the carbon material (A) and the carbon material (B) in 100 mass% of the carbon material composition of the present invention is more preferably 40 to 75 mass% of the carbon material (A) and 25 to 60 mass% of the carbon material (B), and further preferably 50 to 70 mass% of the carbon material (A) and 30 to 50 mass% of the carbon material (B).

[0322] [Physical property ratio of carbon material (A) and carbon material (B)]

[0323] The ratio of d50 of the carbon material (B) of the present invention to d50 of the carbon material (A) of the present invention, Rd50 = [volume-based average particle size (d50) of carbon material (B)] / [volume-based average particle size (d50) of carbon material (A)], is preferably 0.1 to 2.5, more preferably 0.2 to 2.

[0324] If the ratio Rd50 is within the above range, the carbon material (B) can be present in the gaps between the carbon materials (A), or the carbon material (A) can be present in the gaps between the carbon materials (B), so that the negative electrode plate can be made high-density. In addition, the volume changes of the carbon material (A) and the carbon material (B) accompanied by the absorption and release of alkali ions such as Li ions caused by charging and discharging will be absorbed by the gaps formed by the carbon material (A) and the carbon material (B), so the disconnection of the conductive path accompanied by the volume change of the carbon material (A) and the carbon material (B) can be suppressed, resulting in improved cycle characteristics, rapid charge and discharge characteristics, and high capacity.

[0325] The ratio of d10 of the carbon material (B) of the present invention to d10 of the carbon material (A) of the present invention, Rd10=[d10 of carbon material (B)] / [d10 of carbon material (A)], is preferably 0.1 to 2.5, more preferably 0.2 to 2.

[0326] If the ratio Rd10 is within the above range, the carbon material (B) can be present in the gaps between the carbon materials (A), or the carbon material (A) can be present in the gaps between the carbon materials (B), so that the negative electrode plate can be made high-density. In addition, the volume changes of the carbon material (A) and the carbon material (B) accompanied by the absorption and release of alkali ions such as Li ions caused by charging and discharging will be absorbed by the gaps formed by the carbon material (A) and the carbon material (B), so the disconnection of the conductive path accompanied by the volume change of the carbon material (A) and the carbon material (B) can be suppressed, resulting in improved cycle characteristics, rapid charge and discharge characteristics, and high capacity.

[0327] The ratio of d90 of the carbon material (B) of the present invention to d90 of the carbon material (A) of the present invention Rd90=[d90 of carbon material (B)] / [d90 of carbon material (A)] is preferably 0.1 to 2.5, more preferably 0.2 to 2.

[0328] If the ratio Rd90 is within the above range, the carbon material (B) can be present in the gaps between the carbon materials (A), or the carbon material (A) can be present in the gaps between the carbon materials (B), so that the negative electrode plate can be made high-density. In addition, the volume changes of the carbon material (A) and the carbon material (B) accompanied by the absorption and release of alkali ions such as Li ions caused by charging and discharging will be absorbed by the gaps formed by the carbon material (A) and the carbon material (B), so the disconnection of the conductive path accompanied by the volume change of the carbon material (A) and the carbon material (B) can be suppressed, resulting in improved cycle characteristics, rapid charge and discharge characteristics, and high capacity.

[0329] The ratio of the specific surface area (SA) of the carbon material (B) of the present invention to the specific surface area (SA) of the carbon material (A) of the present invention, RSA = [specific surface area (SA) of carbon material (B)] / [specific surface area (SA) of carbon material (A)], is preferably 0.1 to 10, more preferably 0.2 to 5.

[0330] If the specific RSA is within the above range, the area for Li insertion and extraction can be fully ensured during charge and discharge, so the high-speed charge and discharge characteristics and output characteristics are excellent. In addition, the activity of the active material to the electrolyte can be appropriately suppressed, so there is a tendency to suppress the increase in initial irreversible capacity and manufacture high-capacity batteries.

[0331] The ratio of the cumulative pore volume within the range of pore diameter of the carbon material (B) of the present invention within the range of 0.01 μm to 1 μm to the cumulative pore volume within the range of pore diameter of the carbon material (A) of the present invention within the range of 0.01 μm to 1 μm is RCPV = [cumulative pore volume within the range of pore diameter of carbon material (B) within the range of 0.01 μm to 1 μm] / [cumulative pore volume within the range of pore diameter of carbon material (A) within the range of 0.01 μm to 1 μm] is preferably 0.1 to 10, and more preferably 0.2 to 5.

[0332] If the ratio RCPV is within the above range, the area for Li insertion and extraction can be fully ensured during charge and discharge, so the high-speed charge and discharge characteristics and output characteristics are excellent. In addition, the activity of the active material to the electrolyte can be appropriately suppressed, so there is a tendency to suppress the increase in initial irreversible capacity and manufacture high-capacity batteries.

[0333] The ratio of the total pore volume of the carbon material (B) of the present invention to the total pore volume of the carbon material (A) of the present invention RTPV = [total pore volume of carbon material (B)] / [total pore volume of carbon material (A)] is preferably 0.1 to 10, more preferably 0.2 to 5.

[0334] When the specific RTPV is within the above range, the dispersion effect of the thickener and the binder can be easily obtained without making the amount of the binder excessive during the formation of the electrode plate.

[0335] The ratio of the average pore diameter of the carbon material (B) of the present invention to the average pore diameter of the carbon material (A) of the present invention, RAPV = [average pore diameter of carbon material (B)] / [average pore diameter of carbon material (A)], is preferably 0.1 to 10, more preferably 0.2 to 5.

[0336] When the specific RAPV is within the above range, it is not necessary to make the amount of binder excessive during the formation of the electrode plate, and the dispersion effect of the thickener and the binder can be easily obtained.

[0337] [Method for producing carbon material composition]

[0338] The carbon material composition of the present invention can be produced by mixing the carbon material (A) of the present invention and the carbon material (B) of the present invention preferably at the above-mentioned appropriate content ratio.

[0339] The mixing method is not particularly limited as long as the carbon material (A) and the carbon material (B) are sufficiently and uniformly mixed.

[0340] The carbon material composition of the present invention may contain other components in addition to the carbon material (A) of the present invention and the carbon material (B) of the present invention within a range that does not impair the object of the present invention.

[0341] As other components that the carbon material composition of the present invention may contain, one or more conductive aids such as silicon, carbon black, and artificial graphite powder may be cited. When the carbon material composition of the present invention contains these other components, the content ratio thereof is preferably 20% by mass or less, particularly preferably 10% by mass or less in 100% by mass of the carbon material composition of the present invention.

[0342] The carbon material composition of the present invention containing these other components can be produced by mixing the other components together with the carbon material (A) of the present invention and the carbon material (B) of the present invention when producing the carbon material composition of the present invention.

[0343] [Physical properties of carbon material composition]

[0344] The mass reduction rate of the carbon material composition of the present invention is preferably 0.04 mass% or more, more preferably 0.06 mass% or more, further preferably 0.08 mass% or more, and is preferably 0.48 mass% or less, more preferably 0.40 mass% or less, further preferably 0.30 mass% or less, in 100 mass% of the carbon material composition.

[0345] If the mass reduction rate is above the lower limit, the organic compound coating amount of the carbon material (B) is sufficient, and the initial efficiency and high temperature storage characteristics are excellent. If the mass reduction rate is below the upper limit, the organic compound coating amount of the carbon material (B) will not be excessive, and the problems of decreased electronic conductivity of the negative electrode plate, powder falling from the collector, and increased resistance during charging and discharging can be suppressed.

[0346] In this specification, the mass reduction rate of the carbon material composition of the present invention is defined as the mass reduction rate at 200° C. to 700° C. when the carbon material composition of the present invention is heated in nitrogen using a TG-DTA apparatus.

[0347] In order to obtain a carbon material composition having such a mass reduction rate, it is only necessary to adjust the amount of organic compound coating of the carbon material (B) and the blending ratio of the carbon material (A) and the carbon material (B).

[0348] The volume-based average particle size d50 of the carbon material composition of the present invention is preferably 3 μm or more, more preferably 8 μm or more, further preferably 10 μm or more, particularly preferably 12 μm or more, and preferably 30 μm or less, more preferably 27 μm or less, further preferably 25 μm or less, particularly preferably 23 μm or less.

[0349] When d50 is greater than or equal to the lower limit, an increase in irreversible capacity due to an increase in specific surface area can be prevented, while when d50 is less than or equal to the upper limit, a decrease in rapid charge and discharge performance due to a decrease in the contact area between the electrolyte and the particles of the carbon material composition can be prevented.

[0350] The d10 of the carbon material composition of the present invention is preferably 1 μm or more, more preferably 2 μm or more, further preferably 3 μm or more, particularly preferably 5 μm or more, most preferably 7 μm or more, and is preferably 30 μm or less, more preferably 20 μm or less, further preferably 17 μm or less.

[0351] If d10 is within the above range, the aggregation tendency of the particles will not become too strong, which can avoid the occurrence of adverse conditions in the process such as increased slurry viscosity, reduced electrode strength in the secondary battery, and reduced initial charge and discharge efficiency. In addition, there is a tendency to avoid a decrease in high current density charge and discharge characteristics and a decrease in low temperature input and output characteristics.

[0352] The d90 of the carbon material composition of the present invention is preferably 15 μm or more, more preferably 18 μm or more, further preferably 20 μm or more, particularly preferably 25 μm or more, and preferably 100 μm or less, more preferably 70 μm or less, further preferably 60 μm or less, particularly preferably 50 μm or less, and most preferably 45 μm or less.

[0353] If d90 is within the above range, there is a tendency to avoid a decrease in electrode strength and initial charge and discharge efficiency in the secondary battery, and to avoid the occurrence of undesirable conditions in the process such as streaks during slurry coating, a decrease in high current density charge and discharge characteristics, and a decrease in low temperature input and output characteristics.

[0354] The dmax of the carbon material composition of the present invention is preferably 200 μm or less, more preferably 150 μm or less, further preferably 120 μm or less, and particularly preferably 100 μm or less.

[0355] When dmax is within the above range, there is a tendency to suppress process defects such as streaks during electrode formation.

[0356] The frequency of the number of particles with a particle size of less than 3 μm in the carbon material composition of the present invention is preferably greater than 1%, more preferably greater than 10%, and preferably less than 60%, more preferably less than 55%, further preferably less than 50%, particularly preferably less than 40%, and most preferably less than 30%.

[0357] When the particle number frequency is within the above range, particle disintegration and powder separation are less likely to occur during slurry kneading, electrode rolling, charge and discharge, and the like, and low-temperature output characteristics and cycle characteristics tend to be good.

[0358] The ash content contained in the carbon material composition of the present invention is preferably 0.0001 mass % or more and preferably 1 mass % or less, more preferably 0.5 mass % or less, and further preferably 0.1 mass % or less, based on 100 mass % of the carbon material composition.

[0359] If the ash content is within the above range, then in the case of making a secondary battery, the battery performance degradation caused by the reaction of the carbon material composition and the electrolyte can be suppressed to a negligible degree. In addition, when manufacturing the negative electrode material, a large amount of time, energy and equipment for preventing pollution are not required, so the cost increase can also be suppressed.

[0360] The tap density of the carbon material composition of the present invention is preferably 0.8 to 1.8 g / cm 3 , more preferably 0.9 to 1.7 g / cm 3 , more preferably 1.0 to 1.6 g / cm 3 .

[0361] When the tap density is within the above range, when a negative electrode is formed, the electrolyte and the carbon material (B) can be present in the gaps formed by the carbon material (A), thereby achieving high capacity and high rate characteristics.

[0362] The specific surface area of ​​the carbon material composition of the present invention based on the BET method is usually 0.5 m 2 / g or more, preferably 2m 2 / g or more, more preferably 2.5m 2 / g or more, and usually 30m 2 / g or less, preferably 20m 2 / g or less, more preferably 10m 2 / g or less, more preferably 8m 2 / g or less, particularly preferably 6.5m 2 / g or less.

[0363] If the specific surface area is above the lower limit, there are sufficient sites for Li to enter and exit, and the high-speed charge and discharge characteristics, output characteristics, and low-temperature input and output characteristics of the lithium-ion secondary battery are excellent. If the specific surface area is below the upper limit, the activity of the active material to the electrolyte can be suppressed, and the initial charge and discharge efficiency of the battery can be suppressed by suppressing the side reaction with the electrolyte. The increase in gas generation can be suppressed, and the battery capacity is excellent.

[0364] The true density of the carbon material composition of the present invention is preferably 1.9 g / cm 3 More preferably, 2 g / cm 3 More preferably, 2.1 g / cm 3 Above, particularly preferably 2.2 g / cm 3 The upper limit of true density is 2.26 g / cm, which is the theoretical value of graphite. 3 .

[0365] When the true density is within the above range, the crystallinity of carbon will not be too low, and when a secondary battery is produced, an increase in the initial irreversible capacity of the secondary battery can be suppressed.

[0366] The DBP (dibutyl phthalate) oil absorption of the carbon material composition of the present invention is preferably 85 mL / 100 g or less, more preferably 70 mL / 100 g or less, further preferably 65 mL / 100 g or less, particularly preferably 60 mL / 100 g or less, and preferably 30 mL / 100 g or more, more preferably 40 mL / 100 g or more.

[0367] If the DBP oil absorption is below the upper limit, it means that the internal pores can be reduced while maintaining the particle shape, and the high-speed charging characteristics are excellent. If the DBP oil absorption is above the lower limit, there is a pore structure inside the particle, so there is a tendency to avoid a reduction in the reaction surface.

[0368] The cumulative pore volume of the carbon material composition of the present invention within the range of pore diameters of 0.01 μm or more and 1 μm or less is preferably 0.01 mL / g or more, more preferably 0.02 mL / g or more, further preferably 0.03 mL / g or more, and preferably 0.30 mL / g or less, more preferably 0.20 mL / g or less, further preferably 0.15 mL / g or less.

[0369] If the cumulative pore volume within the range of pore diameters of 0.01 μm or more and 1 μm or less is within the above range, the electrolyte can be smoothly and efficiently distributed throughout the particles. Therefore, there is a tendency that the Li ion embedding and de-embedding sites not only present in the periphery of the particles but also in the particles can be effectively and efficiently utilized during charge and discharge, showing good low-temperature output characteristics.

[0370] The total pore volume of the carbon material composition of the present invention is preferably 0.1 mL / g or more, more preferably 0.2 mL / g or more, further preferably 0.25 mL / g or more, particularly preferably 0.5 mL / g or more, and is preferably 10 mL / g or less, more preferably 5 mL / g or less, further preferably 2 mL / g or less, and particularly preferably 1 mL / g or less.

[0371] When the total pore volume is within the above range, the dispersion effect of the thickener and the binder can be easily obtained without making the amount of the binder excessive during the electrode plate formation.

[0372] The average pore diameter of the carbon material composition of the present invention is preferably 0.1 μm or more, more preferably 0.5 μm or more, further preferably 1.0 μm or more, particularly preferably 2.0 μm or more, and is preferably 80 μm or less, more preferably 50 μm or less, further preferably 20 μm or less.

[0373] When the average pore diameter is within the above range, there is a tendency that the amount of binder does not need to be excessive when forming an electrode plate, thereby being able to avoid a decrease in the high current density charge and discharge characteristics of the battery.

[0374] The elution amount of the organic compound in the carbon material composition of the present invention is preferably 20 mass % or less, more preferably 15 mass % or less, further preferably 10 mass % or less, and particularly preferably 5 mass % or less, per 100 mass % of the organic compound contained in the carbon material composition.

[0375] When the elution amount is within the above range, the organic compound is less likely to be peeled off during high-temperature storage or charge-discharge cycles, and the degradation of storage characteristics and charge-discharge cycle characteristics can be effectively suppressed.

[0376] [negative electrode]

[0377] The negative electrode of the present invention (hereinafter appropriately referred to as "negative electrode sheet") comprises a current collector and an active material layer formed on the current collector, wherein the active material layer comprises at least the carbon material composition of the present invention. The active material layer preferably further comprises a binder.

[0378] The negative electrode of the present invention is formed by dispersing the carbon material composition of the present invention and a binder in a dispersion medium to prepare a slurry, and applying the slurry to a current collector.

[0379] As the dispersion medium, an organic solvent such as alcohol or water can be used. The slurry may further contain a conductive additive such as carbon black or artificial graphite powder.

[0380] Examples of the current collector to which the slurry is applied include metal thin films such as rolled copper foil, electrolytic copper foil, and stainless steel foil.

[0381] The density of the active material layer varies depending on the application. For applications where capacity is important, it is preferably 1.45 g / cm 3 More preferably, 1.5 g / cm 3 More preferably, 1.55 g / cm 3 Above, particularly preferably 1.6 g / cm 3 Above, and preferably 1.9 g / cm 3 the following.

[0382] When the density is within the above range, the capacity of the battery per unit volume can be sufficiently ensured, and the rate characteristics are unlikely to decrease.

[0383] [Secondary battery]

[0384] The basic structure of the secondary battery of the present invention, especially the lithium ion secondary battery, is the same as that of conventionally known lithium ion secondary batteries, and generally comprises a positive electrode capable of absorbing and releasing lithium ions, a negative electrode, and an electrolyte. As the negative electrode, the negative electrode of the present invention described above is used.

[0385] The positive electrode is formed by forming a positive electrode active material layer including a positive electrode active material and a binder on a current collector.

[0386] As the electrolyte, a non-aqueous electrolyte solution obtained by dissolving a lithium salt in a non-aqueous solvent, an electrolyte obtained by making the non-aqueous electrolyte solution into a gel, rubber or solid sheet form with an organic polymer compound or the like can be used.

[0387] A porous separator such as a porous film or nonwoven fabric is generally interposed between the positive electrode and the negative electrode to prevent short circuit between the electrodes. In this case, the porous separator is impregnated with a nonaqueous electrolyte solution before use.

[0388] [use]

[0389] The carbon material composition of the present invention can be suitably used as an active material for the negative electrode of a secondary battery, more suitably as an active material for the negative electrode of a non-aqueous secondary battery, and particularly suitably as an active material for the negative electrode of a lithium-ion secondary battery, because it is easy to achieve high density of the negative electrode plate and has excellent initial efficiency, rate characteristics, and residual capacity retention rate after high-temperature storage.

[0390] Example

[0391] Next, specific embodiments of the present invention will be described in more detail with reference to Examples, but the present invention is not limited to these Examples.

[0392] [Measurement method]

[0393] <Volume-based average particle size (d50)>

[0394] 0.01 g of the sample was suspended in 10 mL of a 0.2% by mass aqueous solution of polyoxyethylene sorbitan monolaurate as a surfactant, and introduced into a laser diffraction / scattering particle size distribution measuring apparatus (model name "LA-700", manufactured by Horiba, Ltd.), and irradiated with 28 kHz ultrasonic waves at a power of 60 W for 1 minute, and then the volume-based median particle size in the above-mentioned measuring apparatus was measured, and the volume-based median particle size was set as the volume-based average particle size d50.

[0395] <Mode pore diameter (PD) in the range of pore diameters of 0.01 μm or more and 1 μm or less, cumulative pore volume in the range of pore diameters of 0.01 μm or more and 1 μm or less, and total pore volume>

[0396] Using a mercury intrusion meter (model name "AutoPore9520", manufactured by Micromeritics), weigh about 0.2g of the sample and seal it in a powder container. Degassing is performed at 25°C and vacuum (below 50μmHg) for 10 minutes to implement pretreatment. Next, the pressure is reduced to 4psia (about 28kPa) and mercury is introduced into the above container. The pressure is increased in stages from 4psia (about 28kPa) to 40000psia (about 280MPa), and then reduced to 25psia (about 170kPa). The number of stages during the pressure increase is set to 80 points or more, and after maintaining a balance time of 10 seconds in each stage, the amount of mercury intrusion is measured. Based on the mercury intrusion curve thus obtained, the pore distribution is calculated using the Washburn formula. The surface tension (γ) of mercury is set to 485dyne / cm, and the contact angle (φ) is set to 140° for calculation.

[0397] From the obtained pore distribution, the mode pore diameter (PD) in the pore diameter range of 0.01 μm to 1 μm, the cumulative pore volume in the pore diameter range of 0.01 μm to 1 μm, and the total pore volume were calculated.

[0398] <Tap density>

[0399] Using a powder density measuring device (model name "Tap Denser KYT-3000", manufactured by Seishin Enterprise Co., Ltd.), the carbon material was passed through a sieve with a mesh size of 300 μm and dropped to a particle size of 1.6 cm in diameter and 20 cm in volume. 3 The sample was placed in a cylindrical tapping container and filled to capacity. The container was vibrated 1000 times with a stroke length of 10 mm. The density was calculated based on the volume and mass of the sample at this time, and this value was set as the tap density.

[0400] <Specific surface area (SA)>

[0401] The sample was preliminarily dried at 100°C for 30 minutes under a nitrogen flow using a specific surface area measuring apparatus "Macsorb HM MODEL-1210" (manufactured by Mountech), then cooled to liquid nitrogen temperature, and the specific surface area (SA) was measured by the BET single point method using nitrogen.

[0402] <Circularity>

[0403] Using ion exchange water as a dispersion medium and polyoxyethylene sorbitan monolaurate as a surfactant, the sample is dispersed by ultrasound to obtain a dispersion. Then, a flow image analyzer (model name "FPIA-2000", manufactured by East Asia Electronics Co., Ltd.) is used to photograph the shape of the particles. From the images obtained by photographing at least 1,000 particles, the circularity of particles with a circle equivalent diameter in the range of 1.5 μm to 40 μm is averaged and set as the circularity. The circularity is calculated according to the following formula (3).

[0404] Formula (3): [Circularity] = [Circumference of an equivalent circle having the same area as the particle's projected shape] / [Actual circumference of the particle's projected shape]

[0405] <Mass reduction rate>

[0406] Using a TG-DTA measuring apparatus (model name "STA300", manufactured by Hitachi High-Technologies Corporation), approximately 50 mg of the carbon material composition was accurately weighed and placed in an alumina sample container, and heated from 25°C to 700°C in a nitrogen atmosphere at a heating rate of 10°C / min, and the mass reduction rate between 200°C and 700°C was calculated.

[0407] [Manufacturing of Carbon Material (A)]

[0408] The flaky natural graphite with a d50 of 100 μm was crushed by a dry cyclone mill to obtain a graphite with a d50 of 10.4 μm and a tap density of 0.47 g / cm 3 , flaky natural graphite having a moisture content of 0.08 mass %.

[0409] 12 g of paraffin oil (liquid paraffin, manufactured by Wako Pure Chemical Industries, Ltd., first grade, physical properties at 25°C: viscosity = 95 cP, contact angle = 13.2°, surface tension = 317 mN / m, γCOSθ = 30.9) was added as a granulating agent to 100 g of the obtained flaky natural graphite and stirred and mixed. Then, the obtained sample was crushed and mixed at a rotation speed of 3000 rpm by a hammer mill (MF10 manufactured by IKA) to obtain flaky natural graphite to which the granulating agent was uniformly added.

[0410] The obtained flaky natural graphite to which the granulating agent is uniformly added and attached is subjected to a spheroidization treatment based on mechanical action at a rotor peripheral speed of 85 m / s for 10 minutes using a hybridization system (Hybridization System) NHS-1 manufactured by Nara Machinery Manufacturing Co., Ltd., to adhere the fine powder produced during the spheroidization treatment to the base material and to be enclosed in the spheroidized particles, and then subjected to a heat treatment at 400°C in an inert gas to obtain spheroidized graphite.

[0411] The obtained spheroidized graphite is filled in a rubber container and sealed, and after isotropic pressure treatment, the obtained molded product is crushed and classified. The obtained molded product is mixed with coal tar pitch as an amorphous carbon precursor, and after heat treatment at 1300°C in an inert gas, the roasted product is crushed and classified to obtain a carbon material (A-1) of a multilayer structure carbon material composed of graphite particles and amorphous carbon.

[0412] The roasting yield confirmed that the mass ratio of spherical graphite particles to amorphous carbon (spherical graphite particles: amorphous carbon) in the obtained multilayer structure carbon material (A-1) was 1:0.08. The measurement results of the physical properties of the carbon material (A-1) are as follows.

[0413] d50: 15.3μm

[0414] PD: 0.17μm

[0415] PD / d50: 1.11%

[0416] Cumulative pore volume of 0.01 to 1 μm: 0.03 mL / g

[0417] Total pore volume: 0.51mL / g

[0418] Roundness: 0.93

[0419] [Manufacturing of Carbon Material (B)]

[0420] The specific surface area (SA) is 6.3m 2 / g, granulated spheroidized natural graphite with d50 of 15.9μm was used as the raw material of carbon material (B). In a glass container, a mixture of 100g of the granulated spheroidized natural graphite and 200g of a 0.15% by mass aqueous solution of polyvinyl alcohol resin was stirred at 50°C for 1 hour using a stirring blade, and the graphite powder was filtered and separated by suction filtration. The graphite powder was dried at 200°C for 10 hours under reduced pressure and sieved to obtain a powdered carbon material (B-1).

[0421] A powdery carbon material (B-2) was obtained in the same manner as in the production of the carbon material (B-1) except that the concentration of the polyvinyl alcohol resin aqueous solution was changed to 0.2 mass % aqueous solution.

[0422] A powdery carbon material (B-3) was obtained in the same manner as in the production of the carbon material (B-1) except that the concentration of the polyvinyl alcohol resin aqueous solution was changed to 0.25 mass % aqueous solution.

[0423] Regarding the carbon materials (B-1) to (B-3), by simultaneously measuring the adsorption isotherm and the heat of adsorption using toluene gas, it was confirmed that the basal surface of the granulated spherical natural graphite was coated with a compound derived from the polyvinyl alcohol-based resin.

[0424] For comparison, spherical natural graphite raw material particles not coated with a polyvinyl alcohol resin were used as a carbon material (b-4).

[0425] [Example 1]

[0426] The carbon material (A-1) and the carbon material (B-1) prepared by the above method were mixed at a mass ratio of 60:40 to prepare the carbon material composition of Example 1.

[0427] [Example 2]

[0428] The carbon material (A-1) and the carbon material (B-2) prepared by the above method were mixed at a mass ratio of 60:40 to prepare a carbon material composition of Example 2.

[0429] [Example 3]

[0430] The carbon material (A-1) and the carbon material (B-3) prepared by the above method were mixed at a mass ratio of 60:40 to prepare a carbon material composition of Example 3.

[0431] [Comparative Example 1]

[0432] The carbon material of Comparative Example 1 was a carbon material containing only the carbon material (A-1) produced by the above method and not including the carbon material (B).

[0433] [Comparative Example 2]

[0434] The carbon material (A-1) produced by the above method and the carbon material (b-4) not coated with an organic compound were mixed at a mass ratio of 60:40 to produce a carbon material composition of Comparative Example 2.

[0435] [Comparative Example 3]

[0436] The carbon material of Comparative Example 3 was a carbon material containing no carbon material (A) but only the carbon material (B-1) produced by the above method.

[0437] [Comparative Example 4]

[0438] The carbon material of Comparative Example 4 was a carbon material containing no carbon material (A) but only the carbon material (B-3) produced by the above method.

[0439] The mass reduction rate of the carbon material composition or carbon material produced in each example and comparative example was measured. The results are shown in Table 1 below.

[0440] [Table 1]

[0441]

[0442] [Evaluation of battery performance]

[0443] Using the carbon material compositions or carbon materials of Examples 1 to 3 and Comparative Examples 1 to 4 as negative electrode materials, negative electrode sheets and secondary batteries were prepared by the following methods, and the following evaluations were performed.

[0444] <Production of negative electrode sheet>

[0445] The carbon material composition or carbon material of the above-mentioned embodiment or comparative example is used as a negative electrode material to prepare a negative electrode having an active material layer density of 1.60±0.03 g / cm 3 The active material layer of the electrode plate.

[0446] Specifically, 20.00±0.02 g of the negative electrode material, 20.00±0.02 g (0.200 g in terms of solid content) of a 1% sodium carboxymethyl cellulose (manufactured by Nippon Paper Industries, Ltd., MAC500LC) aqueous solution, and 0.42±0.02 g (0.2 g in terms of solid content) of an aqueous dispersion of styrene-butadiene rubber (manufactured by JSR, TRD102A) were stirred for 5 minutes using a defoaming stirring machine Taro ARE-310 manufactured by THINKY, and defoamed for 30 seconds to obtain a slurry.

[0447] The slurry was coated with a die coating device to deposit 10.00 ± 0.3 mg / cm 2 The active material layer was coated on a copper foil with a thickness of 10 μm as a current collector in a manner of 10 cm in width, and rolled using a roller with a diameter of 20 cm to adjust the density of the active material layer to 1.60 ± 0.03 g / cm 3 And obtain the negative electrode sheet.

[0448] <Evaluation of pressurization pressure>

[0449] The negative electrode sheets of the examples and comparative examples were measured so that the active material layer density was 1.6 g / cm 3 Required pressurization pressure.

[0450] <Evaluation of liquid immersion>

[0451] The liquid impregnation properties of the negative electrode sheets of Examples and Comparative Examples were evaluated as follows.

[0452] About 1 μL of propylene carbonate was dropped onto the negative electrode sheet, and the time until 0.6 μL of the propylene carbonate was absorbed by the negative electrode sheet was defined as the liquid infiltration (seconds).

[0453] <Manufacturing of non-aqueous secondary batteries>

[0454] The negative electrode sheet produced by the above method was cut into a 32 mm×42 mm square and dried under reduced pressure at 190° C. to prepare a negative electrode.

[0455] 10 parts by mass of carbon black, 41.7 parts by mass of a 12% by mass N-methylpyrrolidone solution of polyvinylidene fluoride, and an appropriate amount of N-methylpyrrolidone were added to 85 parts by mass of lithium nickel manganese cobalt composite oxide powder and kneaded to prepare a slurry. The slurry was coated on aluminum foil by a doctor blade method to a unit weight of 22.8 mg / cm 2 The density of the positive electrode was 2.45 g / cm by roller pressing. 3 The positive electrode sheet was cut into 30 mm×40 mm squares and dried at 140° C. to prepare a positive electrode.

[0456] The negative electrode and the positive electrode were separated by a separator impregnated with an electrolyte, and the separator was overlapped and sealed in an aluminum laminate bag to prepare a battery for charge and discharge test. As for the electrolyte, 2% by mass of vinylene carbonate was added to a mixed solution of ethylene carbonate: ethyl methyl carbonate = 30:70 (volume ratio), and LiPF6 was dissolved to 1 mol / L, and the obtained substance was used as the electrolyte.

[0457] <Evaluation of initial efficiency>

[0458] The battery was first charged to 4.1V at 0.2C, then charged to 0.1mA at 4.1V, and then discharged to 3.0V at 0.2C. Next, the battery was charged to 4.2V at 0.2C, then charged to 0.1mA at 4.2V, and then discharged to 3.0V at 0.2C. The 4.2V charge and 0.2C discharge were repeated once more as initial adjustment. The ratio of the initial 0.2C discharge capacity to the 4.1V charge capacity was defined as the initial efficiency.

[0459] <Evaluation of rapid discharge performance>

[0460] The initially conditioned battery was charged at 0.2C to 4.2V, then charged at 4.2V for 2 hours, and then discharged at 0.2C and 3C to 3.0V. The ratio of the 3C discharge capacity to the 0.2C discharge capacity was defined as the 3C / 0.2C discharge rate.

[0461] <Evaluation of Remaining Capacity Maintenance Rate>

[0462] The battery after the initial conditioning was stored at 60°C for 4 weeks while charged to 80% of the charge capacity, and then discharged at 25°C at 0.2C until 3.0 V. The ratio of the 0.2C discharge capacity after storage at 60°C for 4 weeks to the 0.2C discharge capacity at the end of the initial conditioning was taken as the residual capacity maintenance rate.

[0463] [Table 2]

[0464]

[0465] According to Table 2, the hardness of Comparative Example 1 containing only carbon material (A) is high, making it difficult to pressurize the negative electrode plate, and the initial efficiency, rate characteristics, and residual capacity retention rate after high-temperature storage are poor. The liquid immersion property of Comparative Example 2 containing carbon material (A) and carbon material (b) not coated with an organic compound is reduced, and the initial efficiency, rate characteristics, and residual capacity retention rate after high-temperature storage are poor. The liquid immersion property of Comparative Examples 3 to 4 containing only carbon material (B) is reduced, and the initial efficiency and residual capacity retention rate after high-temperature storage are poor.

[0466] Examples 1 to 3 using the carbon material composition of the present invention can achieve a balance between the pressing compactness and liquid immersion properties of the electrode plate, and no fracture surface of the active graphite produced when the carbon material is crushed is observed, thereby suppressing side reactions with the electrolyte, and the initial efficiency, rate characteristics, and residual capacity maintenance rate after high-temperature storage are all excellent.

[0467] Although the present invention has been described in detail using specific embodiments, it will be apparent to one skilled in the art that various modifications can be made without departing from the spirit and scope of the present invention.

[0468] This application is based on Japanese patent application No. 2022-058822 filed on March 31, 2022, and the entire contents of this patent are incorporated herein by reference.

Claims

1. A carbon material composition comprising a carbon material (A) and a carbon material (B), The carbon material (A) has a cumulative pore volume within a range of pore diameters of 0.01 μm or more and 1 μm or less of 0.02 mL / g or more, and a ratio of the pore diameter to the volume-based average particle diameter (PD / d50(%)) represented by the following formula (1) is 1.8 or less, The carbon material (B) is an organic compound-coated carbon material. Formula (1): PD / d50(%)=([mode pore diameter (PD) in the range of pore diameter of 0.01 μm or more and 1 μm or less in pore distribution determined by mercury porosimetry] / [volume-based average particle diameter (d50)])×100.

2. The carbon material composition according to claim 1, wherein The circularity of the carbon material (A) determined by flow particle image analysis is 0.88 or more.

3. The carbon material composition according to claim 1 or 2, wherein The carbon material (A) is derived from natural graphite.

4. The carbon material composition according to any one of claims 1 to 3, wherein The carbon material (A) is a composite carbon material of spheroidized graphite and a carbonaceous material.

5. The carbon material composition according to any one of claims 1 to 4, wherein The carbon material (B) is derived from natural graphite.

6. The carbon material composition according to any one of claims 1 to 5, wherein The organic compound covers the basal surface of the carbon material (B).

7. The carbon material composition according to any one of claims 1 to 6, wherein The organic compound is a compound derived from a polyvinyl alcohol resin.

8. The carbon material composition according to any one of claims 1 to 7, wherein In 100% by mass of the total of the carbon material (A) and the carbon material (B), 20% by mass to 80% by mass of the carbon material (A) and 20% by mass to 80% by mass of the carbon material (B) are contained.

9. The carbon material composition according to any one of claims 1 to 8, wherein The mass reduction rate from 200° C. to 700° C. measured by TG-DTA was 0.04 mass % to 0.48 mass %.

10. A method for producing a carbon material composition, comprising the step of mixing a carbon material (A) and a carbon material (B), The cumulative pore volume of the carbon material (A) within the range of pore diameter of 0.01 μm or more and 1 μm or less is 0.02 mL / g or more, and the ratio of the pore diameter to the volume-based average particle diameter (PD / d50(%)) represented by the following formula (1) is 1.8 or less, The carbon material (B) is an organic compound-coated carbon material; Formula (1): PD / d50(%)=([mode pore diameter (PD) in the range of pore diameter of 0.01 μm or more and 1 μm or less in pore distribution determined by mercury porosimetry] / [volume-based average particle diameter (d50)])×100.

11. A negative electrode comprising a current collector and an active material layer formed on the current collector, The active material layer comprises the carbon material composition according to any one of claims 1 to 9. 12 . A secondary battery comprising a positive electrode, a negative electrode and an electrolyte, wherein the negative electrode is the negative electrode according to claim 11 .