Cathode current collector for lithium-sulfur battery using metal lithium as anode and anode current collector for lithium battery or other lithium ion battery
By using magnesium lithium alloy strips or mesh strips as current collectors, combined with the coating of cathode active substances and the adhesion of metal lithium, the problems of breakage and uneven deposition of metal lithium foils in lithium sulfur batteries and lithium metal batteries are solved, and the problem of metal lithium foils is achieved. It improves battery performance and life, and is suitable for industrial applications of high-energy-density batteries.
Patent Information
- Application Number
- CN202410951921.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-22
AI Technical Summary
Due to the lack of current collector support, existing lithium sulfur batteries and lithium metal batteries cause metal lithium foils to break during the charge and discharge cycle and uneven deposition of lithium metal, resulting in short circuits, circuit breakers and cycle life, and the cost of traditional current collector materials is high. , the process is complex and difficult to industrialize.
Using magnesium lithium alloy strips or mesh strips as current collectors, the lithium content in magnesium lithium alloy is in the range of 3-20 wt%, combined with the coating of cathode active substances such as sulfur or sulfides, and metals are attached by mechanical or electrodeposition methods. Lithium forms a three-dimensional current collector structure to improve electrode reaction efficiency and stability.
Improves the energy density and cycle life of the battery, extends the battery life, reduces the weight of the battery, reduces the risk of breaking metal lithium foil, improves the low-temperature performance and rate performance of the battery, reduces the manufacturing cost and process complexity, and is suitable for large-scale Made in scale.
Smart Images

Figure CN119008964A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium-sulfur batteries or lithium metal batteries, and in particular to a cathode current collector for a lithium-sulfur battery using metallic lithium as an anode and an anode current collector for a lithium battery or other lithium-ion batteries. Background Art
[0002] At present, lithium-sulfur batteries and lithium metal batteries have great application potential in terms of high energy density and long cycle life. However, up to now, the negative electrode (anode) of the above two types of batteries uses a single metal lithium foil. This design has significant defects in the battery charge and discharge cycle. Due to the lack of a current collector as a support and conductive network for the metal lithium foil, the metal lithium foil is prone to fracture and uneven deposition of lithium metal in the early stage of the battery charge and discharge cycle, resulting in short circuit and open circuit failure of the pole piece in the battery, which seriously limits the cycle life of the battery. In addition, the positive electrode (cathode) material is also prone to capacity decay and decreased stability due to the depletion of the lithium source during the cycle.
[0003] In chemical batteries, especially lithium-sulfur batteries or lithium metal batteries, currently, lithium foil is directly used as the negative electrode (anode). Without a current collector to carry the lithium metal, the lithium foil will break in the early cycle, causing the negative electrode (anode) and battery failure.
[0004] Therefore, the Chinese invention patent authorization announcement number CN110828829B points out the importance and solution of 3D current collector, but the current collector material used is a metal material with a relatively heavy unit mass, which is contrary to the prospect of improving the specific energy of the battery. At the same time, it needs to deposit or electroplate precious metals such as gold and silver on the current collector, which is complex and costly. It is not conducive to large-scale manufacturing and industrial application.
[0005] China's invention patent authorization announcement number CN103794800B uses foamed metal as a carrier of metallic lithium. Under current technology, although the preparation uniformity of some metal foam materials has been greatly improved, their consistency is still far from that of mechanical manufacturing methods. The manufacturing process of batteries often ensures their consistency by weight input and monitoring of each component material. Therefore, the difference in the consistency of the above materials has a great impact on the consistency of the single battery, which will ultimately affect the cycle life of the battery. At the same time, the processing cost of foamed metal is also relatively high.
[0006] The core of the Chinese invention patent authorization announcement number CN110061191B is: the current collector is a three-dimensional copper foam as the skeleton, and the metal lithium is dispersed in the gaps of the three-dimensional copper foam; wherein, metal nanomaterials grow on the surface of the three-dimensional copper foam to form a lithium-philic surface; the three-dimensional copper foam forms an alloy with lithium through the metal nanomaterials. The same problems as the above patents, 1: consistency; 2: heavy metals do not meet the requirements of lightweight; 3: the surface of the metal copper needs to be complicatedly processed to make the metal lithium compatible with it. The process is complicated, the cost is high, and it is difficult to industrialize.
[0007] China Invention Patent Authorization Announcement No. CN109713224B This patent also uses foam metal as the current collector and has the same problems as above.
[0008] In addition, using metal foam as the negative electrode (anode) current collector and depositing lithium metal in the foam can theoretically prevent the battery from failing due to the problem of negative electrode (anode) metal lithium, but due to the uniformity and consistency of foam preparation, the weight of metal lithium deposited in a certain area or volume will vary. The battery manufacturing process is often invested and proportioned by the weight of each link and component, so the difference will seriously affect the consistency of the chemical battery reaction, and ultimately lead to early battery failure.
[0009] Inconsistency and unevenness may lead to the following problems:
[0010] 1. Inconsistent battery performance: Uneven lithium metal deposition may lead to performance differences between batteries, and even batteries in the same batch may not perform consistently.
[0011] 2. Difficult quality control: The various components in the battery manufacturing process usually require precise material weight control and ratio to ensure the stability and consistency of the battery. The weight differences introduced by foamed metals may pose challenges to these controls, thereby affecting the overall quality and life of the battery.
[0012] 3. The processing cost of materials such as copper foam and nickel foam is high, and their compatibility with metallic lithium is not good. Surface chemical treatment is required to make the metallic lithium deposition meet the requirements as much as possible, which makes the processing process complicated and costly. In addition, in the design of high-energy-density batteries, the lighter the current collector, the better, and lightweight metals are needed. Summary of the invention
[0013] One of the technical problems to be solved by the present invention is to provide a cathode current collector for lithium-sulfur batteries or lithium metal batteries with low manufacturing cost and easy industrialization in response to the above-mentioned technical problems existing in the existing lithium-sulfur batteries or lithium metal batteries using metallic lithium as the anode (negative electrode) current collector.
[0014] The second technical problem to be solved by the present invention is to provide an anode current collector for lithium-sulfur batteries or lithium metal batteries or other types of lithium-ion batteries with low manufacturing cost and easy industrialization in response to the above-mentioned technical problems existing in the current collectors of the above-mentioned existing lithium-sulfur batteries or lithium metal batteries.
[0015] The cathode current collector for a lithium-sulfur battery as the first aspect of the present invention comprises a magnesium-lithium alloy strip or mesh strip and a cathode active material attached to the magnesium-lithium alloy strip or mesh strip.
[0016] The anode current collector for lithium battery or other lithium ion battery as the second aspect of the present invention comprises a magnesium-lithium alloy strip or mesh and metal lithium attached to the magnesium-lithium alloy strip or mesh.
[0017] In a preferred embodiment of the present invention, the lithium content in the magnesium-lithium alloy strip or mesh is between 3-20wt%.
[0018] In a preferred embodiment of the present invention, the lithium content in the magnesium-lithium alloy strip or mesh is between 5-15wt%.
[0019] In a preferred embodiment of the present invention, the cathode active material is sulfur or sulfide.
[0020] In a preferred embodiment of the present invention, the magnesium-lithium alloy mesh belt is a stretched mesh (or expanded mesh).
[0021] In a preferred embodiment of the present invention, the metallic lithium is formed by mechanically attaching metallic lithium foil to the magnesium-lithium alloy strip or mesh belt.
[0022] In a preferred embodiment of the present invention, the metallic lithium is attached to the magnesium-lithium alloy strip or mesh strip by pressing a metallic lithium foil.
[0023] In a preferred embodiment of the present invention, the metallic lithium is attached to the magnesium-lithium alloy strip or mesh strip by electrodeposition.
[0024] In a preferred embodiment of the present invention, the cathode active material is uniformly attached to the magnesium-lithium alloy strip or mesh belt by wet or dry coating.
[0025] In a preferred embodiment of the present invention, the magnesium-lithium alloy strip or mesh strip is made by a rolling process.
[0026] Due to the adoption of the above technical solution, the present invention has the following advantages:
[0027] 1. Use magnesium-lithium alloy strips or mesh belts as current collectors to carry metallic lithium and cathode active materials. Use wet or dry electrode coating mode. The active material coated per unit area is much higher than the traditional transfer coating mode of pole piece processing mode. Because this method increases the specific surface area of the electrode, the electrode reaction efficiency is improved, and the energy density of the battery is greatly improved.
[0028] 2. As the negative electrode (anode) current collector, it can ensure the stability of the current conduction of the negative electrode (anode) and the surface area of the lithium metal attachment during the entire battery life, thereby greatly extending the battery life. At the same time, the three-dimensional current collector structure also increases the specific surface area of the anode. In the chemical battery system, it can greatly increase the chemical reaction rate, resulting in good low-temperature performance and rate characteristics, which can reduce the stress and damage of the metal lithium foil attached to its surface during the cycle process, and extend the battery cycle life.
[0029] 3. Magnesium is one of the lightest metals, and the addition of lithium to form a magnesium-lithium combination can improve the ductility of the material, making it easier to process the rolled foil and the stretched mesh. Pure magnesium is not suitable for this application due to its insufficient ductility.
[0030] 4. The present invention prepares the magnesium-lithium alloy by an alloy smelting method, and processes it into a magnesium-lithium alloy strip or mesh belt in the shape of a current collector, which can ensure that the magnesium-lithium alloy has good ductility and mechanical strength.
[0031] 5. Use the lithium source (lithium supplement) in the magnesium-lithium alloy to improve the stability of the positive electrode (cathode) material, thereby greatly extending the cycle life of the battery.
[0032] 6. Use high-purity lithium metal foil and use mechanical pressing or electrodeposition to uniformly attach or deposit lithium metal on a magnesium-lithium alloy strip or mesh belt to increase the specific surface area of the negative electrode (anode).
[0033] 7. The positive electrode (cathode) active material (such as sulfur and sulfur compounds) is attached to the surface of the magnesium-lithium alloy strip or mesh belt by a coating method to ensure heavy-load coating and uniform distribution of the material.
[0034] 8. During the battery charging and discharging process, the lithium source in the magnesium-lithium alloy provides additional lithium ions (lithium supplement), improving the stability of the cathode material.
[0035] 9. Selecting a magnesium-lithium alloy with a lithium content in the range of 3-20wt% can slow down the dissolution rate of lithium to a certain extent while maintaining the mechanical strength of the magnesium-lithium alloy.
[0036] 10. The magnesium-lithium alloy current collector provides stable mechanical support to prevent the metal lithium foil from accidentally breaking due to the accidental metal lithium deposition area during the battery charge and discharge cycle, thereby greatly extending the battery cycle life. The magnesium-lithium alloy network in the cathode improves the stability of the cathode material by supplementing lithium ions.
[0037] 11. Due to the improved stability of the anode and cathode, the battery maintains better performance and higher energy density during charging and discharging.
[0038] 12. The specific surface area of the anode can be increased by rolling metal lithium foil and electrodeposition, which can improve the low temperature performance and rate performance of the battery.
[0039] 13. The use of magnesium-lithium alloy current collectors can reduce the potential safety hazards caused by the breakage of metal lithium foil and improve the safety of batteries. The improved stability of cathode materials also helps prevent overcharging and other adverse reactions.
[0040] 14. Reduce physical damage to lithium metal: The current collector can share the stress in the battery and reduce the risk of deformation and breakage of lithium metal during the charging and discharging process.
[0041] 15. Improve the cycle stability of the battery: By improving the anode design, the resistance change and performance degradation during the battery cycle can be reduced, and the battery cycle life can be extended.
[0042] 16. Improve safety: Reduce local hot spots and safety hazards of lithium metal during charging and improve battery safety performance.
[0043] 17. Magnesium-lithium alloy is a very light metal material, which is very suitable for use as a negative electrode (anode) current collector of the battery, helping to improve the energy density and overall weight efficiency of the battery.
[0044] 18. The magnesium-lithium alloy contains metallic lithium, which enables the subsequent metallic lithium electrodeposition or mechanical rolling process to better combine with the substrate, thereby improving the stability and cycle life of the anode.
[0045] 19. The three-dimensional mesh material constructed by magnesium-lithium alloy through mechanical stretching process can achieve high pore uniformity and consistency, which is crucial for weight control and performance stability in the battery manufacturing process.
[0046] 20. Processing magnesium-lithium alloy foil using conventional machining modes (such as stretching process) may be easier to achieve than methods such as foam metal, and can be optimized in terms of cost and technical complexity.
[0047] 21. The mechanical stretching mesh (expanded mesh) processing mode of magnesium-lithium alloy can effectively utilize magnesium-lithium alloy foil materials with almost no waste, which is very important for cost control and sustainability.
[0048] 22. The processing mode of mechanical stretching mesh (expanded mesh) for magnesium-lithium alloy is generally more economical than other high-cost processing methods such as punching or laser drilling, because it does not involve complex equipment or high-energy consumption process steps. The processing process of mechanical stretching mesh is relatively simple, easy to implement and control, and reduces technical risks and the influence of variables in the manufacturing process. This processing method can be easily expanded to large-scale production to meet the high-volume requirements in battery manufacturing. In terms of large-scale production, the processing flow of mechanical stretching mesh can be further improved through automation and process optimization to ensure the stability of product quality and production efficiency. This is a crucial factor in meeting market demand, reducing unit costs, and promoting the successful commercial application of new technologies. Mechanical stretching mesh as a processing mode can indeed effectively solve the problems of waste materials and high costs, especially in the application of lightweight metal materials such as magnesium-lithium alloys, it has significant advantages. This method not only helps to improve production efficiency, but also reduces manufacturing costs, laying the foundation for the commercialization and widespread application of new technologies.
[0049] The main significance of the present invention using magnesium-lithium alloy as the anode three-dimensional current collector is: 1. Providing an attachment surface area with excellent conductivity for the lithium source; 2. Maintaining the integrity of the current collector and the consistency of current distribution throughout the life of the battery; 3. Making the metallic lithium have a higher specific surface area than foil, increasing the chemical reaction rate, and greatly improving the low temperature performance and rate performance of the chemical battery.
[0050] The present invention uses magnesium-lithium alloy as the cathode or anode current collector of lithium-sulfur battery or lithium metal battery or other lithium-ion battery using metal lithium negative electrode, and increases the specific surface area of metal lithium by electrodeposition, which can significantly improve the cycle life and overall performance of the battery, solve the problem that the traditional metal lithium foil anode is easy to break during the cycle process, and improve the low temperature performance and rate performance of the battery. The magnesium-lithium alloy mesh in the cathode improves the stability of the cathode material by supplementing lithium ions, further extending the cycle life of the battery. This innovative method is expected to play an important role in the development and application of high energy density batteries. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 It is a schematic structural diagram of a magnesium-lithium alloy mesh belt (stretching mesh) of the present invention.
[0052] Figure 2 It is a schematic structural diagram of another magnesium-lithium alloy mesh belt (stretching mesh) of the present invention.
[0053] Figure 3 Schematic diagram of the structure of the cathode current collector of Example 1.
[0054] Figure 4 Schematic diagram of the structure of the cathode current collector of Example 2.
[0055] Figure 5 Schematic diagram of the structure of the anode current collector of Example 3.
[0056] Figure 6 Schematic diagram of the structure of the anode current collector of Example 4.
[0057] Figure 7 This is a schematic diagram of pressing a metallic lithium foil onto a magnesium-lithium alloy mesh belt (stretched mesh) in Example 5. DETAILED DESCRIPTION
[0058] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0059] Example 1
[0060] See also Figure 3 , a cathode current collector for a lithium-sulfur battery, comprising a magnesium-lithium alloy strip 1a and a positive electrode (cathode) active material 2a uniformly attached to the magnesium-lithium alloy strip 1a by coating. The positive electrode (cathode) active material is sulfur or sulfide, wherein the sulfur content is greater than 50%, such as a sulfur-carbon mixed material, a polymerized sulfur / carbon mixed material, a lithium sulfide / carbon mixed material. The active material coating can be a double-sided rolling coating mode. The lithium content in the magnesium-lithium alloy strip 1a is between 3-20wt%, preferably between 5-15wt%.
[0061] The magnesium-lithium alloy strips are made by rolling process and have a thickness of 0.02-0.09mm.
[0062] The process of coating the positive electrode (cathode) active material 2a onto the magnesium-lithium alloy strip 1a is a single-sided transfer coating mode.
[0063] Example 2
[0064] See also Figure 4 , a positive electrode (cathode) current collector for a lithium-sulfur battery, comprising a magnesium-lithium alloy mesh belt 1b and a positive electrode (cathode) active material 2b uniformly attached to the magnesium-lithium alloy mesh belt 1b by electrodeposition. The positive electrode (cathode) active material 2b is sulfur or sulfide, such as a sulfur / carbon / binder mixed material, a polymerized sulfur / carbon / binder mixed material, or a lithium sulfide / carbon / binder mixed material. The coating method can be a double-sided rolling coating mode. The lithium content in the magnesium-lithium alloy mesh belt 1b is between 3-20wt%, preferably between 5-15wt%.
[0065] The process of electrodepositing the positive electrode (cathode) active material 2a onto the magnesium-lithium alloy mesh belt 1b is to use the lithium-magnesium alloy mesh as the negative electrode and metallic lithium as the positive electrode, and to deposit metallic lithium on the lithium-magnesium alloy mesh belt through constant current charging in an organic solvent that can dissolve metallic lithium as an electrolyte. The deposition thickness and morphology can be controlled by adjusting the current density and process time.
[0066] Magnesium-lithium alloy mesh belt 1b is Figure 1 and Figure 2 The stretched mesh structure shown has a thickness of 0.02-0.09 mm and can also be made by a rolling process with a thickness of 0.02-0.09 mm, and the holes are round holes or special-shaped holes.
[0067] Example 3
[0068] See also Figure 5 , used for an anode current collector of a lithium battery or other lithium-ion battery, comprising a magnesium-lithium alloy strip 1c and metallic lithium 3a uniformly attached to the magnesium-lithium alloy strip 1c by electrodeposition, wherein the lithium content in the magnesium-lithium alloy strip 1c is between 3-20wt%, preferably between 5-15wt%.
[0069] The magnesium-lithium alloy strips are made by rolling process and have a thickness of 0.02-0.09mm.
[0070] Example 4
[0071] See also Figure 6 , used for the anode current collector of lithium batteries or other lithium-ion batteries, including a magnesium-lithium alloy mesh belt 1d and metallic lithium 3b uniformly attached to the magnesium-lithium alloy mesh belt 1d by electrodeposition, the lithium content in the magnesium-lithium alloy mesh belt 1d is between 3-20wt%, preferably between 5-15wt%.
[0072] Magnesium-lithium alloy mesh belt 1b is Figure 1 and Figure 2 The stretched mesh structure shown has a thickness of 0.02-0.09 mm and can also be made by a rolling process with a thickness of 0.02-0.09 mm, and the holes are round holes or special-shaped holes.
[0073] Example 5
[0074] See also Figure 7 , used for the anode current collector of lithium battery or other lithium ion battery, including magnesium-lithium alloy mesh belt 1e and metal lithium 3c attached to the magnesium-lithium alloy mesh belt 1d by pressing, the lithium content in the magnesium-lithium alloy mesh belt 1e is between 3-20wt%, preferably between 5-15wt%.
[0075] Magnesium-lithium alloy mesh belt 1b is Figure 1 and Figure 2The stretched mesh structure shown has a thickness of 0.02-0.09 mm and can also be made by a rolling process with a thickness of 0.02-0.09 mm, and the holes are round holes or special-shaped holes.
Claims
1. A cathode current collector for a lithium-sulfur battery, characterized in that: It comprises a magnesium-lithium alloy strip or mesh strip and a cathode active material attached to the magnesium-lithium alloy strip or mesh strip.
2. The cathode current collector for a lithium-sulfur battery according to claim 1, characterized in that: The lithium content in the magnesium-lithium alloy strip or mesh is between 3-20wt%.
3. The cathode current collector for a lithium-sulfur battery according to claim 1, characterized in that: The positive electrode cathode active material is sulfur or a sulfur compound, wherein the proportion of sulfur is greater than 50%.
4. The cathode current collector for a lithium-sulfur battery according to claim 1, characterized in that: The magnesium-lithium alloy mesh belt is a stretched mesh.
5. The cathode current collector for a lithium-sulfur battery according to claim 1, characterized in that: The magnesium-lithium alloy strip or mesh strip is made by a rolling process.
6. The cathode current collector for a lithium-sulfur battery according to claim 1, characterized in that: The cathode active material is uniformly attached to the magnesium-lithium alloy strip or mesh belt by wet transfer coating or dry extrusion coating.
7. Anode current collector for lithium battery or other lithium ion battery, characterized in that: The invention comprises a magnesium-lithium alloy strip or mesh strip and metal lithium attached to the magnesium-lithium alloy strip or mesh strip.
8. The anode current collector for a lithium battery or other lithium ion battery according to claim 7, characterized in that: The lithium content in the magnesium-lithium alloy strip or mesh is between 3-20wt%.
9. The anode current collector for a lithium battery or other lithium ion battery according to claim 7, characterized in that: The magnesium-lithium alloy mesh belt is a stretched mesh.
10. The anode current collector for lithium battery or other lithium ion battery according to claim 7, characterized in that: The magnesium-lithium alloy strip or mesh strip is made by a rolling process.
11. The anode current collector for lithium battery or other lithium ion battery according to claim 7, characterized in that: The lithium is attached to the magnesium-lithium alloy strip or mesh belt by mechanical means using metal lithium foil.
12. The anode current collector for lithium battery or other lithium ion battery according to claim 7, characterized in that: The lithium is attached to the magnesium-lithium alloy strip or mesh strip by pressing using metal lithium foil.
13. The anode current collector for lithium battery or other lithium ion battery according to claim 7, characterized in that: The lithium is attached to the magnesium-lithium alloy strip or mesh belt by electrodeposition.
Citation Information
Patent Citations
Lithium-ion battery current collectors, electrodes, and lithium-ion batteries and their preparation methods, applications of lithium-ion batteries
CN103794800B
Composite lithium metal anode and its preparation method, lithium-ion battery
CN109713224B
A three-dimensional lithium metal anode, its preparation method and application
CN110061191B
A 3D lithium-loving porous metal current collector, anode, and their preparation and application
CN110828829B