Gas antibacterial microneedle for treating periodontitis and preparation method thereof

By combining enol polymers with Fe3(CO)12, the synergistic effect of photothermal and CO gas is used to solve the antibacterial activity and local treatment problems in periodontitis treatment, achieving efficient and safe teeth Treatment of periarthritis.

CN118873479APending Publication Date: 2024-11-01STOMATOLOGICAL HOSPITAL OF CHONGQING MEDICAL UNIV
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410911849.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing microneedles lack broad-spectrum antibacterial activity in the treatment of periodontitis, which easily triggers drug resistance, cannot achieve local treatment, is inconvenient to operate, and is less biocompatible and safe.

Method used

Microneedles that combine enol polymer with Fe3(CO)12 are used to achieve antibacterial effects through the synergistic effect of photothermal and CO gas, and local treatment is carried out through the precise penetration and controlled release functions of microneedles.

Benefits of technology

It significantly improves the antibacterial effect, reduces side effects, improves the accuracy and safety of treatment, and enhances the patient experience.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118873479A_ABST
    Figure CN118873479A_ABST
Patent Text Reader

Abstract

The invention relates to the field of periodontitis treatment, and discloses a gas antibacterial microneedle for treating periodontitis and a preparation method thereof.The preparation method specifically comprises the steps that an enol polymer is dissolved in DMSO under the high-temperature condition, a catalyst is added, 3, 4-dihydroxycinnamic acid is added after the temperature is lowered, dialysis, concentration and freeze-drying are conducted, and PCA-CA is obtained; the preparation method comprises the following steps: dissolving PCA-CA in dd water to obtain a PCA gel solution, adding Fe3 (CO) 12 powder into the PCA gel solution, and stirring to obtain a PCA-Fe3 (CO) 12 gel solution; and finally, putting the PCA / PCA-Fe3 (CO) 12 micro-needle into a micro-needle array mold, vacuumizing, concentrating and drying, and demolding until the micro-needle array mold is completely filled, so as to obtain the PCA / PCA-Fe3 (CO) 12 micro-needle. The problems that an existing microneedle does not have broad-spectrum antibacterial activity, drug resistance is likely to be caused, local treatment cannot be achieved, operation is inconvenient, and biocompatibility and safety are low are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of periodontitis treatment, and in particular to a gas antibacterial microneedle for treating periodontitis and a preparation method thereof. Background Art

[0002] Periodontitis is a common oral disease, mainly caused by bacterial infection, which often leads to inflammation and destruction of periodontal tissues. Traditional treatments for periodontitis include oral cleaning, medication, and surgery, but these methods often have problems such as long treatment cycles, unstable effects, and poor patient experience. Therefore, it is particularly important to develop a new, efficient, and patient-friendly treatment for periodontitis.

[0003] In recent years, with the rapid development of nanotechnology and biomedical engineering, microneedles, as a new drug delivery and treatment method, have gradually shown their great potential in the treatment of oral diseases. Microneedles have tiny sizes and can easily penetrate the oral mucosa to achieve precise drug release and local treatment. More importantly, microneedles can integrate multiple functions, such as drug controlled release, photothermal therapy, and gas release, thereby achieving comprehensive treatment of oral diseases. Summary of the invention

[0004] The present invention aims to provide a gas antibacterial microneedle for treating periodontitis and a preparation method thereof, so as to solve the problems that the existing microneedles do not have broad-spectrum antibacterial activity, are prone to induce drug resistance, cannot achieve local treatment, are inconvenient to operate, and have low biocompatibility and safety.

[0005] In order to achieve the above object, the present invention provides the following method:

[0006] Specifically, it relates to a gas antibacterial microneedle for treating periodontitis and a preparation method thereof, which is characterized by:

[0007] S1: dissolving the enol polymer in DMSO at high temperature, then adding a catalyst, and after the temperature is lowered, adding 3,4-dihydroxycinnamic acid to react to obtain a PCA-CA solution;

[0008] S2: dialyzing the PCA-CA solution to remove excess monomers and toxic organic solvents, performing a concentration process using a suspension evaporator, and then freeze-drying the PCA-CA solution after the concentration process to obtain a dry and loose hydrogel PCA-CA;

[0009] S3: dissolving the dry and loose hydrogel PCA-CA in dd water to obtain a PCA gel solution, and then adding Fe3(CO) 12 Powder and stir to obtain PCA-Fe3(CO) 12 Gel solution;

[0010] S4: the PCA-Fe3(CO) 12 The gel solution was placed in a microneedle array mold, and vacuum was drawn using a vacuum drying oven. Then, the vacuumed PCA-Fe3(CO 12 The gel solution is concentrated and dried;

[0011] S5: Repeat step S3 multiple times until the microneedle array mold is completely filled and then demoulded to obtain PCA / PCA-Fe3(CO) 12 Microneedling.

[0012] In an optional embodiment, the vinyl polymer is polyvinyl alcohol.

[0013] In an optional embodiment, the high temperature condition is 90-110°C.

[0014] In an optional embodiment, the catalyst is NaHSO4·H2O.

[0015] Preferably, the step of obtaining the PCA-CA solution is: dissolving the polymer polyvinyl alcohol in DMSO at high temperature, then adding the catalyst NaHSO4·H2O, and adding 3,4-dihydroxycinnamic acid after the temperature drops to 80°C to react to obtain the PCA-CA solution.

[0016] In an optional embodiment, the polymer polyvinyl alcohol is dissolved in a non-protonic polar solvent DMSO under high temperature conditions, and then a catalyst NaHSO4·H2O is added, and after the temperature is reduced to 80°C, 3,4-dihydroxycinnamic acid is added to react to obtain a PCA-CA solution in a reaction environment of reacting for 12 hours under N2 protection.

[0017] Preferably, the step of dialyzing the PCA-CA solution to remove excess monomers and toxic organic solvents, and concentrating the solution by a suspension evaporator comprises: dialyzing the PCA-CA solution to remove excess monomers and toxic organic solvents, and then concentrating the solution by a suspension evaporator until the volume ratio of the PCA-CA solution before and after concentration is 5:1.

[0018] In an optional embodiment, the step of freeze-drying the PCA-CA solution after the concentration process to obtain a dry and loose hydrogel PVA-CA is as follows: freeze-dry the PCA-CA solution after the dialysis and concentration process using a freeze dryer for 2 days until the solution is in a relatively homogeneous white freeze-dried block to obtain a dry and loose hydrogel PVA-CA.

[0019] In an optional embodiment, the dry and loose hydrogel PCA-CA is dissolved in dd water to obtain a PCA gel solution, and then Fe3(CO) is added to the PCA gel solution. 12 Powder and stir to obtain PCA-Fe3(CO) 12 The step of preparing a gel solution comprises: dissolving the dry and loose hydrogel PCA-CA in dd water at 100 mg / ml to obtain a PCA gel solution, and then adding Fe3(CO) 12 The powder was stirred at room temperature for 2-4 hours until the powder was evenly distributed in the gel solution to obtain PCA-Fe3(CO) 12 Gel solution.

[0020] In an optional embodiment, the PCA-Fe3(CO) 12 The gel solution was placed in a microneedle array mold, and vacuum was drawn using a vacuum drying oven. Then, the vacuumed PCA-Fe3(CO 12 The step of drying and concentrating the gel solution comprises: 12 The gel solution was placed in a microneedle array mold, and after evacuating the mold in a vacuum oven for 5-8 minutes, the microneedle array mold was immediately returned to normal pressure, and then the vacuumed PCA-Fe3(CO) 12 The gel solution is concentrated and dried for 6-24 hours until it is solid and not liquid.

[0021] The present invention has the following beneficial effects: Compared with the prior art, the present invention has the synergistic effect of photothermal and CO to enhance the antibacterial effect: the microneedle can not only kill bacteria through the photothermal effect, but also produce CO gas to further inhibit the growth and reproduction of bacteria. This synergistic effect of photothermal and CO can significantly improve the antibacterial effect and has significant advantages in the treatment of oral diseases such as periodontitis; local treatment and reduced side effects: the microneedle can accurately apply the drug and photothermal effect to the lesion site in the oral cavity to achieve local treatment. Compared with systemic medication, this method can reduce the distribution and metabolism of the drug in the body, thereby reducing the occurrence of side effects; simple operation and good patient experience: the microneedle is small in size and can easily penetrate the oral mucosa to achieve painless or minimally invasive drug administration. At the same time, the use of microneedles is relatively simple, and patients can easily cooperate with the treatment to improve the overall treatment experience; excellent drug controlled release performance: the microneedle can accurately control the release rate and dosage of the drug and CO gas to ensure that an effective therapeutic concentration is maintained in the oral cavity. This controlled drug release performance makes the treatment more precise and efficient; High biocompatibility and safety: The materials used in the microneedles have good biocompatibility and safety, can exist stably in the body, and do not cause significant immune responses. This ensures the safety of the treatment process and the comfort of the patient. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following is a brief introduction to the drawings required for the specific embodiments or the description of the prior art. In all the drawings, similar elements or parts are generally identified by similar reference numerals. In the drawings, the elements or parts are not necessarily drawn according to the actual scale.

[0023] Figure 1 It is a photographic image of PCA MN and PCA@FeCO 3MN provided in the embodiments of the present invention.

[0024] Figure 2 These are scanning electron microscope (SEM) and energy dispersive spectrum analysis (EDS) images of PCA MN and PCA@FeCO 3MN provided in the embodiments of the present invention. The needle length is about 650 μm, the distance between the needle tips is about 700 μm, and the diameter of the bottom of the needle tip is about 290 μm.

[0025] Figure 3 It is the X-ray photoelectron spectrum (XPS) of PCA MN and PCA@FeCO 3MN provided by the examples of the present invention.

[0026] Figure 4 3 is a compression force-distance curve of the PCA@FeCO 3MN microneedle provided in an embodiment of the present invention.

[0027] Figure 5It is a near-infrared photothermal curve diagram of PCA@FeCO 3MN provided in an embodiment of the present invention.

[0028] Figure 6 This is a probe fluorescence spectrum of PCA@FeCO 3MN provided in an embodiment of the present invention.

[0029] Figure 7 This is a fluorescence staining effect diagram of Staphylococcus aureus COP-1 provided in an embodiment of the present invention.

[0030] Figure 8 It is a comparison chart of the antibacterial properties of various groups of microneedles provided in the embodiments of the present invention.

[0031] Fig. 9 Graph showing the anti-biofilm effect of PCA@FeCO 3MN provided in an embodiment of the present invention.

[0032] Fig.10 The PCA MN and PCA@FeCO 3MN provided by the examples of the present invention are photographs of the periodontitis in the maxillary first molar of a rat.

[0033] Fig.11 This is a Micro-CT image of PCA MN and PCA@FeCO 3MN provided by the examples of the present invention applied to the maxillary first molar of rats for 4 weeks. DETAILED DESCRIPTION

[0034] In order to make the technical personnel in the technical field better understand the scheme of the present invention, the technical scheme in the embodiment of the present invention will be clearly and completely described below in combination with the drawings in the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all the embodiments. Based on the embodiment of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] The terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish different objects rather than to describe a specific order. In addition, the terms "including" and "having" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, device, product or end including a series of steps or units is not limited to the listed steps or units, but may optionally include steps or units that are not listed, or may optionally include other steps or units inherent to these processes, methods, products or ends.

[0036] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present invention. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.

[0037] In recent years, with the rapid development of nanotechnology and biomedical engineering, microneedles, as a new drug delivery and treatment method, have gradually shown their great potential in the treatment of oral diseases. Microneedles have tiny sizes and can easily penetrate the oral mucosa to achieve precise drug release and local treatment. More importantly, microneedles can integrate multiple functions, such as drug controlled release, photothermal therapy, and gas release, thereby achieving comprehensive treatment of oral diseases.

[0038] The present invention aims to provide a gas antibacterial microneedle for treating periodontitis and a preparation method thereof, so as to solve the problems that the existing microneedles do not have broad-spectrum antibacterial activity, are prone to induce drug resistance, cannot achieve local treatment, are inconvenient to operate, and have low biocompatibility and safety.

[0039] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0040] This embodiment provides a gas antibacterial microneedle for treating periodontitis and a preparation method thereof, which is characterized by:

[0041] S1: The enol polymer is dissolved in DMSO at high temperature, and then a catalyst is added. After the temperature is lowered, 3,4-dihydroxycinnamic acid is added to react to obtain a PCA-CA solution.

[0042] In an optional embodiment, the vinyl polymer is polyvinyl alcohol.

[0043] In an optional embodiment, the high temperature condition is 90-110°C.

[0044] In an optional embodiment, the catalyst is NaHSO4·H2O.

[0045] Preferably, the step of obtaining the PCA-CA solution is: dissolving the polymer polyvinyl alcohol in DMSO at high temperature, then adding the catalyst NaHSO4·H2O, and adding 3,4-dihydroxycinnamic acid after the temperature drops to 80°C to react to obtain the PCA-CA solution.

[0046] In an optional embodiment, the polymer polyvinyl alcohol is dissolved in a non-protonic polar solvent DMSO under high temperature conditions, and then a catalyst NaHSO4·H2O is added, and after the temperature is reduced to 80°C, 3,4-dihydroxycinnamic acid is added to react to obtain a PCA-CA solution in a reaction environment of reacting for 12 hours under N2 protection.

[0047] S2: dialyzing the PCA-CA solution to remove excess monomers and toxic organic solvents, performing a concentration process using a suspension evaporator, and then freeze-drying the PCA-CA solution after the concentration process to obtain a dry and loose hydrogel PCA-CA.

[0048] Preferably, the step of dialyzing the PCA-CA solution to remove excess monomers and toxic organic solvents, and concentrating the solution by a suspension evaporator comprises: dialyzing the PCA-CA solution to remove excess monomers and toxic organic solvents, and then concentrating the solution by a suspension evaporator until the volume ratio of the PCA-CA solution before and after concentration is 5:1.

[0049] In an optional embodiment, the step of freeze-drying the PCA-CA solution after the concentration process to obtain a dry and loose hydrogel PVA-CA is as follows: freeze-dry the PCA-CA solution after the dialysis and concentration process using a freeze dryer for 2 days until the solution is in a relatively homogeneous white freeze-dried block to obtain a dry and loose hydrogel PVA-CA.

[0050] S3: dissolving the dry and loose hydrogel PCA-CA in dd water to obtain a PCA gel solution, and then adding Fe3(CO) 12 Powder and stir to obtain PCA-Fe3(CO) 12 Gel solution.

[0051] In an optional embodiment, the dry and loose hydrogel PCA-CA is dissolved in dd water to obtain a PCA gel solution, and then Fe3(CO) is added to the PCA gel solution. 12 Powder and stir to obtain PCA-Fe3(CO) 12 The step of preparing a gel solution comprises: dissolving the dry and loose hydrogel PCA-CA in dd water at 100 mg / ml to obtain a PCA gel solution, and then adding Fe3(CO) 12 The powder was stirred at room temperature for 2-4 hours until the powder was evenly distributed in the gel solution to obtain PCA-Fe3(CO) 12 Gel solution.

[0052] S4: the PCA-Fe3(CO) 12 The gel solution was placed in a microneedle array mold, and vacuum was drawn using a vacuum drying oven. Then, the vacuumed PCA-Fe3(CO 12 The gel solution was concentrated to dryness.

[0053] In an optional embodiment, the PCA-Fe3(CO) 12 The gel solution was placed in a microneedle array mold, and vacuum was drawn using a vacuum drying oven. Then, the vacuumed PCA-Fe3(CO 12 The step of drying and concentrating the gel solution comprises: 12 The gel solution was placed in a microneedle array mold, and after evacuating the mold in a vacuum oven for 5-8 minutes, the microneedle array mold was immediately returned to normal pressure, and then the vacuumed PCA-Fe3(CO) 12 The gel solution is concentrated and dried for 6-24 hours until it is solid and not liquid.

[0054] S5: Repeat step S3 multiple times until the microneedle array mold is completely filled and then demoulded to obtain PCA / PCA-Fe3(CO) 12 Microneedling.

[0055] like Figure 1 As shown, it can be seen that PCA MN is brown, PCA@FeCO 3MN microneedles are dark green, the single needle tip is conical, the array is arranged in an orderly manner, and the needle body and backing are in good morphology.

[0056] like Figure 2 As shown, the needle length is about 650 μm, the distance between the needle tips is about 700 μm, and the diameter of the bottom of the needle tip is about 290 μm, ensuring that the microneedle can penetrate the bacterial biofilm and the gingival epithelium.

[0057] like Figure 3 As shown, chemical analysis of PCA MN and PCA@FeCO 3MN by X-ray photoelectron spectroscopy (XPS) showed the existence of Fe-O bonds in the PCA@FeCO 3MN group, confirming that the two were combined.

[0058] like Figure 4 As shown in the figure, the compressive strength of PCA@FeCO 3MN was tested using a universal mechanical tester. From the compression force-distance curve of the microneedle, it can be seen that the maximum compression force that the microneedle can withstand is about 9.5N, which is much larger than the minimum breaking force of 0.05N / needle required to penetrate the stratum corneum.

[0059] like Figure 5As shown in Figure 3, the temperature change was recorded from 31°C to 47°C within 5 minutes of irradiation with a near-infrared laser (NIR) of 808 nm at a distance of 10 cm from the sample, confirming that PCA@FeCO 3MN has excellent photothermal performance.

[0060] like Figure 6 As shown, the microneedle was placed in 10 ml of 50°C dd water, and samples were taken at 1 minute, 5 minutes, and 10 minutes, respectively, and the CO fluorescent probe COP-1 was used to detect the generation of CO. The fluorescence spectrum showed a specific absorption peak at a wavelength of about 520 nm, confirming that Fe3(CO)12 was decomposed into CO after heating, and the fluorescence intensity increased with time.

[0061] like Figure 7 As shown, the treated bacteria were fluorescently stained with COP-1, and it was observed that the content of CO increased after treatment.

[0062] like Figure 8 As shown, Staphylococcus aureus ( Figure 8 A) and Escherichia coli ( Figure 8 B) As experimental bacteria. It can be seen that after 15 minutes of NIR irradiation, PCA@FeCO 3MN achieved almost 100% antibacterial effect on both Staphylococcus aureus and Escherichia coli, confirming the effectiveness of CO gas therapy in synergizing mild photothermal sterilization.

[0063] like Fig. 9 As shown in the figure, in order to further study the removal effect of PCA@FeCO 3MN on Staphylococcus aureus biofilm, we first cultured Staphylococcus aureus in a 24-well plate for 5 days to form a relatively thick biofilm. Then, PCA@FeCO 3MN was used to treat the formed biofilm and crystal violet staining was used to Fig. 9 A and live-dead staining Fig. 9 B. The biofilm status was characterized by two technical means and it was found that PCA@FeCO 3MN also had an excellent removal effect on Staphylococcus aureus biofilm.

[0064] like Fig.10 As shown in the figure, in order to further verify the therapeutic effect of PCA@FeCO 3MN on periodontitis, a periodontitis model was firstly established by silk thread ligation of the maxillary first molar of rats, and PCA MN and PCA@FeCO 3MN groups were set up. Intraoral photography of rats confirmed that microneedles of both materials could be applied to the gingival tissue.

[0065] like Fig.11 As shown in the figure, Micro-CT confirmed that the rat periodontitis model was successfully established as judged by the degree of alveolar bone recession, and after PCA@FeCO 3MN treatment, alveolar bone resorption was reduced and the degree of periodontitis was alleviated.

[0066] Example 1

[0067] First, 4.2 grams of polyvinyl alcohol (PVA) were weighed, and then, at 100°C, we completely dissolved the PVA in DMSO. Subsequently, we added 6 grams of sodium bisulfate hydrate as a catalyst and ensured that it was completely dissolved in the solution. After completing these steps, we lowered the temperature of the solution to 80°C. While maintaining this temperature, 3 g of caffeic acid was added, and nitrogen was filled into the flask for protection. The reaction was allowed to proceed at 80°C for 12 hours; after that, the resulting solution was dialyzed for three days. After the dialysis was completed, the dialysate was placed in a suspension evaporator to evaporate most of the water until the volume of the solution was reduced to about 40 ml. The 40 ml of liquid was placed in a freeze dryer and freeze-dried for two days to obtain a dry and loose hydrogel PVA-CA.

[0068] The dry and loose hydrogel PVA-CA was dissolved in dd water at a concentration of 100 mg / ml to obtain PCA gel solution. Then 1 mg of Fe3(CO) 12 Powder, stir at room temperature for 2-4h, stir until the powder is evenly distributed in the gel solution to obtain PCA-Fe3(CO) 12 Gel solution.

[0069] PCA-Fe3(CO) 12 0.5 ml of gel solution was dropped into the microneedle array mold, and vacuum was applied in a vacuum drying oven for 5-8 minutes, followed by concentration and drying at room temperature for 6-24 hours. Vacuuming and concentration and drying were repeated several times until the needles and substrate of the microneedles were completely filled and then demolded to obtain PCA / PCA-Fe3(CO) 12 Microneedle PCA MN / PCA@FeCO 1MN.

[0070] Example 2

[0071] First, 4.2 grams of polyvinyl alcohol (PVA) were weighed, and then, at 100°C, we completely dissolved the PVA in DMSO. Subsequently, we added 6 grams of sodium bisulfate hydrate as a catalyst and ensured that it was completely dissolved in the solution. After completing these steps, we lowered the temperature of the solution to 80°C. While maintaining this temperature, 3 g of caffeic acid was added, and nitrogen was filled into the flask for protection. The reaction was allowed to proceed at 80°C for 12 hours; after that, the resulting solution was dialyzed for three days. After the dialysis was completed, the dialysate was placed in a suspension evaporator to evaporate most of the water until the volume of the solution was reduced to about 40 ml. The 40 ml of liquid was placed in a freeze dryer and freeze-dried for two days to obtain a dry and loose hydrogel PVA-CA.

[0072] The dry and loose hydrogel PVA-CA was dissolved in dd water at a concentration of 100 mg / ml to obtain PCA gel solution. Then, 2 mg Fe3(CO) 12 Powder, stir at room temperature for 2-4h, stir until the powder is evenly distributed in the gel solution to obtain PCA-Fe3(CO) 12 Gel solution.

[0073] PCA-Fe3(CO) 12 0.5 ml of gel solution was dropped into the microneedle array mold, and vacuum was applied in a vacuum drying oven for 5-8 minutes, followed by concentration and drying at room temperature for 6-24 hours. Vacuuming and concentration and drying were repeated several times until the needles and substrate of the microneedles were completely filled and then demolded to obtain PCA / PCA-Fe3(CO) 12 Microneedle PCA MN / PCA@FeCO 2MN.

[0074] Example 3

[0075] First, 4.2 grams of polyvinyl alcohol (PVA) were weighed, and then, at 100°C, we completely dissolved the PVA in DMSO. Subsequently, we added 6 grams of sodium bisulfate hydrate as a catalyst and ensured that it was completely dissolved in the solution. After completing these steps, we lowered the temperature of the solution to 80°C. While maintaining this temperature, 3 g of caffeic acid was added, and nitrogen was filled into the flask for protection. The reaction was allowed to proceed at 80°C for 12 hours; after that, the resulting solution was dialyzed for three days. After the dialysis was completed, the dialysate was placed in a suspension evaporator to evaporate most of the water until the volume of the solution was reduced to about 40 ml. The 40 ml of liquid was placed in a freeze dryer and freeze-dried for two days to obtain a dry and loose hydrogel PVA-CA.

[0076] The dry and loose hydrogel PVA-CA was dissolved in dd water at a concentration of 100 mg / ml to obtain PCA gel solution. Then 4 mg Fe3(CO) 12 Powder, stir at room temperature for 2-4h, stir until the powder is evenly distributed in the gel solution to obtain PCA-Fe3(CO) 12 Gel solution.

[0077] PCA-Fe3(CO) 12 0.5 ml of gel solution was dropped into the microneedle array mold, and vacuum was applied in a vacuum drying oven for 5-8 minutes, followed by concentration and drying at room temperature for 6-24 hours. Vacuuming and concentration and drying were repeated several times until the needles and substrate of the microneedles were completely filled and then demolded to obtain PCA / PCA-Fe3(CO) 12 Microneedle PCA MN / PCA@FeCO 3MN.

[0078] The above is only an embodiment of the present invention, and the common knowledge such as the known specific technical solutions or characteristics in the solution is not described in detail here. It should be pointed out that for those skilled in the art, without departing from the solution of the present invention, several modifications and improvements can be made, which should also be regarded as the protection scope of the present invention, and these will not affect the effect of the present invention and the practicality of the patent. The scope of protection required by this application shall be based on the content of its claims, and the specific implementation methods and other records in the specification can be used to interpret the content of the claims.

Claims

1. A gas antibacterial microneedle for treating periodontitis and a preparation method thereof, characterized in that: The method comprises: S1: dissolving the enol polymer in DMSO at high temperature, then adding a catalyst, and after the temperature is lowered, adding 3,4-dihydroxycinnamic acid to react to obtain a PCA-CA solution; S2: dialyzing the PCA-CA solution to remove excess monomers and toxic organic solvents, performing a concentration process using a suspension evaporator, and then freeze-drying the PCA-CA solution after the concentration process to obtain a dry and loose hydrogel PCA-CA; S3: dissolving the dry and loose hydrogel PCA-CA in dd water to obtain a PCA gel solution, and then adding Fe3(CO) 12 Powder and stir to obtain PCA-Fe3(CO) 12 Gel solution; S4: the PCA-Fe3(CO) 12 The gel solution was placed in a microneedle array mold, and vacuum was drawn using a vacuum drying oven. Then, the vacuumed PCA-Fe3(CO 12 The gel solution is concentrated and dried; S5: Repeat step S4 multiple times until the microneedle array mold is completely filled and then demoulded to obtain PCA / PCA-Fe3(CO) 12 Microneedling.

2. A gas antibacterial microneedle for treating periodontitis and a preparation method thereof according to claim 1, characterized in that: The vinyl alcohol polymer is polyvinyl alcohol.

3. The gas antibacterial microneedle for treating periodontitis and the preparation method thereof according to claim 1, characterized in that: The high temperature condition is 90-110°C.

4. The gas antibacterial microneedle for treating periodontitis and the preparation method thereof according to claim 1, characterized in that: The catalyst is NaHSO4·H2O.

5. The gas antibacterial microneedle for treating periodontitis and the preparation method thereof according to claim 1, characterized in that: The polymer polyvinyl alcohol is dissolved in DMSO under high temperature conditions, and then a catalyst NaHSO4·H2O is added. After the temperature is lowered to 80°C, 3,4-dihydroxycinnamic acid is added to react to obtain a PCA-CA solution.

6. The gas antibacterial microneedle for treating periodontitis and the preparation method thereof according to claim 5, characterized in that: The polymer polyvinyl alcohol was dissolved in the non-protonic polar solvent DMSO under high temperature conditions, and then the catalyst NaHSO4·H2O was added. After the temperature was reduced to 80°C, 3,4-dihydroxycinnamic acid was added to react to obtain the PCA-CA solution in a reaction environment of 12 hours under N2 protection.

7. The gas antibacterial microneedle for treating periodontitis and the preparation method thereof according to claim 1, characterized in that: The step of dialyzing the PCA-CA solution to remove excess monomers and toxic organic solvents and concentrating the solution by a suspension evaporator comprises: The PCA-CA solution is dialyzed to remove excess monomers and toxic organic solvents, and then concentrated using a suspension evaporator until the volume ratio of the PCA-CA solution before and after concentration is 5:

1.

8. The gas antibacterial microneedle for treating periodontitis and the preparation method thereof according to claim 1, characterized in that: The step of freeze-drying the PCA-CA solution after the concentration process to obtain a dry loose hydrogel PVA-CA is: The PCA-CA solution after the dialysis and concentration process was freeze-dried using a freeze dryer for 2 days until the solution became a relatively homogeneous white freeze-dried block to obtain a dry and loose hydrogel PVA-CA.

9. The gas antibacterial microneedle for treating periodontitis and the preparation method thereof according to claim 1, characterized in that: The dry and loose hydrogel PCA-CA is dissolved in dd water to obtain a PCA gel solution, and then Fe3(CO) is added to the PCA gel solution. 12 Powder and stir to obtain PCA-Fe3(CO) 12 The steps of gelling the solution include: The dry and loose hydrogel PCA-CA is dissolved in dd water at 100 mg / ml to obtain a PCA gel solution, and then Fe3(CO)12 powder is added to the PCA gel solution and stirred at room temperature for 2-4 hours until the powder is evenly distributed in the gel solution to obtain a PCA-Fe3(CO)12 gel solution.

10. A gas antibacterial microneedle for treating periodontitis and a preparation method thereof according to claim 9, characterized in that: The PCA-Fe3(CO) 12 The gel solution was placed in a microneedle array mold, and vacuum was drawn using a vacuum drying oven. Then, the vacuumed PCA-Fe3(CO 12 The step of drying and concentrating the gel solution comprises: The PCA-Fe3(CO)12 gel solution is placed in a microneedle array mold, and after evacuating the mold in a vacuum drying oven for 5-8 minutes, the microneedle array mold is immediately returned to normal pressure. The vacuumed PCA-Fe3(CO)12 gel solution is concentrated and dried for 6-24 hours until it is solid and not liquid.

Citation Information

Cited By

  • Soluble microneedle drug delivery system with adhesive backing and preparation method of soluble microneedle drug delivery system

    CN119792791A

  • Hydrogel double-layer microneedle material as well as preparation method and application thereof

    CN122229750A

  • Hydrogel double-layer microneedle material and preparation method and application thereof

    CN122229750B