Alumina carrier containing wormlike crystal grains and preparation method thereof

By growing worm-like alumina grains on the micron-scale spherical cavity and outer surface of the alumina support, forming a suitable pore structure, the problem that traditional alumina support cannot meet the hydrotreatment needs of heavy oil is solved, and efficient catalysts are achieved Performance and simple preparation method.

CN118874401AActive Publication Date: 2024-11-01CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202310457472.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-11-01
Estimated Expiration
2043-04-26

AI Technical Summary

Technical Problem

Traditional small-pore alumina support cannot meet the demand for heavy oil hydrotreatment. In the prior art, the pore structure on the catalyst surface is not conducive to the diffusion of reactant molecules, and the rod-like structure has limited degree of adjustment of the pores.

Method used

By growing worm-like alumina grains in situ on the micron-scale spherical cavity and outer surface of the alumina carrier, a large number of large pores and mesoporous penetration channels are formed. The preparation method includes immersing in aqueous propylene oxide solution for sealing heat treatment, drying and calculating. , alumina carrier with high coverage and suitable pore distribution is formed.

Benefits of technology

The opening of the support surface and internal pores is achieved, and the molecular diffusion capacity of reactants is improved. It is suitable for macromolecular heterogeneous catalytic reactions, especially in the field of heavy residue hydrotreatment. The method is simple and suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874401A_ABST
    Figure CN118874401A_ABST
Patent Text Reader

Abstract

The invention discloses an alumina carrier containing vermicular crystal grains and a preparation method thereof.The alumina carrier containing the vermicular crystal grains comprises micron-sized spherical cavities growing on the alumina carrier in situ and vermicular alumina crystal grains on the outer surface, the filling rate of the micron-sized spherical cavities is 20%-50%, and the filling rate of the vermicular alumina crystal grains is 20%-50%. And the coverage rate of the outer surface of the alumina carrier is 90-100%. The preparation method comprises the following steps: immersing the alumina carrier containing the micron-sized spherical cavity into an epoxy propane aqueous solution, carrying out sealed heat treatment at 60-100 DEG C for 1-4 hours, then carrying out sealed heat treatment at 110-180 DEG C for 2-6 hours, carrying out solid-liquid separation on the treated material, and drying and roasting the solid-phase material to obtain the alumina carrier containing the wormlike grains. Wormlike alumina crystal grains growing in situ on the outer surface of the alumina carrier and in micron-sized pore channels are stacked to form a large number of macroporous and mesoporous through pore channels, the alumina carrier can be used for preparing a heterogeneous catalytic reaction catalyst, and the preparation method is simple and suitable for industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of material synthesis, and in particular relates to an alumina carrier containing worm-like crystals and a preparation method thereof. Background Art

[0002] Activated alumina is a porous material with excellent physical and chemical properties. It is widely used as a catalyst or carrier. The pore structure of the alumina carrier not only affects the dispersion of the active components loaded, but is also closely related to the activity, selectivity, and life of the catalyst. As crude oil becomes increasingly heavy, traditional small-pore alumina can no longer meet production requirements, and the research and development and production of mesoporous and macroporous activated alumina are becoming increasingly important.

[0003] CN105983412A discloses a hydrogenation catalyst with high denitrification performance and a preparation method thereof, wherein silicon-containing pseudo-boehmite is first prepared, a phosphate is added to the silicon-containing pseudo-boehmite during the peptization process to obtain a carrier, and finally an active component is loaded to obtain a catalyst. Although the catalyst prepared by the method has a high pore volume, specific surface area, a certain 20-30 nm pore content and suitable acid properties, the pore structure on the catalyst surface is not conducive to the diffusion of reactant molecules.

[0004] CN109718860A discloses an alumina carrier and a preparation method thereof. The alumina carrier prepared by the method comprises a main alumina and a rod-shaped alumina, wherein at least part of the rod-shaped alumina is distributed on the outer surface of the main alumina carrier, and the rod-shaped alumina is 1-12µm long and 100-300nm in diameter. The preparation method of the alumina carrier comprises mixing the alumina carrier, ammonium bicarbonate and water, and then performing a sealed heat treatment, and drying and calcining the material after the heat treatment to obtain the alumina carrier. The method adjusts the pore structure of the carrier by growing a rod-shaped alumina on the surface of the alumina carrier, and the rod-shaped structure has a limited degree of adjustment for the pores. Summary of the invention

[0005] In view of the deficiencies in the prior art, the present invention provides an alumina carrier containing worm-like grains and a method for preparing the same. The worm-like alumina grains grown in situ on the outer surface and in the micron-sized pores of the alumina carrier are accumulated to form a large number of macropores and mesopores through the pores. The alumina carrier can be used to prepare catalysts for multiphase catalytic reactions. The preparation method is simple and suitable for industrial applications.

[0006] The alumina carrier containing worm-like crystals of the present invention comprises worm-like alumina crystals in-situ grown in micron-sized spherical cavities and on the outer surface of the alumina carrier.

[0007] In the alumina carrier of the present invention, the filling rate of the micron-sized spherical cavity is 20%-50%; wherein the filling rate refers to the percentage of the worm-like alumina grains in the volume of the micron-sized spherical cavity.

[0008] In the alumina carrier of the present invention, the coverage rate of the outer surface of the alumina carrier is 90%-100%, wherein the coverage rate refers to the percentage of the worm-like alumina grains to the outer surface area of ​​the alumina carrier.

[0009] In the alumina carrier of the present invention, the worm-like alumina grain size is 80nm-350nm; In the alumina carrier of the present invention, worm-like alumina crystals are accumulated in the micron-sized spherical cavities to form pores of 30-50 nm.

[0010] In the alumina carrier of the present invention, the worm-like alumina grains on the outer surface of the alumina carrier are accumulated to form pores of 30-100 nm.

[0011] In the alumina carrier of the present invention, the size of the micron-sized spherical cavity is preferably 1-3 μm.

[0012] The alumina carrier of the present invention further comprises spherical crystals constituting the alumina carrier, and the crystal size is 80-200 nm.

[0013] The specific surface area of ​​the alumina carrier of the present invention is 170-310m 2 / g, the pore volume is 0.8-1.0mL / g, and the pores of 8.5-20nm account for 50%-75% of the total pore volume.

[0014] The preparation method of the alumina carrier containing worm-like grains of the present invention comprises the following contents: immersing the alumina carrier containing micron-sized spherical cavities in an aqueous solution of propylene oxide, firstly sealing and heat treating it at 60-100°C for 1-4 hours, and then sealing and heat treating it at 110-180°C for 2-6 hours, separating the material from the solid and liquid after the treatment, and drying and calcining the solid phase material to obtain the alumina carrier containing worm-like grains.

[0015] In the method of the present invention, the alumina carrier containing micron-sized spherical cavities is prepared by the following method: pseudo-boehmite and micron-sized spherical activated carbon are mixed, deionized water is added to the mixed materials to form a slurry, and the slurry is subjected to liquid-solid separation and drying treatment. The dried material is kneaded, formed, dried, and calcined to obtain an alumina carrier containing micron-sized spherical cavities.

[0016] The pseudo-boehmite particles are generally granular and can be commercially available products or prepared by methods such as acid precipitation, alkali precipitation, alcohol aluminum hydrolysis, etc. Pseudo-boehmite with a pore size of 8.5-15 nm is preferred.

[0017] The diameter of the micron spherical activated carbon is 1-3 μm, and the micron spherical activated carbon can be prepared by existing methods or purchased.

[0018] The mass ratio of the activated carbon to the pseudo-boehmite is 1:19-1:32, and the amount of deionized water added is such that the liquid-solid mass ratio in the slurry is 5:1-10:1.

[0019] The kneading and molding are carried out by conventional methods in the art, and an extrusion aid and a peptizing agent are added as needed during molding. The extrusion aid is sesbania powder, and the amount added is 0.1wt%-0.5wt% of the weight of the final alumina carrier. The peptizing agent is one or more of hydrochloric acid, nitric acid, sulfuric acid, acetic acid, oxalic acid, etc., and the amount of the peptizing agent added is 0.1wt%-1.5wt% of the weight of the alumina carrier, which ultimately depends on the molding effect. The drying temperature is 100-160°C, and the drying time is 4-10 hours; the calcination temperature is 450-700°C, preferably 450-600°C, and the calcination time is 4-6 hours; the calcination is carried out in an oxygen-containing atmosphere.

[0020] In the method of the present invention, the mass percentage concentration of the propylene oxide aqueous solution is 2.5%-12%, preferably 4%-8%, and the mass ratio of the propylene oxide aqueous solution to the alumina carrier precursor is 3:1-10:1, preferably 4:1-8:1.

[0021] In the method of the present invention, the sealed heat treatment is preferably carried out in a closed autoclave, and the sealed heat treatment is preferably first carried out at 60-100° C. for 1-4 hours, and then at 120-160° C. for 2-6 hours.

[0022] In the method of the present invention, the drying temperature is 100-160° C., the drying time is 2-8 hours, the roasting temperature is 500-750° C., the roasting time is 4-6 hours, and the roasting is carried out in an oxygen-containing atmosphere, preferably in an air atmosphere.

[0023] The application of the alumina carrier of the present invention in macromolecular heterogeneous catalytic reactions is particularly suitable for the field of heavy residue oil hydroprocessing.

[0024] The present invention also provides a hydrogenation catalyst, which comprises the above-mentioned alumina carrier.

[0025] Compared with the prior art, the present invention has the following advantages: The surface and micron-sized cavities of the alumina carrier of the present invention have worm-like alumina grains grown in situ. The worm-like particles on the surface of the carrier are accumulated to form open channels of 30-100 nm that are conducive to the diffusion of reactant molecules. The worm-like alumina grains in the micron-sized spherical cavities are accumulated to form 30-50 nm channels, and the content of 8.5-20 nm channels inside the carrier is high. The pore distribution of the alumina carrier utilizes mass transfer of macromolecular materials and can be used to prepare catalysts for macromolecular heterogeneous catalytic reactions. The preparation method is simple and suitable for industrial applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] FIG. 1 is a SEM image of the surface of the alumina support prepared in Example 1.

[0027] Figure 2 This is a SEM image of the cross section of the alumina support prepared in Example 1.

[0028] FIG3 is a SEM image of the surface of the alumina support prepared in Comparative Example 2.

[0029] Figure 4 This is the SEM image of the cross section of the alumina support prepared in Comparative Example 2. DETAILED DESCRIPTION

[0030] The technical scheme and technical effect of the present invention are further described below in conjunction with the embodiments, but are not limited to the following embodiments. In the present invention, wt% represents mass fraction.

[0031] BET method: N2 physical adsorption-desorption was used to characterize the pore structure of the carriers of the embodiment and the comparative example. The specific operation was as follows: The pore structure of the sample was characterized by using an ASAP-2420 N2 physical adsorption-desorption instrument. A small amount of sample was vacuum treated at 300°C for 3-4 hours, and finally the product was placed under liquid nitrogen low temperature (-200°C) for nitrogen adsorption-desorption test. The specific surface area was obtained according to the BET equation, and the pore volume and the distribution rate of pore diameters below 30nm were obtained according to the BJH model.

[0032] Scanning electron microscopy was used to characterize the microstructure of the alumina carrier. The specific operation was as follows: a JSM-7500F scanning electron microscope was used to characterize the microstructure of the carrier, with an accelerating voltage of 5 KV, an accelerating current of 20 µA, and a working distance of 8 mm. Example 1

[0033] (1) Weigh 500 g of pseudo-boehmite (pore size 10 nm) and 24 g of micron-shaped spherical activated carbon with a diameter of 1-3 μm, mix them evenly, then add 3000 g of deionized water and stir for 2 hours. The mixture is filtered and dried at 140°C for 6 hours. Add 1.8 g of sesbania powder to the above dry materials and mix them evenly. Then add an appropriate amount of 0.5% acetic acid solution to the mixture and knead it evenly. Extrude into strips, dry the shaped materials at 145°C for 6 hours, and calcine at 500°C for 5 hours to obtain an alumina carrier precursor.

[0034] (2) Weigh 100 g of the alumina carrier precursor prepared in step (1), add 550 g of a 6.4% propylene oxide aqueous solution, transfer the mixture into an autoclave, seal the autoclave, place it in an oven and seal it at 85° C. for 2 hours, then heat it to 145° C. and seal it for 3.5 hours. After treatment, the material is cooled, washed, and filtered. The solid material is dried at 140° C. for 6 hours and calcined at 550° C. for 5 hours to obtain an alumina carrier S1. The scanning electron microscope image of the outer surface of the alumina carrier is shown in FIG. Figure 1 , cross-sectional SEM images are shown in Figure 2 , the carrier properties are shown in Table 1. Example 2

[0035] The same as Example 1, except that the amount of micron spherical activated carbon added in step (1) is 18 g. In step (2), the concentration of propylene oxide is 5.5%, the amount of solution used is 650 g, and the hydrothermal treatment is first performed at 75° C. for 2.5 hours and then at 135° C. for 4.5 hours to obtain an alumina carrier S2. The properties of the carrier are shown in Table 1. Example 3

[0036] The same as Example 1, except that the amount of micron spherical activated carbon added in step (1) is 16 g. In step (2), the concentration of propylene oxide is 7.7%, the amount of solution used is 450 g, and the hydrothermal treatment is first performed at 65° C. for 3 hours and then at 155° C. for 2.5 hours to obtain an alumina carrier S3. The properties of the carrier are shown in Table 1. Example 4

[0037] The same as Example 1, except that the amount of micron spherical activated carbon added in step (1) is 25 g. In step (2), the concentration of propylene oxide is 4.3%, the amount of solution used is 750 g, and the hydrothermal treatment is first performed at 95° C. for 1.5 hours and then at 125° C. for 5.5 hours to obtain an alumina carrier S4. The properties of the carrier are shown in Table 1.

[0038] Comparative Example 1 The same method as Example 1 was used, except that in step (2), the propylene oxide aqueous solution was replaced with an ammonia aqueous solution of the same mass concentration to obtain an alumina carrier S5. The properties of the carrier are shown in Table 1.

[0039] Comparative Example 2 The same as Example 1, except that in step (2), the propylene oxide aqueous solution is replaced with an ethylene oxide solution of the same concentration to obtain an alumina carrier S6. The scanning electron microscope image of the outer surface of the alumina carrier is shown in Figure 3 , cross-sectional SEM images are shown in Figure 4 , the carrier properties are shown in Table 1.

[0040] Comparative Example 3 The same method as Example 1, except that the concentration of propylene oxide in step (2) was 0.8%, to obtain an alumina carrier S7. The properties of the carrier are shown in Table 1.

[0041] Comparative Example 4 The same as Example 1, except that the hydrothermal treatment in step (2) is a one-step hydrothermal treatment, the treatment temperature is 85°C, the treatment time is 5.5 hours, and an alumina carrier S8 is obtained. The properties of the carrier are shown in Table 1.

[0042] Table 1 Alumina support properties Example 1 Example 2 Example 3 Example 4 Comparative Example 1 Comparative Example 2 Comparative Example 3 Comparative Example 4 catalyst S1 S2 S3 S4 S5 S6 S7 S8 <![CDATA[Specific surface area, m 2 / g]]> 225 236 218 247 203 192 213 218 Pore ​​volume, mL / g 0.92 0.93 0.95 0.91 0.81 0.83 0.85 0.86 8.5-20nm pore content, % 63.3 61.1 57.9 65.2 41.1 42.6 45.2 45.6 The coverage of worm-like alumina on the carrier surface, % 95 93 96 91 — — — 96 The pore size formed by the accumulation of worm-like alumina on the carrier surface, nm 30-90 40-95 35-95 35-90 10-90 10-95 15-90 10-90 Micron-sized spherical cavity worm-like alumina filling rate, % 33.5 29.5 35.5 31.5 — — — — Micron-sized spherical cavity worm-like alumina accumulation forms pore size, nm 30-45 30-40 30-50 35-45 — — — — From the data in Table 1 and Figure 1-4 It can be seen that compared with the alumina carrier, the alumina carrier prepared by the method of the present invention has open macropores on the surface and a high content of 8.5-20 nm pores inside the carrier.

Claims

1. An alumina carrier containing worm-like grains, characterized in that: The invention comprises micron-sized spherical cavities in-situ grown on an alumina carrier and worm-like alumina grains on the outer surface.

2. The alumina carrier according to claim 1, characterized in that: The filling rate of the micron-sized spherical cavity is 20%-50%, wherein the filling rate refers to the percentage of the worm-like aluminum oxide grains in the volume of the micron-sized spherical cavity.

3. The alumina carrier according to claim 1, characterized in that: The coverage rate of the outer surface of the alumina carrier is 90%-100%, wherein the coverage rate refers to the percentage of the worm-like alumina grains to the outer surface area of ​​the alumina carrier.

4. The alumina carrier according to claim 1, characterized in that: The worm-like aluminum oxide grain size is 80nm-350nm; The alumina carrier according to claim 1 is characterized in that the worm-like alumina grains in the micron-sized spherical cavities are accumulated to form pores of 30-50 nm.

5. The alumina carrier according to claim 1, characterized in that: The worm-like alumina grains on the outer surface of the alumina carrier are accumulated to form pores of 30-100 nm.

6. The alumina carrier according to claim 1, characterized in that: The size of the micron-sized spherical cavity is preferably 1-3 μm.

7. The alumina carrier according to claim 1, characterized in that: The alumina carrier also includes spherical crystallites constituting the alumina carrier, and the crystallites have a size of 80-200 nm.

8. The alumina carrier according to claim 1, characterized in that: The specific surface area of ​​alumina carrier is 170-310m 2 / g, the pore volume is 0.8-1.0mL / g, and the pores of 8.5-20nm account for 50%-75% of the total pore volume.

9. A method for preparing an alumina carrier containing worm-like grains according to any one of claims 1 to 9, characterized in that The method comprises the following contents: immersing an alumina carrier containing micron-sized spherical cavities into an aqueous solution of propylene oxide, firstly subjecting the carrier to sealed heat treatment at 60-100°C for 1-4 hours, and then subjecting the carrier to sealed heat treatment at 110-180°C for 2-6 hours, subjecting the treated material to solid-liquid separation, and subjecting the solid-phase material to drying and roasting to obtain an alumina carrier containing worm-like grains.

10. The method according to claim 10, characterized in that: The alumina carrier containing micron-sized spherical cavities is prepared by the following method: pseudo-boehmite and micron-sized spherical activated carbon are mixed, deionized water is added to the mixed materials to form a slurry, and the slurry is subjected to liquid-solid separation and drying treatment. The dried material is kneaded, formed, dried, and calcined to obtain an alumina carrier containing micron-sized spherical cavities.

11. The method according to claim 11, characterized in that: The pseudo-boehmite particles are in granular form, preferably pseudo-boehmite with a pore size of 8.5-15 nm.

12. The method according to claim 11, characterized in that: The diameter of the micron spherical activated carbon is 1-3 μm.

13. The method according to claim 11, characterized in that: The mass ratio of the activated carbon to the pseudo-boehmite is 1:19-1:32, and the amount of deionized water added is such that the liquid-solid mass ratio in the slurry is 5:1-10:

1.

14. The method according to claim 10, characterized in that: The mass percentage concentration of the propylene oxide aqueous solution is 2.5%-12%, preferably 4%-8%, and the mass ratio of the propylene oxide aqueous solution to the alumina carrier precursor is 3:1-10:1, preferably 4:1-8:

1.

15. The method according to claim 10, characterized in that: The sealed heat treatment is carried out in a closed autoclave; the sealed heat treatment is preferably first carried out at 60-100°C for 1-4 hours, and then at 120-160°C for 2-6 hours.

16. The method according to claim 11, characterized in that: The drying temperature is 100-160° C., and the drying time is 2-8 hours; the calcination temperature is 500-750° C., and the calcination time is 4-6 hours, and the calcination is carried out in an oxygen-containing atmosphere.

17. Use of the alumina carrier containing worm-like crystals according to any one of claims 1 to 9 in macromolecular heterogeneous catalytic reactions.

18. A hydrogenation catalyst, characterized in that: The catalyst comprises the alumina carrier containing worm-like crystals as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Composite carrier of exhaust gas cleaning catalyst and preparation method of carrier

    CN102962104A

  • Wormlike mesoporous Al2O3 / molecular sieve composite material and preparation method thereof

    CN107297220A

  • Carrier for hydrodenitrogenation, catalyst and preparation method thereof

    CN111821964A

  • Double-pore distribution alumina spherical particle and preparation method thereof

    CN114644352A

  • Porous alumina crystalline particle, and production method therefor

    JP2005015323A