Preparation method of super-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium

By introducing carbon nanotubes as self-assembly inducers to form ultra-large pore composite microspheres, the problem of insufficient mass transfer rate and adsorption site of cellulose microspheres is solved, and efficient protein isolation and purification is achieved. The material has excellent mechanical properties and recyclability.

CN118874441APending Publication Date: 2024-11-01SICHUAN UNIV +1

Patent Information

Application Number
CN202411019707.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing cellulose microspheres are limited by nanopore size in protein purification, resulting in low mass transfer rate and reduced adsorption sites. The mechanical strength of macroporous materials is insufficient, making it difficult to widely use and recover.

Method used

Carbon nanotubes are used as self-assembly inducing cellulose self-assembly through size matching and hydrophobic action to form ultra-large pores, high specific surface area cellulose-based composite microspheres, providing spacious mass transfer channels and rich active adsorption sites. High-strength composite microspheres were prepared by emulsification.

Benefits of technology

It has achieved the expansion of the macromolecular mass transfer channel, improved the adsorption capacity and mechanical properties, broadened the operating conditions and recyclable properties, and is suitable for the rapid and efficient separation and purification of proteins.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874441A_ABST
    Figure CN118874441A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a super-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium, and relates to the technical field of chromatographic medium materials. The preparation method comprises the following steps: (1) magnetically stirring sodium hydroxide, thiourea and deionized water; pouring a carbon nanotube and stirring to obtain a carbon nanotube / alkali urea dispersion liquid; (2) weighing microcrystalline cellulose, adding the dispersion liquid, stirring, and adding epichlorohydrin for pre-crosslinking to obtain a pre-crosslinked cellulose / carbon nanotube composite solution; and (3) adding the composite solution into an oil phase, emulsifying, dropwise adding an ethanol solution, stirring, standing, and sequentially centrifuging, cleaning, gradient soaking and freeze-drying to obtain the super-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium. According to the invention, the carbon nanotubes are used as an initiator for cellulose self-assembly to obtain microbeams, and the composite microbeams are self-wound to construct a super-macroporous, high-specific-surface and high-strength cellulose chromatographic medium, thereby opening up a new way for developing a high-efficiency separation medium for biomacromolecules.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chromatographic medium materials, and in particular to a method for preparing a super-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium. Background Art

[0002] Highly purified biomacromolecules such as proteins play an increasingly critical role in the fields of medicine, biopharmaceuticals, and emerging technologies and are urgently needed. In order to meet the growing demand, it is urgent to develop efficient, reliable, environmentally friendly and low-cost protein purification methods. In recent years, various methods have been used in this regard, including chromatography, extraction, precipitation, etc. Among these technologies, chromatography is considered to be the most suitable process for protein separation and purification due to its mild conditions and high resolution. Among them, the chromatographic medium is the core of chromatographic separation and largely determines the performance of chromatographic separation (such as capacity, efficiency, mass transfer and selectivity, etc.). Therefore, it is necessary to immediately develop chromatographic media with selective separation and high adsorption capacity for proteins.

[0003] Cellulose is the most widely distributed and most abundant natural macromolecule in nature. It has the advantages of being non-toxic, non-polluting, degradable, renewable, biocompatible, easy to modify, and stable in chemical properties. In particular, due to its high specific surface area, easy to modify and operate, cellulose microspheres have been widely used as chromatographic media for protein separation and purification. Unfortunately, cellulose microspheres are greatly limited by the nanopore size (10-200nm) in protein purification applications. The narrow pores not only limit the mass transfer rate of biomacromolecules, but also reduce the adsorbable sites due to the long diffusion path and large mass transfer resistance. In order to improve the above shortcomings, the introduction of macropores has attracted attention. In the macroporous channel, the mobile phase is transported to the interior of the particles by convection, resulting in higher column efficiency and promoting the industrialization of protein purification. Most researchers adopt the template method to prepare macroporous cellulose materials, and the removal of the template increases the difficulty and economic burden of the preparation. In addition, changing the emulsification method can also successfully prepare macroporous cellulose materials, but the mechanical strength will be reduced due to the large pores. More importantly, the poor mechanical strength easily leads to rupture or even collapse under stress and strain, which greatly limits its application in chromatography and recyclability. Therefore, it is a great challenge to prepare high-strength macroporous cellulose materials in a green and simple one-step method. Summary of the invention

[0004] In order to solve the above technical problems, the purpose of the present invention is to provide a method for preparing an ultra-large-pore cellulose / carbon nanotube composite microsphere chromatographic medium, wherein carbon nanotubes are used as initiators for cellulose self-assembly to obtain microbundles, and the composite microbundles are self-entangled to construct an ultra-large-pore, high-specific surface area, and high-strength cellulose-based chromatographic medium. The composite microsphere chromatographic medium provides a spacious mass transfer channel for macromolecules, abundant active adsorption sites, a wide range of operable conditions, and excellent recyclability, thus opening up a new path for the development of efficient separation media for biomacromolecules.

[0005] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing a super-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium is provided, comprising the following steps:

[0006] (1) magnetically stirring sodium hydroxide, thiourea and deionized water until the solid is completely dissolved to obtain an alkaline urea solution; then pouring the carbon nanotubes into the alkaline urea solution and magnetically stirring at the same time to obtain a carbon nanotube / alkaline urea dispersion;

[0007] (2) placing microcrystalline cellulose in a three-necked flask, then adding the carbon nanotube / alkaline urea dispersion obtained in step (1) under ice bath conditions and stirring until the solution is transparent, and then adding epichlorohydrin for pre-crosslinking to obtain a pre-crosslinked cellulose / carbon nanotube composite solution;

[0008] (3) adding the pre-crosslinked cellulose / carbon nanotube composite solution obtained in step (2) to the premixed oil phase, emulsifying under mechanical stirring, then dropping into an ethanol solution and stirring to solidify, allowing to stand for stratification, and then centrifuging, washing, gradient soaking and freeze-drying in sequence to obtain an ultra-large pore cellulose / carbon nanotube composite microsphere chromatographic medium.

[0009] Furthermore, in step (1), the mass volume ratio of sodium hydroxide, thiourea, carbon nanotubes and deionized water is 5g:4g:0.1-0.2g:50mL.

[0010] Furthermore, in step (1), carbon nanotubes are added and magnetically stirred at 300 rpm for 30 min.

[0011] Furthermore, in step (2), the mass volume ratio of microcrystalline cellulose, carbon nanotube / alkaline urea dispersion and epichlorohydrin is 3g:50mL:1.2-1.5mL.

[0012] Furthermore, in step (2), pre-crosslinking is performed for 30-40 seconds.

[0013] Furthermore, in step (3), the volume ratio of the pre-crosslinked cellulose / carbon nanotube composite solution to the ethanol solution is 10-12 mL:100 mL.

[0014] Furthermore, in step (3), the premixed oil phase is prepared by the following method: premixing Span-80, Tween-80, white oil and isooctane in a 25° C. water bath for 30 minutes to obtain the premixed oil phase.

[0015] Furthermore, the mass volume ratio of Span-80, Tween-80, white oil and isooctane is 5.5 g: 1 g: 40 mL: 80 mL.

[0016] Furthermore, in step (3), emulsification is performed under mechanical stirring at 250 rpm for 10-30 min.

[0017] Furthermore, in step (3), 50 vol% ethanol solution is slowly dripped in and stirred for solidification.

[0018] Further, in step (3), the oil-water layers are separated after standing, the aqueous phase is centrifuged at 4000 rpm for 2-4 min and the upper aqueous phase is discarded, and then the microspheres are washed with a 50 vol% ethanol solution under vigorous shaking and centrifugation, and the washing is repeated three times, and then washed with pure water at least three times, and then the microspheres are soaked in ethanol solutions with gradient concentrations of 20 vol%, 40 vol%, 60 vol%, 80 vol% and 100 vol%, each time for at least 10 min, and soaked in 100 vol% ethanol for at least three times, and finally soaked in a tert-butyl alcohol solution for gradient soaking and freeze-dried.

[0019] Furthermore, the replacement of the tert-butyl alcohol ethanol solution was carried out in a 30° C. water bath with shaking.

[0020] The present invention also provides a super-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium prepared by the preparation method of the super-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium.

[0021] The present invention has the following beneficial effects:

[0022] 1. The present invention uses carbon nanotubes as self-assembly inducers, and utilizes size matching and hydrophobic effects to induce cellulose to self-assemble into microbundles, and then the microbundles are self-entangled to construct ultra-large pores, high specific surface area, and high-strength cellulose-based chromatographic media, which have micron-level macropores, abundant micro-mesopores, and excellent mechanical properties. The composite microsphere chromatographic media provides spacious mass transfer channels for macromolecules, abundant active adsorption sites, wide operating conditions, and excellent recyclability, opening up a new path for the development of efficient separation media for biomacromolecules.

[0023] 2. The ultra-large-pore cellulose / carbon nanotube composite microsphere chromatographic medium prepared by the present invention has micron-sized macropores, which can provide a more spacious mass transfer channel and effectively reduce the mass transfer resistance in the chromatographic separation process; it has abundant micro-mesopores, provides a large number of active adsorption sites and improves the adsorption capacity; it has excellent permeability, which provides strong support for the rapid and efficient separation of proteins; it has outstanding mechanical strength, broadens the operable flow rate range in the separation process and enhances the reusability. The ultra-large-pore, high-strength cellulose / carbon nanotube composite microsphere chromatographic medium prepared by the present invention has superior mass transfer performance, high adsorption capacity, good permeability, wide operable conditions, good recycling performance, and is suitable for the rapid separation and efficient purification of biomacromolecules. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The scanning electron microscope results of the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium obtained in Example 1; Figure A is pure cellulose microspheres, and Figure B is the composite microsphere chromatographic medium obtained in Example 1;

[0025] Figure 2 The nitrogen adsorption / desorption curve results of the ultra-large porous cellulose / carbon nanotube composite microsphere chromatographic medium obtained in Example 1; Figure A is the nitrogen adsorption / desorption curve, and Figure B is the pore size distribution;

[0026] Figure 3 The mechanical properties test results of the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium obtained in Example 1; Figure A is the centrifugal stability result, and Figure B is the pressure flow rate curve;

[0027] Figure 4 These are the separation performance test results of the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium obtained in Example 1; Figure A is the adsorption thermodynamics result, Figure B is the adsorption kinetics result, and Figure C is the dynamic adsorption result. DETAILED DESCRIPTION

[0028] The principles and features of the present invention are described below, and the examples are only used to explain the present invention and are not used to limit the scope of the present invention. If no specific conditions are specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments is not specified, they are all conventional products that can be purchased commercially.

[0029] Embodiment 1:

[0030] A super-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium, the preparation method of which comprises the following steps:

[0031] (1) 10.2 g of sodium hydroxide, 8 g of thiourea and 100 mL of deionized water were magnetically stirred until the solid was completely dissolved to obtain an alkaline urea solution; then 0.31 g of carbon nanotubes were poured into the alkaline urea solution and magnetically stirred at 300 rpm for 30 min to obtain a carbon nanotube / alkaline urea dispersion;

[0032] (2) 6 g of microcrystalline cellulose was placed in a three-necked flask, and then 100 mL of the carbon nanotube / alkaline urea dispersion obtained in step (1) was added under ice bath conditions and vigorously stirred for 2 min until the solution was transparent, and then 2.6 mL of epichlorohydrin was added for pre-crosslinking for 36 s to obtain a pre-crosslinked cellulose / carbon nanotube composite solution;

[0033] (3) 21.5 mL of the pre-crosslinked cellulose / carbon nanotube composite solution obtained in step (2) was added to the premixed oil phase (80 mL of white oil, 160 mL of isooctane, 11 g of Span-80, and 2 g of Tween-80), and emulsified for 30 min under mechanical stirring at 250 rpm, and then 200 mL of 50 vol% ethanol solution was slowly dropped and stirred to solidify. After standing, the oil and water layers were separated, and the aqueous phase was centrifuged at 4000 rpm for 3 min and the upper aqueous phase was poured out. Subsequently, the microspheres were washed with 50 vol% ethanol solution under vigorous shaking and centrifugation, and the washing was repeated three times. Then, the microspheres were washed with pure water three times, and then the microspheres were soaked with ethanol solutions of gradient concentrations of 20 vol%, 40 vol%, 60 vol%, 80 vol% and 100 vol%, each time for at least 10 min, and the 100 vol% ethanol soaking was performed at least three times. Finally, tert-butyl alcohol ethanol solution was used for gradient soaking, and freeze-dried to obtain ultra-large porous cellulose / carbon nanotube composite microsphere chromatographic medium.

[0034] The scanning electron microscope, nitrogen adsorption / desorption curve, and mechanical property test results of the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium obtained in Example 1 are obtained as follows: Figure 1-3 As shown. Among them, Figure 2 In the figure, cellulose / carbon nanotube-0.2 indicates a composite microsphere chromatography medium compounded with 0.2 g of carbon nanotubes.

[0035] Depend on Figure 1 It can be seen that the scanning electron microscopy image shows that after doping with carbon nanotubes, a macroporous structure appears on the surface of the microspheres, which is beneficial to the improvement of mass transfer efficiency. In the subsequent adsorption performance test, the mass transfer channel is widened to facilitate the transport of proteins, thereby improving the separation performance.

[0036] Depend on Figure 2 It can be seen that the cellulose / carbon nanotube composite microspheres have rich micro-mesoporous structures and large specific surface area, which provide abundant adsorption sites and lay the foundation for higher adsorption capacity.

[0037] Depend on Figure 3It can be seen that with the increase of carbon nanotube content, the centrifugal stability of the microspheres is improved, the back pressure is low, the permeability is better, and in the application of chromatographic separation, the microspheres have good stability, a wide range of operable flow rates, and a considerable recovery rate.

[0038] Embodiment 2:

[0039] A super-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium, the preparation method of which comprises the following steps:

[0040] (1) 5 g of sodium hydroxide, 4 g of thiourea and 50 mL of deionized water were magnetically stirred until the solid was completely dissolved to obtain an alkaline urea solution; then 0.2 g of carbon nanotubes were poured into the alkaline urea solution and magnetically stirred at 300 rpm for 30 min to obtain a carbon nanotube / alkaline urea dispersion;

[0041] (2) 3 g of microcrystalline cellulose was placed in a three-necked flask, and then 50 mL of the carbon nanotube / alkaline urea dispersion obtained in step (1) was added under ice bath conditions and vigorously stirred for 2 min until the solution was transparent, and then 1.3 mL of epichlorohydrin was added for pre-crosslinking for 35 s to obtain a pre-crosslinked cellulose / carbon nanotube composite solution;

[0042] (3) 11 mL of the pre-crosslinked cellulose / carbon nanotube composite solution obtained in step (2) is added to the premixed oil phase (80 mL of white oil, 160 mL of isooctane, 11 g of Span-80, and 2 g of Tween-80), and emulsified under mechanical stirring at 250 rpm for 10-30 min, and then 200 mL of a 50 vol% ethanol solution is slowly dropped in for stirring and solidification. After standing, the oil and water layers are separated, and the aqueous phase is centrifuged at 4000 rpm for 3 min and the upper aqueous phase is poured out. Subsequently, the microspheres are washed with a 50 vol% ethanol solution under vigorous shaking and centrifugation, and the washing is repeated three times. The microspheres are then washed with pure water for at least three times, and then the microspheres are soaked with ethanol solutions of gradient concentrations of 20 vol%, 40 vol%, 60 vol%, 80 vol% and 100 vol%, each time for at least 10 min, and the 100 vol% ethanol soaking is performed at least three times. Finally, the microspheres are soaked in a gradient tert-butyl alcohol solution, and freeze-dried to obtain a super-large porous cellulose / carbon nanotube composite microsphere chromatographic medium.

[0043] Embodiment 3:

[0044] The ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium obtained in Example 1 was used to perform function and adsorption performance tests, and the specific steps are as follows:

[0045] Chromatographic Media Functionalization:

[0046] (1) Weigh 10.0 g of the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium obtained in Example 1 into a 100 mL three-necked flask, then add 20 mL of 3M sodium hydroxide solution and 20 mL of dimethyl sulfoxide, and react in a 40° C. water bath for 0.5 h, then add 10 mL of epichlorohydrin and react at 40° C. for 2.5 h;

[0047] (2) The microspheres obtained above were washed with water and dried, and then 20 mL of 400 mg / mL dextran-40 solution, 20 mL of 1 M sodium hydroxide solution and 0.1 g of sodium borohydride were added and reacted at 25° C. for 18 h.

[0048] (3) Wash the microspheres obtained above with water, and drain them to obtain functionalized microspheres.

[0049] Chromatographic media adsorption performance test:

[0050] (1) Adsorption thermodynamics: different concentrations (100-1000 mg L -1 ) of pancreatic kallikreinogenase solution, take 10 mL respectively, then add 10 mg of the above functionalized microspheres respectively, adsorb at room temperature for 24 h, and then measure the concentration after adsorption with a UV spectrophotometer;

[0051] (2) Adsorption kinetics: 500 mg L -1 Add 0.15 g of functionalized microspheres to 250 mL of kallikreinogenase solution, and record the absorbance of the solution at different adsorption times to calculate the concentration at different adsorption times.

[0052] (3) Cyclic adsorption: The adsorbed microspheres were eluted with 0.5 M sodium chloride solution, and then subjected to static adsorption, which was repeated multiple times.

[0053] The above experimental results are as follows Figure 4 shown.

[0054] Depend on Figure 4 It can be seen that the maximum adsorption capacity of pancreatic kallikrein in the functionalized macroporous microspheres is as high as 550 mg / g. The adsorption kinetics show that the adsorption quickly reaches equilibrium within 100 minutes. The cyclic adsorption shows that the cellulose / carbon nanotube composite chromatographic microspheres have good recyclability.

[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium, characterized in that: The following steps are involved: (1) magnetically stirring sodium hydroxide, thiourea and deionized water until the solid is completely dissolved to obtain an alkaline urea solution; then pouring the carbon nanotubes into the alkaline urea solution and magnetically stirring at the same time to obtain a carbon nanotube / alkaline urea dispersion; (2) placing microcrystalline cellulose in a three-necked flask, then adding the carbon nanotube / alkaline urea dispersion obtained in step (1) under ice bath conditions and stirring until the solution is transparent, and then adding epichlorohydrin for pre-crosslinking to obtain a pre-crosslinked cellulose / carbon nanotube composite solution; (3) adding the pre-crosslinked cellulose / carbon nanotube composite solution obtained in step (2) to the premixed oil phase, emulsifying under mechanical stirring, then dropping into an ethanol solution and stirring to solidify, allowing to stand for stratification, and then centrifuging, washing, gradient soaking and freeze-drying in sequence to obtain an ultra-large pore cellulose / carbon nanotube composite microsphere chromatographic medium.

2. The method for preparing the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium according to claim 1, characterized in that: In step (1), the mass volume ratio of sodium hydroxide, thiourea, carbon nanotubes and deionized water is 5g:4g:0.1-0.2g:50mL.

3. The method for preparing the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium according to claim 1, characterized in that: In step (1), carbon nanotubes were added and magnetically stirred at 300 rpm for 30 min.

4. The method for preparing the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium according to claim 1, characterized in that: In step (2), the mass volume ratio of microcrystalline cellulose, carbon nanotube / alkaline urea dispersion and epichlorohydrin is 3g:50mL:1.2-1.5mL.

5. The method for preparing the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium according to claim 1, characterized in that: In step (3), the volume ratio of the pre-crosslinked cellulose / carbon nanotube composite solution to the ethanol solution is 10-12 mL:100 mL.

6. The method for preparing the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium according to claim 1, characterized in that: In step (3), the premixed oil phase is prepared by the following method: premixing Span-80, Tween-80, white oil and isooctane in a 25° C. water bath for 30 minutes to obtain the premixed oil phase.

7. The method for preparing the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium according to claim 6, characterized in that: The mass volume ratio of Span-80, Tween-80, white oil and isooctane is 5.5g:1g:40mL:80mL.

8. The method for preparing the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium according to claim 1, characterized in that: In step (3), emulsification is carried out under mechanical stirring at 250 rpm for 10-30 min.

9. The method for preparing the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium according to claim 1, characterized in that: In step (3), the oil-water layers are separated after standing, the aqueous phase is centrifuged at 4000 rpm for 2-4 min and the upper aqueous phase is discarded, then washed with 50 vol% ethanol solution and centrifuged, the washing is repeated three times, and then washed with pure water at least three times, and then the microspheres are soaked in ethanol solutions with gradient concentrations of 20 vol%, 40 vol%, 60 vol%, 80 vol% and 100 vol%, each time for at least 10 min, and soaked in 100 vol% ethanol for at least three times, and finally soaked in tert-butanol ethanol solution for gradient soaking and freeze-drying.

10. The ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium obtained by the method for preparing the ultra-macroporous cellulose / carbon nanotube composite microsphere chromatographic medium according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method for preparing super-hole fibrin microsphere protein absorbing medium

    CN101036876A

  • Cellulose micro-sphere with uniform size as well as preparation method and application thereof

    CN103756016A

  • Green synthetic method of macroporous cellulose chromatographic microspheres

    CN104759271A

Cited By

  • Bifunctional cellulose porous chromatographic medium, preparation method thereof and exosome enrichment method

    CN121244183A