Preparation method and application of catalyst for hydrogen production through methane cracking
Through the preparation method of Fe-Ni catalyst, combined with transition metal additives and equal volume impregnation method, the activity and stability of methane cracking catalysts are solved, high-purity hydrogen generation and the formation of carbon nanotube metal symbiotic materials are achieved, and the catalyst is improved The activity and stability of the solution solve the problems of sintering and carbonaceous compounds blockage.
Patent Information
- Application Number
- CN202410499832.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-24
- Publication Date
- 2024-11-01
AI Technical Summary
The existing methane cracking hydrogen production catalyst has low activity and service life, and is prone to inactivation due to sintering and blockage of carbonaceous compounds.
Using Fe-Ni as the active component and combined with transition metal as an additive, the catalyst is prepared by equal volume impregnation method to avoid amorphous carbon blockage, promote the growth of carbon nanotubes on metal particles, and improve the uniformity and dispersion of active sites. , enhance the stability of the catalyst.
The formation of high-purity hydrogen and the formation of carbon nanotube metal symbiotic materials are achieved, the activity and stability of the catalyst are improved, the service life is extended, and structural stability is maintained under high temperature conditions.
Smart Images

Figure BDA0004808331550000111 
Figure BDA0004808331550000121 
Figure BDA0004808331550000122
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of methane catalytic cracking hydrogen production, and relates to a preparation method and application of a methane cracking hydrogen production catalyst. Background Art
[0002] Traditional natural gas hydrogen production mainly includes steam reforming (SMR), partial oxidation (POX) and autothermal reforming (ATR) which is a combination of the above two routes. At present, more than 50% of hydrogen production in the world comes from natural gas hydrogen production, and 90% of hydrogen abroad comes from natural gas hydrogen production, and most of them use traditional SMR process. The traditional technical route has high energy consumption, and CO will be produced during the conversion, and CO will cover the active sites of the Pt catalyst in the fuel cell. Therefore, the volume fraction of CO for transportation hydrogen is required to be below 0.001%. There is no CO or CO2 generated in the methane cracking hydrogen production reaction, and pure hydrogen can be obtained. The key to methane catalytic cracking hydrogen production is the catalyst. At present, the methane hydrogen production catalyst mainly uses precious metals (Pt, Ru, Pd) and a small amount of non-precious metals (Ni, Fe, Co) as active sites. Precious metal catalysts have good catalytic activity, but they cannot be produced on a large scale industrially due to their high price. Non-metallic catalysts reduce the reaction cost and can obtain more ideal reaction activity, so they have been widely used. Patent CN102489311A discloses a methane catalytic cracking hydrogen production catalyst, which has the characteristics of high activity, good dispersibility, and strong temperature resistance, but the use of precious metals increases the reaction cost. Patent CN106000444A discloses a method for preparing a highly dispersed nickel-based methane carbon dioxide reforming catalyst, which has high reaction activity, but due to the small Ni particles, this series of catalysts is very easy to sinter, and the production of carbonaceous compounds will block or cover the active sites of the catalyst, resulting in low catalyst activity and easy deactivation. Therefore, the development of highly active, highly stable, and non-sintering anti-carbon deposition catalysts is still a key issue in the development of methane catalytic cracking hydrogen production. Summary of the invention
[0003] One object of the present invention is to provide a method for preparing a methane cracking hydrogen production catalyst, which solves the problem of low activity and service life of the existing methane cracking hydrogen production catalyst.
[0004] Another object of the present invention is to provide an application method of the methane cracking hydrogen production catalyst.
[0005] The first technical scheme adopted by the present invention is a method for preparing a methane cracking hydrogen production catalyst, comprising preparing a catalyst precursor with Fe-Ni as an active component, preparing an auxiliary agent aqueous solution with a transition metal as an auxiliary agent metal source, adding the catalyst precursor to the auxiliary agent aqueous solution by an equal volume impregnation method, standing and aging, and finally drying and calcining to obtain a methane cracking catalyst.
[0006] The specific steps include:
[0007] Step 1, carrier treatment, the carrier is soaked and rinsed with ultrapure water, ultrasonically cleaned, dried and calcined to obtain a catalyst carrier;
[0008] Step 2, preparing the active component, weighing the nickel source and the iron source, and preparing an active component aqueous solution, the concentration of the active component aqueous solution is 0.1-2.0 mol / L, and the molar ratio of Ni / Fe is 1-10;
[0009] Step 3, using an ion exchange method, adding the catalyst support to the active component aqueous solution, performing ion exchange in a 70-85° C. water bath, then filtering, washing, drying, and calcining in a muffle furnace to obtain a catalyst precursor;
[0010] Step 4, preparing an auxiliary agent aqueous solution, based on the total mass of the catalyst, the loading amount of the auxiliary agent is 0.1-1.5%wt, and the auxiliary agent metal source is weighed according to the auxiliary agent loading amount to prepare an auxiliary agent aqueous solution;
[0011] Step 5, adding the catalyst precursor to the auxiliary agent aqueous solution by an equal volume impregnation method, aging, drying and calcining at room temperature to obtain a methane cracking catalyst.
[0012] The carrier is one or more of CeO2, SiO2, Al2O3, TiO2 and MgO.
[0013] The nickel source is nickel nitrate or nickel chloride, and the iron source is ferric nitrate or ferric chloride.
[0014] In step 3, the catalyst carrier is added into the aqueous solution of the active component, the mass of the catalyst carrier is x, x is in g, the volume of the aqueous solution of the active component is y, y is in mL, and y=6x.
[0015] In step 3, the drying temperature is 95-110° C., the drying time is 7 h-12 h, and the calcination is carried out in a muffle furnace, including raising the furnace temperature to 550-750° C. at 2° C. / min-5° C. / min and maintaining it for 6 h-12 h.
[0016] In step 4, the auxiliary metal source is Zr, Co, La, Cu, Mn or Zn.
[0017] In step 5, the aging time at room temperature is 12h-28h, the drying temperature is 95-110°C, the drying time is 7-12h, the heating rate of roasting is 2°C / min-5°C / min, the roasting temperature is 550-750°C, and the roasting time is 6h-12h.
[0018] The second technical solution adopted by the present invention is the application of methane cracking hydrogen production catalyst, which includes placing the prepared methane cracking catalyst in a tubular furnace, first introducing argon gas to replace the air and then introducing methane, heating to 500-700°C for reaction, collecting high-purity hydrogen, and after the reaction is completed, cooling the temperature in the argon atmosphere to room temperature to obtain a carbon nanotube metal material.
[0019] First, argon is introduced to replace the air and then methane is introduced. The argon flow rate is 100-500mL / min, the replacement time is 0.5h-5h, the methane space velocity is 20-30L / g / h, and the methane cracking reaction pressure is normal pressure.
[0020] The beneficial effects of the present invention are as follows:
[0021] (1) Fe-Ni is used as the active component of the methane cracking catalyst to prepare a catalyst precursor, a transition metal is used as an auxiliary metal source to prepare an auxiliary aqueous solution, the catalyst precursor is added to the auxiliary aqueous solution by an equal volume impregnation method to prepare a methane cracking catalyst, and the catalyst is used to catalytically crack methane to obtain high-purity hydrogen and carbon nanotube metal symbiotic materials. This method avoids the amorphous carbon generated by the methane cracking hydrogen production reaction blocking or covering the catalyst active sites, resulting in low catalyst activity or deactivation;
[0022] (2) During the catalytic cracking of methane, carbon nanotubes are grown in situ on metal particles. The metal active components loaded on carbon nanotubes can expose more active sites, thereby improving the uniformity and dispersion of the active metals. At the same time, carbon nanotubes can anchor metal particles, thereby avoiding the aggregation and loss of active components and improving the activity and stability of the methane cracking hydrogen production catalyst.
[0023] (3) The high-purity hydrogen produced by methane cracking can be directly used in hydrogen fuel cells;
[0024] (4) The synthesized carbon nanotube-metal symbiotic material has high structural regularity, high mechanical strength, and strong stability, especially under high temperature conditions. The spatial confinement effect of carbon nanotubes can effectively inhibit the growth and accumulation of metal particles during high-temperature reactions, which is beneficial to the efficient and long-term operation of methane cracking to produce hydrogen. DETAILED DESCRIPTION
[0025] The present invention is described in detail below in conjunction with specific implementation modes.
[0026] Example 1
[0027] A method for preparing a methane cracking hydrogen production catalyst and application of the catalyst, comprising the following steps:
[0028] Step 1, preparing a methane cracking catalyst, the specific process is as follows:
[0029] Step 1.1, carrier treatment, 15 g of silica was rinsed by immersion in ultrapure water, ultrasonically cleaned, dried and calcined to obtain a catalyst carrier;
[0030] Step 1.2, prepare the active component, weigh 12.18 g of nickel nitrate and 16.12 g of ferric nitrate and add them into a 200 mL volumetric flask to prepare a 0.5 mol / L active component aqueous solution, with a Ni / Fe molar ratio of 4;
[0031] Step 1.3, using an ion exchange method, adding all the catalyst supports prepared in step 1.1 to 90 mL of an active component aqueous solution, performing ion exchange in an 80° C. water bath, then filtering and washing, drying at 100° C. for 10 h, and then placing in a muffle furnace, raising the furnace temperature to 650° C. at a rate of 2° C. / min, and calcining for 8 h to obtain a catalyst precursor;
[0032] Step 1.4, preparing an auxiliary agent aqueous solution, weighing 1.26 g of manganese nitrate, and preparing an auxiliary agent aqueous solution, wherein the Mn loading amount is 0.5%wt;
[0033] Step 1.5, adding the catalyst precursor to the aqueous solution of the additive by an equal volume impregnation method, aging at room temperature for 24 hours, then drying at 100°C for 11 hours, and finally calcining at 700°C at a rate of 3°C / min for 7 hours to obtain a methane cracking catalyst.
[0034] Step 2, application of methane cracking catalyst, comprising placing the prepared methane cracking catalyst in a tubular furnace, first introducing argon to replace air and then introducing methane, the argon flow rate is 200 mL / min, the replacement time is 2 h, the methane space velocity is 24 L / g / h, heating to 600 ° C for reaction, the reaction pressure is normal pressure, the reaction tail gas enters the chromatographic automatic sampling system for analysis, the results are shown in Table 1, after the reaction is completed, the argon atmosphere is cooled to room temperature, and the carbon nanotube metal material is obtained.
[0035] In a fixed bed reactor, the carbon nanotube metal material prepared in Example 1 is used as a catalyst for the methanation reaction of carbon dioxide. Under normal pressure Ar atmosphere, the temperature is raised to 300°C at 6°C / min, and then raised to 400°C at 2°C / min. Then, it is switched to 10% H2 / Ar for reduction activation for 4h, and then switched to argon gas. The temperature is lowered to 300°C and the reaction gas is switched to react. The reaction gases are CO2, H2 and Ar, CO2:H2:Ar=1:4:2, the gas space velocity is 3.5L / g / h, the reaction pressure is 0.2MPa, and the reaction product is analyzed by a chromatographic automatic sampling system. The analysis results show that the carbon nanotube metal material is used as a catalyst for the methanation reaction of carbon dioxide. The CH4 conversion rate is 98.2% and the H2 selectivity is 100%, indicating that the catalyst has good catalytic effect and strong stability.
[0036] Example 2
[0037] A method for preparing a methane cracking hydrogen production catalyst and application of the catalyst, comprising the following steps:
[0038] Step 1, preparing a methane cracking catalyst, the specific process is the same as that of Example 1;
[0039] Step 2, application of methane cracking catalyst, comprising placing the prepared methane cracking catalyst in a tubular furnace, first introducing argon to replace air and then introducing methane, the argon flow rate is 100 mL / min, the replacement time is 5 h, the methane space velocity is 20 L / g / h, heating to 500° C. for reaction, the reaction pressure is normal pressure, the reaction tail gas enters the chromatographic automatic sampling system for analysis, the results are shown in Table 1, and after the reaction is completed, the temperature drops to room temperature in the argon atmosphere to obtain the carbon nanotube metal material.
[0040] Example 3
[0041] A method for preparing a methane cracking hydrogen production catalyst and application of the catalyst, comprising the following steps:
[0042] Step 1, preparing a methane cracking catalyst, the specific process is the same as that of Example 1;
[0043] Step 2, application of methane cracking catalyst, comprising placing the prepared methane cracking catalyst in a tubular furnace, first introducing argon to replace air and then introducing methane, the argon flow rate is 500 mL / min, the replacement time is 0.5 h, the methane space velocity is 30 L / g / h, heating to 700° C. for reaction, the reaction pressure is normal pressure, the reaction tail gas enters the chromatographic automatic sampling system for analysis, the results are shown in Table 1, and after the reaction is completed, the temperature drops to room temperature in the argon atmosphere to obtain the carbon nanotube metal material.
[0044] Example 4
[0045] A method for preparing a methane cracking hydrogen production catalyst and application of the catalyst, comprising the following steps:
[0046] Step 1, preparing a methane cracking catalyst, the specific process is as follows:
[0047] Step 1.1, carrier treatment, 15 g of cerium dioxide is soaked and rinsed with ultrapure water, ultrasonically cleaned, dried and calcined to obtain a catalyst carrier;
[0048] Step 1.2, prepare the active component, weigh 5.48 g of nickel nitrate and 14.51 g of ferric nitrate and add them into a 200 mL volumetric flask to prepare a 0.3 mol / L active component aqueous solution, with a Ni / Fe molar ratio of 2;
[0049] Step 1.3, using an ion exchange method, adding all the catalyst supports prepared in step 1.1 to 90 mL of an active component aqueous solution, performing ion exchange in a 70°C water bath for 7 h, then filtering and washing with ultrapure water, drying at 95°C for 12 h, and then placing in a muffle furnace, raising the furnace temperature to 550°C at 2°C / min, and calcining for 12 h to obtain a catalyst precursor;
[0050] Step 1.4, preparing an auxiliary agent aqueous solution, weighing 0.073 g of cobalt nitrate, and preparing an auxiliary agent aqueous solution, wherein the loading amount of Co is 0.3%wt;
[0051] Step 1.5, adding the catalyst precursor to the auxiliary agent aqueous solution by equal volume impregnation method, aging at room temperature for 28 hours, then drying at 95°C for 12 hours, and finally calcining at 550°C at 2°C / min for 12 hours to obtain a methane cracking catalyst.
[0052] Step 2, application of methane cracking catalyst, comprising placing the prepared methane cracking catalyst in a tubular furnace, first introducing argon to replace air and then introducing methane, the argon flow rate is 500 mL / min, the replacement time is 0.5 h, the methane space velocity is 20 L / g / h, heating to 500 ° C for reaction, the reaction pressure is normal pressure, the reaction tail gas enters the chromatographic automatic sampling system for analysis, the results are shown in Table 1, after the reaction is completed, the argon atmosphere is cooled to room temperature, and the carbon nanotube metal material is obtained.
[0053] Example 5
[0054] A method for preparing a methane cracking hydrogen production catalyst and application of the catalyst, comprising the following steps:
[0055] Step 1, preparing a methane cracking catalyst, the specific process is as follows:
[0056] Step 1.1, carrier treatment, 15 g of aluminum oxide was rinsed and soaked in ultrapure water, ultrasonically cleaned, dried and calcined to obtain a catalyst carrier;
[0057] Step 1.2, prepare the active component, weigh 26.10 g of nickel nitrate and 27.64 g of ferric nitrate and add them into a 200 mL volumetric flask to prepare a 1.0 mol / L active component aqueous solution, with a Ni / Fe molar ratio of 5;
[0058] Step 1.3, using an ion exchange method, adding all the catalyst supports prepared in step 1.1 to 90 mL of an active component aqueous solution, performing ion exchange in a 75°C water bath for 6 hours, then filtering and washing with ultrapure water, drying at 105°C for 10 hours, and then placing in a muffle furnace, raising the furnace temperature to 600°C at 3°C / min, and calcining for 9 hours to obtain a catalyst precursor;
[0059] Step 1.4, preparing an auxiliary agent aqueous solution, weighing 0.199 g of lanthanum nitrate, and preparing an auxiliary agent aqueous solution, wherein the loading amount of lanthanum is 1.0%wt;
[0060] Step 1.5, adding the catalyst precursor to the aqueous solution of the additive by an equal volume impregnation method, aging at room temperature for 20 hours, then drying at 105°C for 10 hours, and finally calcining at 600°C at a rate of 3°C / min for 9 hours to obtain a methane cracking catalyst.
[0061] Step 2, application of methane cracking catalyst, comprising placing the prepared methane cracking catalyst in a tubular furnace, first introducing argon to replace air and then introducing methane, the argon flow rate is 400 mL / min, the replacement time is 1.5 h, the methane space velocity is 24 L / g / h, heating to 600° C. for reaction, the reaction pressure is normal pressure, the reaction tail gas enters the chromatographic automatic sampling system for analysis, the results are shown in Table 1, and after the reaction is completed, the temperature drops to room temperature in the argon atmosphere to obtain the carbon nanotube metal material.
[0062] Example 6
[0063] A method for preparing a methane cracking hydrogen production catalyst and application of the catalyst, comprising the following steps:
[0064] Step 1, preparing a methane cracking catalyst, the specific process is as follows:
[0065] Step 1.1, carrier treatment, 15 g of titanium oxide was rinsed and soaked in ultrapure water, ultrasonically cleaned, dried and calcined to obtain a catalyst carrier;
[0066] Step 1.2, prepare the active component, weigh 60.90g of nickel nitrate and 32.25g of ferric nitrate and add them into a 200mL volumetric flask to prepare a 2.0 mol / L active component aqueous solution, with a Ni / Fe molar ratio of 10;
[0067] Step 1.3, using an ion exchange method, adding all the catalyst supports prepared in step 1.1 to 90 mL of an active component aqueous solution, performing ion exchange in an 85°C water bath for 5 h, then filtering and washing with ultrapure water, drying at 110°C for 7 h, and then placing in a muffle furnace, raising the furnace temperature to 750°C at 5°C / min, and calcining for 6 h to obtain a catalyst precursor;
[0068] Step 1.4, preparing an auxiliary aqueous solution, weighing 0.354 g of copper nitrate, and preparing an auxiliary aqueous solution, the copper loading amount is 1.5%wt;
[0069] Step 1.5, adding the catalyst precursor to the auxiliary agent aqueous solution by equal volume impregnation method, aging at room temperature for 20 hours, then drying at 110°C for 7 hours, and finally calcining at 750°C at 5°C / min for 6 hours to obtain a methane cracking catalyst.
[0070] Step 2, application of methane cracking catalyst, comprising placing the prepared methane cracking catalyst in a tubular furnace, first introducing argon to replace air and then introducing methane, the argon flow rate is 300 mL / min, the replacement time is 2.5 h, the methane space velocity is 30 L / g / h, heating to 700 ° C for reaction, the reaction pressure is normal pressure, the reaction tail gas enters the chromatographic automatic sampling system for analysis, the results are shown in Table 1, after the reaction is completed, the argon atmosphere is cooled to room temperature, and the carbon nanotube metal material is obtained.
[0071] Example 7
[0072] A method for preparing a methane cracking hydrogen production catalyst and application of the catalyst, comprising the following steps:
[0073] Step 1, preparing a methane cracking catalyst, the specific process is as follows:
[0074] Step 1.1, carrier treatment, 15 g of silica was rinsed by immersion in ultrapure water, ultrasonically cleaned, dried and calcined to obtain a catalyst carrier;
[0075] Step 1.2, prepare the active component, weigh 1.22g of nickel nitrate and 6.45g of ferric nitrate and add them into a 200mL volumetric flask to prepare a 0.1 mol / L active component aqueous solution, with a Ni / Fe molar ratio of 1;
[0076] Step 1.3, using an ion exchange method, adding all the catalyst supports prepared in step 1.1 to 90 mL of an active component aqueous solution, performing ion exchange in a water bath at 83°C for 5.5 hours, then filtering and washing with ultrapure water, drying at 102°C for 8.5 hours, and then placing in a muffle furnace, raising the furnace temperature to 680°C at a rate of 2.5°C / min, and calcining for 8.5 hours to obtain a catalyst precursor;
[0077] Step 1.4, preparing an auxiliary agent aqueous solution, weighing 0.027 g of zirconium nitrate, and preparing an auxiliary agent aqueous solution, the copper loading amount is 0.1%wt;
[0078] Step 1.5, adding the catalyst precursor to the aqueous solution of the additive by an equal volume impregnation method, aging at room temperature for 15 hours, then drying at 110°C for 7 hours, and finally calcining at 700°C at 4°C / min for 6 hours to obtain a methane cracking catalyst.
[0079] Step 2, application of methane cracking catalyst, comprising placing the prepared methane cracking catalyst in a tubular furnace, first introducing argon to replace air and then introducing methane, the argon flow rate is 200 mL / min, the replacement time is 4 hours, the methane space velocity is 30 L / g / h, heating to 700°C for reaction, the reaction pressure is normal pressure, the reaction tail gas enters the chromatographic automatic sampling system for analysis, the results are shown in Table 1, and after the reaction is completed, the temperature drops to room temperature in the argon atmosphere to obtain the carbon nanotube metal material.
[0080] Example 8
[0081] A method for preparing a methane cracking hydrogen production catalyst and application of the catalyst, comprising the following steps:
[0082] Step 1, preparing a methane cracking catalyst, the specific process is as follows:
[0083] Step 1.1, carrier treatment, 15 g of magnesium oxide is soaked and rinsed with ultrapure water, ultrasonically cleaned, dried and calcined to obtain a catalyst carrier;
[0084] Step 1.2, prepare the active component, weigh 23.39 g of nickel nitrate and 15.48 g of ferric nitrate and add them into a 200 mL volumetric flask to prepare a 0.8 mol / L active component aqueous solution, with a Ni / Fe molar ratio of 8;
[0085] Step 1.3, using an ion exchange method, adding all the catalyst supports prepared in step 1.1 to 90 mL of an active component aqueous solution, performing ion exchange in an 85°C water bath for 7 h, then filtering and washing with ultrapure water, drying at 110°C for 11 h, and then placing in a muffle furnace, raising the furnace temperature to 700°C at 4°C / min, and calcining for 12 h to obtain a catalyst precursor;
[0086] Step 1.4, preparing an auxiliary agent aqueous solution, weighing 0.09 g of zinc nitrate, and preparing an auxiliary agent aqueous solution, the zinc loading amount is 0.9%wt;
[0087] Step 1.5, adding the catalyst precursor to the aqueous solution of the additive by an equal volume impregnation method, aging at room temperature for 19 hours, then drying at 110°C for 12 hours, and finally calcining at 700°C at a rate of 5°C / min for 12 hours to obtain a methane cracking catalyst.
[0088] Step 2, application of methane cracking catalyst, comprising placing the prepared methane cracking catalyst in a tubular furnace, first introducing argon to replace air and then introducing methane, the argon flow rate is 350 mL / min, the replacement time is 2 h, the methane space velocity is 30 L / g / h, heating to 700° C. for reaction, the reaction pressure is normal pressure, the reaction tail gas enters the chromatographic automatic sampling system for analysis, the results are shown in Table 1, and after the reaction is completed, the argon atmosphere is cooled to room temperature to obtain a carbon nanotube metal material.
[0089] Example 9
[0090] A method for preparing a methane cracking hydrogen production catalyst and application of the catalyst, comprising the following steps:
[0091] Step 1, preparing a methane cracking catalyst, the same as in Example 7;
[0092] Step 2, application of methane cracking catalyst, comprising placing the prepared methane cracking catalyst in a tubular furnace, first introducing argon to replace air and then introducing methane, the argon flow rate is 500 mL / min, the replacement time is 0.5 h, the methane space velocity is 22 L / g / h, heating to 600 ° C for reaction, the reaction pressure is normal pressure, the reaction tail gas enters the chromatographic automatic sampling system for analysis, and the reaction results of 10h, 20h, 30h, 50h, 100h, 200h, and 300h are collected respectively, as shown in Table 2, and after the reaction is completed, the temperature drops to room temperature in the argon atmosphere to obtain a carbon nanotube metal material.
[0093] Table 1 Methane cracking reaction results
[0094]
[0095]
[0096] Table 2 Stability test of methane cracking catalyst
[0097]
Claims
1. A method for preparing a catalyst for producing hydrogen by cracking methane, characterized in that: The method comprises preparing a catalyst precursor with Fe-Ni as an active component, preparing an auxiliary agent aqueous solution with a transition metal as an auxiliary agent metal source, adding the catalyst precursor into the auxiliary agent aqueous solution by an equal volume impregnation method, standing and aging, and finally drying and calcining to obtain a methane cracking hydrogen production catalyst.
2. The method for preparing a methane cracking hydrogen production catalyst according to claim 1, characterized in that: The specific steps include: Step 1, carrier treatment, the carrier is soaked and rinsed with ultrapure water, ultrasonically cleaned, dried and calcined to obtain a catalyst carrier; Step 2, preparing the active component, weighing the nickel source and the iron source, and preparing an active component aqueous solution, the concentration of the active component aqueous solution is 0.1-2.0 mol / L, and the molar ratio of Ni / Fe is 1-10; Step 3, using an ion exchange method, adding the catalyst support to the active component aqueous solution, performing ion exchange in a 70-85° C. water bath, then filtering, washing, drying, and calcining in a muffle furnace to obtain a catalyst precursor; Step 4, preparing an auxiliary agent aqueous solution, based on the total mass of the catalyst, the loading amount of the auxiliary agent is 0.1-1.5%wt, and the auxiliary agent metal source is weighed according to the auxiliary agent loading amount to prepare an auxiliary agent aqueous solution; Step 5, adding the catalyst precursor to the auxiliary agent aqueous solution by an equal volume impregnation method, aging, drying and calcining at room temperature to obtain a methane cracking hydrogen production catalyst.
3. The method for preparing a methane cracking hydrogen production catalyst according to claim 2, characterized in that: The carrier is one or more of CeO2, SiO2, Al2O3, TiO2 and MgO.
4. The method for preparing a catalyst for producing hydrogen by cracking methane according to claim 3, characterized in that: The nickel source is nickel nitrate or nickel chloride, and the iron source is ferric nitrate or ferric chloride.
5. The method for preparing a catalyst for producing hydrogen from methane cracking according to claim 4, characterized in that: In the step 3, the catalyst carrier is added into the aqueous solution of the active component, the mass of the catalyst carrier is x, x is in g, the volume of the aqueous solution of the active component is y, y is in mL, and y=6x.
6. The method for preparing a catalyst for producing hydrogen by cracking methane according to claim 5, characterized in that: In the step 3, the drying temperature is 95-110° C., the drying time is 7 h-12 h, and the calcination is carried out in a muffle furnace, including raising the furnace temperature to 550-750° C. at a rate of 2° C. / min-5° C. / min and maintaining it for 6 h-12 h.
7. The method for preparing a catalyst for producing hydrogen by cracking methane according to claim 6, characterized in that: In step 4, the auxiliary metal source is Zr, Co, La, Cu, Mn or Zn.
8. The method for preparing a catalyst for producing hydrogen by cracking methane according to claim 6, characterized in that: In step 5, the aging time at room temperature is 12h-28h, the drying temperature is 95-110°C, the drying time is 7-12h, the heating rate of roasting is 2°C / min-5°C / min, the roasting temperature is 550-750°C, and the roasting time is 6h-12h.
9. Use of a methane cracking hydrogen production catalyst prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The method comprises placing the prepared methane cracking hydrogen production catalyst in a tubular furnace, introducing argon gas to replace the air first and then introducing methane, heating to 500-700°C for reaction, collecting high-purity hydrogen, and cooling the argon atmosphere to room temperature after the reaction is completed, thereby obtaining the carbon nanotube metal material.
10. The use of the catalyst for producing hydrogen from methane cracking according to claim 9, characterized in that: First, argon is introduced to replace the air and then methane is introduced. The argon flow rate is 100-500mL / min, the replacement time is 0.5h-5h, the methane space velocity is 20-30L / g / h, and the methane cracking reaction pressure is normal pressure.
Citation Information
Patent Citations
Catalyst for preparing H2 and CNTs through direct cracking of natural gas, and preparation method and application of catalyst
CN111167460A
Preparation method of methane cracking catalyst
CN114011418A
Catalytic cracking process for preparing hydrogen or hydrogenane from methane
CN1350977A
Catalyst for hydrogen production by methane catalytic cracking and preparation method thereof
CN1689699A
Catalytic Decomposition of Lower Hydrocarbons to Produce Carbon Oxides Free Hydrogen and Bamboo Shaped Carbon Nanotubes
US20160129424A1