Preparation method and application of thin-layer porous carbon nitride
The thin-layer porous carbon nitride catalyst was prepared by combining solvent-thermal method and polyol intercalation, which solved the problem of low efficiency of traditional carbon nitride catalysts, and achieved efficient breaking of C-C bonds in aromatic ortho-diols, and the catalyst was repeated. Good performance.
Patent Information
- Application Number
- CN202410896157.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-05
AI Technical Summary
In the prior art, the catalyst for breaking the C-C bond in aromatic ortho-diol is low in efficiency and has poor reuse performance. The traditional carbon nitride catalyst has a narrow absorption spectrum, a small specific surface area and a low photogenerated carrier recombination rate, resulting in light. The catalytic performance is not high.
The thin-layer porous carbon nitride catalyst was prepared by combining solvent-thermal method-polyol intercalation and high-temperature calcination, and the C-C bond in the broken aromatic o-diol was used in the aqueous medium, and the C-C bond in the alcohol reflux solution was peeled off. A carbon nitride photocatalyst formed in a thin layer state.
The efficiency of photocatalytic fracture of aromatic o-diol C-C bonds is significantly improved, the reaction rate is increased by about 3 times, the substrate conversion rate can reach 97.6%, and the catalyst has good reusability.
Smart Images

Figure CN118874508A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the preparation and application of a porous photocatalyst, and in particular to a preparation method of a thin layer of porous carbon nitride and the application of the thin layer of porous carbon nitride in photocatalytic cleavage of the CC bond of aromatic vicinal diols. Background Art
[0002] The molecular structure of biomass is relatively complex and contains a high amount of oxygen, which makes it difficult to break the CC bonds in its molecular structure and prepare small molecule compounds with high added value by hydrogenation and deoxygenation. In the past, the catalysts commonly used to break CC bonds were mainly precious metals, which were expensive. Non-precious metal catalysts have low efficiency in breaking CC bonds, and the catalysts are not reusable.
[0003] Photocatalysis is a green and sustainable technology that uses solar energy as energy. Carbon nitride (CN), as a typical non-metallic photocatalyst, has excellent stability in photocatalytic reactions, and its preparation raw materials are readily available and non-toxic, making it a highly promising photocatalytic material. However, the narrow absorption spectrum, small specific surface area, and high recombination rate of photogenerated carriers of carbon nitride lead to its low photocatalytic performance, and its efficiency in breaking CC bonds in aromatic vicinal diols with different substituents is low.
[0004] Chinese patent 202011053924.X discloses a method for preparing a black nickel oxide catalyst and applying it to the cleavage of CC bonds in aromatic vicinal diols. The method requires a reaction temperature of 30-190°C, a pressure of 0.1-10MPa, and a reaction time of 2-30h. The reaction conditions are harsh, the energy consumption is high, and the reaction time is long. Chinese patent 202110917000.8 discloses a reaction system composed of an iron catalyst, an organic base, and an organic solvent. The system can cleave CC bonds in aromatic alcohols to obtain high-value chemicals such as ketones and aldehydes. However, it is difficult to separate the product from the organic base in this method, and the catalyst reuse rate is low. Reference (Green Chem., 23(24)(2021):10071-10078.) reports a method for photocatalytic cleavage of CC bonds in 1,2-diphenylethanol by a heterojunction photocatalyst composed of carbon nitride and silver phosphate in an organic system. However, the catalyst uses precious metal silver and the catalytic performance still has a lot of room for improvement. Summary of the invention
[0005] Purpose of the invention: The purpose of the present invention is to provide a method for preparing a thin layer of porous carbon nitride, to solve the problem of how to prepare a carbon nitride catalyst that can efficiently break the CC bond in aromatic vicinal diols. Another purpose of the present invention is to propose the application of the thin layer of porous carbon nitride in the photocatalytic breaking of the CC bond of aromatic vicinal diols, to solve the problem of how to break the CC bond in aromatic vicinal diols with different substituents in an aqueous medium.
[0006] Technical solution: The method for preparing a thin layer of porous carbon nitride according to the present invention comprises the following steps:
[0007] (1) hydrothermally reacting melamine and cyanuric acid to obtain a tubular precursor;
[0008] (2) using an alcohol reflux solution to strip the tubular precursor to obtain an intermediate;
[0009] (3) Calcination of the intermediate to obtain a thin layer of porous carbon nitride.
[0010] The present invention adopts a solvent thermal method-polyol intercalation and high temperature calcination combined method to prepare a thin layer porous carbon nitride photocatalyst, and applies it to photocatalytically break the C—C bond of aromatic vicinal diols with different substituents in an aqueous medium, thereby obtaining an excellent substrate conversion rate and a high yield of aromatic aldehydes and acids of high value chemicals. In step (2), the tubular precursor is stripped mainly by refluxing the alcohol to form a thin layer of carbon nitride photocatalyst.
[0011] Preferably, in step (1), the hydrothermal reaction method is: adding melamine and cyanuric acid into water and mixing them evenly, performing hydrothermal reaction at 140-180° C. for 6-24 hours, and obtaining a tubular precursor through cooling, filtering, washing and drying.
[0012] Preferably, in step (1), the mass ratio of melamine to cyanuric acid is 1:1-1.5.
[0013] Preferably, in step (2), the stripping of the tubular precursor using an alcohol reflux liquid comprises the following steps:
[0014] (21) mixing diethylene glycol and ethanol to obtain a reflux liquid or using only diethylene glycol as the reflux liquid;
[0015] (22) The tubular precursor is added to a reflux liquid to obtain a suspension, and the suspension is refluxed to obtain an intermediate.
[0016] Preferably, in step (21), the volume ratio of diethylene glycol to ethanol is 1:1-5.
[0017] Preferably, in step (22), the material-liquid ratio of the tubular precursor to the reflux liquid is 0.4-0.8 g: 10-30 mL, and the reflux conditions are: reflux at 80-100° C. for 1-5 h.
[0018] Preferably, in step (3), the calcination method is: in an inert gas atmosphere, the temperature is raised to 500-650° C. at 5-10° C. / min, and the temperature is kept for 3-5 hours. The inert gas can be nitrogen, argon or other inert gases.
[0019] The present invention further applies the thin layer porous carbon nitride prepared by the above preparation method to the photocatalytic cleavage of the CC bond of aromatic vicinal diols.
[0020] The thin layer porous carbon nitride prepared by the above method has excellent light absorption range, photogenerated carrier separation efficiency and suitable energy band structure, and can significantly improve the efficiency of photocatalytic cleavage of C—C bonds of aromatic vicinal diols with different substituents. This application can prepare aromatic aldehydes and aromatic acids by cleavage of C—C bonds of aromatic vicinal diols.
[0021] The above application includes the following steps:
[0022]
[0023] The catalyst is a thin layer of porous carbon nitride prepared by the preparation method according to any one of claims 1 to 7, wherein R1 and R2 are independently selected from substituted or unsubstituted aromatic groups, H, substituted or unsubstituted furanyl groups, R1 and R2 are not H at the same time, and the substituent group of the aromatic group is selected from halogen or C 1-3 The halogen can be selected from F, Cl, Br, I, and the R3 and R4 are independently selected from methyl or H.
[0024] Preferably, the R1 is selected from phenyl, phenyl substituted with halogen or methyl, and the R2 is selected from phenyl, phenyl substituted with halogen or methyl, H.
[0025] In some embodiments, compound (I) is 1,2-diphenylethylene glycol, 2,3-diphenyl-2,3-butanediol, 1,2-di-p-tolylethane-1,2-diol, 1,2-bis(4-chlorophenyl)ethane-1,2-diol, 1,2-di(furan-2-yl)ethane-1,2-diol, 1-phenylethane-1,2-diol, and its structural formula is as follows:
[0026]
[0027] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0028] Compared with carbon nitride prepared by traditional methods, the thin-layer porous carbon nitride catalyst prepared by the present invention has a higher photocatalytic cleavage efficiency for the CC bonds of aromatic vicinal diols with different substituents (the reaction rate is increased by about 3 times), and the conversion rate of the raw materials can reach 97.6%. It successfully solves the problem of low photocatalytic cleavage efficiency of existing carbon nitride catalysts for the CC bonds of aromatic vicinal diols, can be used for the efficient preparation of aromatic aldehydes and aromatic acids, and has good application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a scanning electron microscope image of the thin layer of porous carbon nitride prepared by the present invention;
[0030] Figure 2 XRD patterns of CN prepared by conventional methods and thin-layer porous carbon nitride prepared by the present invention;
[0031] Figure 3 Fourier infrared spectra of CN prepared by traditional methods and thin layer porous carbon nitride prepared by the present invention;
[0032] Figure 4 The photocurrent diagrams of CN prepared by the traditional method and the thin layer porous carbon nitride prepared by the present invention;
[0033] Figure 5 Impedance diagrams of CN prepared by conventional methods and thin-layer porous carbon nitride prepared by the present invention;
[0034] Figure 6 Mott-Schottky diagrams of CN prepared by conventional methods and thin-layer porous carbon nitride prepared by the present invention;
[0035] Figure 7 The photoluminescence spectra of CN prepared by the traditional method and the thin layer porous carbon nitride prepared by the present invention are shown;
[0036] Figure 8 It is a time course curve of the breaking of the CC bond of 1,2-diphenylethylene glycol by the thin layer porous carbon nitride prepared in Example 1;
[0037] Fig. 9 This is a diagram showing the repeated use performance of the thin layer of porous carbon nitride prepared in Example 1 by breaking the CC bond of 1,2-diphenylethylene glycol. DETAILED DESCRIPTION
[0038] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0039] Example 1: A method for preparing a thin layer of porous carbon nitride is as follows:
[0040] Weigh 1g of melamine and 1.2g of cyanuric acid and add them to 80mL of deionized water. After stirring in an 80℃ oil bath for 30min, pour them into a stainless steel reactor with polytetrafluoroethylene for hydrothermal reaction. The temperature of the hydrothermal reaction is 160℃ and the insulation time is 10h. The solution in the reactor is filtered, washed, dried and ground to obtain a tubular precursor.
[0041] Weigh 0.6g of tubular precursor, 5mL of diethylene glycol and 10mL of ethanol into a 50mL round-bottom flask and reflux at 90℃ for 3h. After cooling, centrifugation, drying and grinding, put it into a quartz boat and heat it to 550℃ at a heating rate of 10℃ / min in a nitrogen atmosphere in a tubular furnace for 4h. After cooling and grinding, a thin layer of porous carbon nitride can be obtained, and its microstructure is as follows: Figure 1 shown.
[0042] The standard conditions for photocatalytic cleavage of the CC bond of aromatic vicinal diols are as follows. First, 0.01g of the prepared carbon nitride-based photocatalyst, 0.01g of the reaction substrate (aromatic vicinal diol), 200μL of acetic acid and 2.8mL of micellar aqueous phase medium (sodium dodecyl sulfonate solution with a mass fraction of 8‰) were added to a ground quartz test tube, and the ground quartz test tube was sealed with a rubber stopper. After that, the above-mentioned quartz test tube was placed in an ultrasonic generator for 10min, and then evacuated and filled with oxygen using a syringe and a vacuum pump. This operation was repeated three times. Finally, the quartz test tube was placed under a 300W xenon lamp for light irradiation for a specified time. After the reaction was completed, 3mL of acetonitrile and 200μL of naphthalene solution (internal standard) were added to the quartz test tube. After stirring for 5min, the above-mentioned suspension was drawn with a syringe and the catalyst was filtered using a 0.22μm nylon filter membrane to obtain a solution to be analyzed containing substrates and products. High performance liquid chromatography was used to test the contents of substrates and products in the solution to be analyzed, and the substrate conversion rate and product yield were calculated.
[0043] Under standard conditions, the photocatalytic conversion rate of 1,2-diphenylethylene glycol by the thin layer of porous carbon nitride was 92.1%, the yield of benzaldehyde was 43.3%, and the yield of benzoic acid was 45.2%.
[0044] Embodiment 2: The rest is the same as Embodiment 1, except that:
[0045] 0.6 g of the tubular precursor and 15 mL of diethylene glycol were weighed into a 50 mL round-bottom flask and refluxed at 90 °C for 3 h.
[0046] Under standard conditions, the photocatalytic conversion rate of 1,2-diphenylethylene glycol by the thin layer porous carbon nitride prepared in this example was 83.2%, the yield of benzaldehyde was 53.7%, and the yield of benzoic acid was 35.2%.
[0047] Embodiment 3: The rest is the same as Embodiment 1, except that:
[0048] Weigh 2 g of melamine and add it into 80 mL of deionized water.
[0049] Under standard conditions, the photocatalytic conversion rate of 1,2-diphenylethylene glycol by the thin layer porous carbon nitride prepared in this example was 65.8%, the yield of benzaldehyde was 42.6%, and the yield of benzoic acid was 18.7%.
[0050] Example 4: A method for preparing a thin layer of porous carbon nitride is as follows:
[0051] Weigh 1g of melamine and 1.5g of cyanuric acid and add them to 80mL of deionized water. After stirring in an 80℃ oil bath for 30min, pour them into a stainless steel reactor with polytetrafluoroethylene for hydrothermal reaction. The temperature of the hydrothermal reaction is 180℃ and the insulation time is 6h. The solution in the reactor is filtered, washed, dried and ground to obtain a tubular precursor. Weigh 0.8g of tubular precursor, 5mL of diethylene glycol and 25mL of ethanol into a 50mL round-bottom flask and reflux at 100℃ for 3 hours. After cooling, centrifugation, drying and grinding, put it into a quartz boat and heat it to 650℃ at a heating rate of 10℃ / min in a nitrogen atmosphere in a tubular furnace for 3h. After cooling and grinding, a thin layer of porous carbon nitride can be obtained.
[0052] Under standard conditions, the photocatalytic conversion rate of 2,3-diphenyl-2,3-butanediol by the thin layer porous carbon nitride prepared in this example was 95.6%, the yield of benzaldehyde was 51.2%, and the yield of benzoic acid was 40.7%.
[0053] Example 5: A method for preparing a thin layer of porous carbon nitride is as follows:
[0054] The specific steps are as follows: weigh 1g of melamine and 1g of cyanuric acid and add them to 80mL of deionized water. After stirring in an 80℃ oil bath for 30min, pour them into a stainless steel reactor with polytetrafluoroethylene for hydrothermal reaction. The temperature of the hydrothermal reaction is 140℃ and the insulation time is 24h. The solution in the reactor is filtered, washed, dried and ground to obtain a tubular precursor. Weigh 0.4g of tubular precursor, 5mL of diethylene glycol and 5mL of ethanol into a 50mL round-bottom flask and reflux at 80℃ for 5 hours. After cooling, centrifugation, drying and grinding, put it into a quartz boat and heat it to 500℃ at a heating rate of 5℃ / min in an argon atmosphere in a tubular furnace for 5h. After cooling and grinding, a thin layer of porous carbon nitride can be obtained.
[0055] Under standard conditions, the photocatalytic conversion rate of 1,2-bis(4-chlorophenyl)ethane-1,2-diol by the thin layer porous carbon nitride prepared in this example was 91.8%, the yield of p-chlorobenzaldehyde was 48.3%, and the yield of p-chlorobenzoic acid was 40.2%.
[0056] Example 6: A method for preparing a thin layer of porous carbon nitride is as follows:
[0057] The specific steps are as follows: weigh 1g of melamine and 1.4g of cyanuric acid and add them to 80mL of deionized water. After stirring in an 80℃ oil bath for 30min, pour them into a stainless steel reactor with polytetrafluoroethylene for hydrothermal reaction. The temperature of the hydrothermal reaction is 170℃ and the insulation time is 16h. The solution in the reactor is filtered, washed, dried and ground to obtain a tubular precursor. Weigh 0.7g of tubular precursor, 5mL of diethylene glycol and 15mL of ethanol into a 50mL round-bottom flask and reflux at 95℃ for 4 hours. After cooling, centrifugation, drying and grinding, put it into a quartz boat and heat it to 600℃ at a heating rate of 8℃ / min in a helium atmosphere in a tubular furnace for 4h. After cooling and grinding, a thin layer of porous carbon nitride can be obtained.
[0058] Under standard conditions, the photocatalytic conversion rate of 1,2-di-p-tolylethane-1,2-diol by the thin layer porous carbon nitride prepared in this example was 87.3%, the yield of p-tolualdehyde was 42.6%, and the yield of p-toluic acid was 40.4%.
[0059] Example 7: A method for preparing a thin layer of porous carbon nitride is as follows:
[0060] Weigh 1g of melamine and 1.1g of cyanuric acid and add them to 80mL of deionized water. After stirring in an 80℃ oil bath for 30min, pour them into a stainless steel reactor with polytetrafluoroethylene for hydrothermal reaction. The temperature of the hydrothermal reaction is 150℃ and the insulation time is 12h. The solution in the reactor is filtered, washed, dried and ground to obtain a tubular precursor. Weigh 0.5g of tubular precursor, 10mL of diethylene glycol and 10mL of ethanol into a 50mL round-bottom flask and reflux at 85℃ for 4 hours. After cooling, centrifugation, drying and grinding, put it into a quartz boat and heat it to 550℃ at a heating rate of 10℃ / min in a nitrogen atmosphere in a tubular furnace for 5h. After cooling and grinding, a thin layer of porous carbon nitride can be obtained.
[0061] Under standard conditions, the photocatalytic conversion rate of 1,2-di(furan-2-yl)ethane-1,2-diol by the thin layer porous carbon nitride prepared in this example was 97.6%, the yield of furan-2-carboxaldehyde was 61.3%, and the yield of furan-2-carboxylic acid was 30.2%.
[0062] Example 8: The preparation method of thin layer porous carbon nitride is as follows:
[0063] The specific steps are as follows: weigh 1g of melamine and 1.5g of cyanuric acid and add them to 80mL of deionized water. After stirring in an 80℃ oil bath for 30min, pour them into a stainless steel reactor with polytetrafluoroethylene for hydrothermal reaction. The temperature of the hydrothermal reaction is 160℃ and the insulation time is 18h. The solution in the reactor is filtered, washed, dried and ground to obtain a tubular precursor. Weigh 0.6g of tubular precursor, 10mL of diethylene glycol and 15mL of ethanol into a 50mL round-bottom flask and reflux at 90℃ for 2 hours. After cooling, centrifugation, drying and grinding, put it into a quartz boat and heat it to 550℃ at a heating rate of 5℃ / min in a nitrogen atmosphere in a tubular furnace for 5h. After cooling and grinding, a thin layer of porous carbon nitride can be obtained.
[0064] Under standard conditions, the photocatalytic conversion rate of 1-phenylethane-1,2-diol by the thin layer porous carbon nitride prepared in this example was 67.8%, the yield of benzaldehyde was 46.3%, and the yield of benzoic acid was 17.2%.
[0065] Comparative Example 1: Carbon nitride photocatalyst was prepared as follows:
[0066] 10 g of melamine was weighed, ground evenly and added to a 50 mL crucible. The crucible was placed in a muffle furnace and heated to 550 ° C at a heating rate of 10 ° C / min and kept at this temperature for 4 hours. After cooling and grinding, the carbon nitride photocatalyst CN prepared by the traditional method was obtained.
[0067] Under standard conditions, the photocatalytic conversion rate of 1,2-diphenylethylene glycol by the carbon nitride photocatalyst was 32.4%, the yield of benzaldehyde was 21.6%, and the yield of benzoic acid was 8.2%.
[0068] The carbon nitride prepared in Example 1 and Comparative Example 1 was used as a sample, and XRD test, Fourier transform infrared spectroscopy test, photocurrent measurement, impedance measurement, Mott-Schottky test and photoluminescence spectroscopy test were performed respectively. The results are as follows: Figure 2-7 shown.
[0069] Comparative Example 2: Carbon nitride photocatalyst was prepared as follows:
[0070] 10g of urea was weighed, ground evenly and added to a 50mL crucible. The crucible was placed in a muffle furnace and heated to 550℃ at a heating rate of 10℃ / min and kept at this temperature for 4h. After cooling and grinding, a light yellow carbon nitride photocatalyst was obtained.
[0071] Under standard conditions, the carbon nitride photocatalyst has a photocatalytic conversion rate of 1,2-diphenylethylene glycol of 46.3%, a yield of benzaldehyde of 31.6%, and a yield of benzoic acid of 9.7%.
[0072] Comparative Example 3: Carbon nitride photocatalyst was prepared as follows:
[0073] A method for preparing carbon nitride photocatalyst for the cleavage of CC bonds of aromatic vicinal diols with different substituents has been reported in the reference (ChemSusChem, 13(19)(2020):5248-5255.). The specific steps are as follows:
[0074] Disperse 40g of urea in a mixed solution of 60mL of 0.2mol / L HCl and 52mL of ethanol. Add 32mL of ethyl orthosilicate to the mixed solution under constant stirring. After continuous stirring at room temperature for 3h, remove the solvent by rotary evaporation, and then obtain a white solid powder after drying and grinding. In a N2 atmosphere, use a tubular furnace to heat up to 550℃ at a heating rate of 2.5℃ / min and keep warm for 4 hours. After cooling and grinding, a carbon nitride photocatalyst is obtained.
[0075] Under standard conditions, the carbon nitride photocatalyst achieved a 78.6% conversion rate of 1,2-diphenylethylene glycol, a 60.3% yield of benzaldehyde, and a 13.2% yield of benzoic acid.
[0076] Comparative Example 4: The rest is the same as Example 1, except that:
[0077] The mixture of 5 mL of diethylene glycol and 10 mL of ethanol was replaced with 15 mL of 5 M nitric acid aqueous solution.
[0078] Under standard conditions, the carbon nitride photocatalyst prepared in this example has a photocatalytic conversion rate of 1,2-diphenylethylene glycol of 34.8%, a yield of benzaldehyde of 14.8%, and a yield of benzoic acid of 17.1%.
[0079] This comparative example shows that the selection of the reflux liquid is crucial to the catalytic activity of the carbon nitride photocatalyst, and the conventional strong acid reflux treatment cannot obtain a carbon nitride product with high catalytic activity.
[0080] Comparative Example 5: The rest is the same as Example 1, except that:
[0081] The tubular precursor was first calcined, and then the calcined product was refluxed with 5 mL of diethylene glycol and 10 mL of ethanol. The parameters of the calcination step and the reflux step were the same as those in Example 1.
[0082] Under standard conditions, the carbon nitride photocatalyst prepared in this example has a photocatalytic conversion rate of 1,2-diphenylethylene glycol of 45.5%, a yield of benzaldehyde of 32.8%, and a yield of benzoic acid of 10.7%.
[0083] This comparative example shows that only by calcining the tubular precursor after reflux stripping can a suitable product microstructure be formed, thereby obtaining a better photocatalytic effect. Otherwise, the catalytic effect of the catalyst will be greatly reduced.
[0084] Comparative Example 6: Under standard conditions, the thin layer of porous carbon nitride prepared in Examples 1-8 was used to photocatalyze 1,2-diphenylethane and bisphenol F, respectively. The results are as follows:
[0085] Table 1 Photocatalytic conversion effect of thin layer porous carbon nitride on 1,2-diphenylethane and bisphenol F
[0086]
[0087] From the results in Table 1, it can be seen that the thin layer porous carbon nitride in the present invention has a high catalytic selectivity for CC bonds in aromatic vicinal diols, but has a low catalytic activity for CC bonds in 1,2-diphenylethane and bisphenol F, and cannot be used for the CC bond breaking catalytic reaction of these substances.
[0088] It can be seen from the above comparative examples that the method for preparing a thin layer of porous carbon nitride described in the present invention is significantly better than the performance of photocatalysts prepared in reported Chinese patents and literature in catalytically cleaving CC bonds in aromatic vicinal diols. The method for preparing a thin layer of porous carbon nitride provided by the present invention and its application in the reaction of photocatalytically cleaving CC bonds in aromatic vicinal diols has excellent substrate catalytic activity, excellent reaction efficiency and product yield, and the thin layer of porous carbon nitride catalyst has high reusability.
Claims
1. A method for preparing a thin layer of porous carbon nitride, characterized in that: The steps include: (1) hydrothermally reacting melamine and cyanuric acid to obtain a tubular precursor; (2) using an alcohol reflux solution to strip the tubular precursor to obtain an intermediate; (3) Calcination of the intermediate to obtain a thin layer of porous carbon nitride.
2. The method for preparing a thin layer of porous carbon nitride according to claim 1, characterized in that: In step (1), the hydrothermal reaction method is: adding melamine and cyanuric acid into water and mixing them evenly, carrying out hydrothermal reaction at 140-180° C. for 6-24 hours, and obtaining a tubular precursor through cooling, filtering, washing and drying.
3. The method for preparing a thin layer of porous carbon nitride according to claim 2, characterized in that: In step (1), the mass ratio of melamine to cyanuric acid is 1:1-1.
5.
4. The method for preparing a thin layer of porous carbon nitride according to claim 1, characterized in that: In step (2), the stripping of the tubular precursor using an alcohol reflux solution comprises the following steps: (21) mixing diethylene glycol and ethanol to obtain a reflux liquid or using only diethylene glycol as the reflux liquid; (22) The tubular precursor is added to a reflux liquid to obtain a suspension, and the suspension is refluxed to obtain an intermediate.
5. The method for preparing a thin layer of porous carbon nitride according to claim 4, characterized in that: In step (21), the volume ratio of diethylene glycol to ethanol is 1:1-5.
6. The method for preparing a thin layer of porous carbon nitride according to claim 4, characterized in that: In step (22), the material-liquid ratio of the tubular precursor to the reflux liquid is 0.4-0.8 g:10-30 mL, and the reflux conditions are: reflux at 80-100° C. for 1-5 h.
7. The method for preparing a thin layer of porous carbon nitride according to claim 1, characterized in that: In step (3), the calcination method is: in an inert gas atmosphere, the temperature is raised to 500-650° C. at a rate of 5-10° C. / min and kept at this temperature for 3-5 hours.
8. Use of the thin layer porous carbon nitride prepared according to the preparation method according to any one of claims 1 to 7 in photocatalytic cleavage of the CC bond of aromatic vicinal diols.
9. The use according to claim 8, characterized in that: The steps include: The catalyst is a thin layer of porous carbon nitride prepared by the preparation method according to any one of claims 1 to 7, wherein R1 and R2 are independently selected from substituted or unsubstituted aromatic groups, H, substituted or unsubstituted furanyl groups, R1 and R2 are not H at the same time, and the substituent group of the aromatic group is selected from halogen or C 1-3 Alkyl, wherein R3 and R4 are independently selected from methyl or H.
10. The method for preparing a thin layer of porous carbon nitride according to claim 9, characterized in that: The R1 and R2 are independently selected from phenyl, phenyl substituted with halogen or methyl, and furyl.
Citation Information
Patent Citations
Curly carbon nitride sheet and preparation method thereof, and application of curly carbon nitride sheet in photocatalytic decomposition of water into hydrogen
CN110882714A
Donor-acceptor unit modified porous ultrathin g-C3N4 tube photocatalyst as well as preparation method and application thereof
CN114558601A