Co-crystallization molecular sieve, catalyst, preparation method of co-crystallization molecular sieve and catalyst and application of co-crystallization molecular sieve in denitration
By preparing co-crystallized molecular sieves with topologies such as CHA, AEI, LTA, ERI, OFF, and KFI and loading them with active metals, the problem of insufficient hydrothermal stability of aluminum-rich copper-based molecular sieve catalysts was solved, achieving high-efficiency denitrification performance and long-life catalyst application.
Patent Information
- Application Number
- CN202410845487.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-11-01
AI Technical Summary
Existing aluminum-rich copper-based molecular sieve catalysts have shortcomings in hydrothermal stability, which limits their application in diesel vehicle exhaust denitrification systems.
Co-crystallized molecular sieves, including mixed crystal forms with topologies such as CHA, AEI, LTA, ERI, OFF, and KFI, are used. By mixing alkali sources, aluminum sources, silicon sources, and structure directing agents in specific proportions, molecular sieves with co-crystallized structures are prepared and loaded with active metals such as copper to form catalysts.
It improves the hydrothermal stability of the catalyst, maintains good denitrification performance, extends the service life of the catalyst, and meets the requirements of low-temperature activity and harsh hydrothermal environment.
Smart Images

Figure CN118874531A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalysts, and in particular relates to a co-crystallized molecular sieve, a catalyst, a preparation method and an application of the co-crystallized molecular sieve in denitration. Background Art
[0002] Selective catalytic reduction of ammonia to remove nitrogen oxides (NH 3 -SCR) is one of the most effective technologies for removing nitrogen oxides. Due to its excellent denitrification temperature window and outstanding hydrothermal stability, high-silicon Cu-SSZ-13 (Si / Al≥10) catalyst has been commercialized for diesel vehicle exhaust denitrification after-treatment system.
[0003] As the pollutants emitted by diesel vehicle exhaust during cold start-up become increasingly important, the requirements for the low-temperature activity of denitrification catalysts in diesel vehicle exhaust denitrification aftertreatment systems are becoming increasingly high. Acid sites show significantly better low-temperature activity than corresponding high-silicon molecular sieve catalysts, and thus have attracted extensive research attention. However, poor hydrothermal stability limits the industrial application of aluminum-rich copper-based molecular sieve catalysts. Summary of the invention
[0004] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a co-crystallized molecular sieve, a catalyst and a preparation method and application in denitration.
[0005] To achieve the above object, the technical solution adopted by the present invention is:
[0006] A co-crystallized molecular sieve, the topological structure of which includes any two or more of CHA, AEI, LTA, ERI, OFF, KFI, LEV, etc.; preferably, the dominant crystal form of the topological structure is a mixed crystal form of CHA / OFF-ERI.
[0007] The present invention also includes a method for preparing a co-crystallized molecular sieve, comprising the following steps: S1: dissolving an alkali source in water, adding an aluminum source, and continuing to stir until the solution is evenly mixed; S2: subsequently adding a structure directing agent, and continuing to stir until the solution is evenly mixed; S3: adding a silicon source, and continuing to stir until the solution is evenly mixed; S4: loading into a reactor, crystallizing, and after crystallization is completed, washing, drying, and roasting to obtain a powder of the co-crystallized molecular sieve.
[0008] The structure directing agent includes any two or more of 18-crown-6, strontium oxide, strontium nitrate, N,N,N-trimethyl-1-adamantanammonium hydroxide, N,N-dimethyl-3,5-dimethylpiperidinium hydroxide, 1,2-dimethyl-3-(4-methylbenzyl)-imidazole hydroxide, and diethyldimethylamine; preferably, it is a mixture of strontium oxide, 18-crown-6 and N,N,N-trimethyl-1-adamantanammonium hydroxide.
[0009] The molar ratio of silicon source, aluminum source, alkali source, structure directing agent and water is 1: (0.02-0.20): (0.075-0.4): (0.2-1.5): (50-200); preferably: 1: 0.1: 0.23: 1.1: 160.
[0010] The alkali source includes one or more of potassium hydroxide, sodium hydroxide, and cesium hydroxide;
[0011] Preferably, the aluminum source includes one or more of aluminum powder, aluminum hydroxide, and sodium aluminate;
[0012] Preferably, the silicon source includes one or more of sodium silicate, white carbon black, and silica sol.
[0013] The present invention also includes a catalyst, comprising the co-crystallized molecular sieve and an active metal loaded on the co-crystallized molecular sieve.
[0014] The mass content of the active metal is 0.5-7.0% of the catalyst content; preferably 1.5-4.5%.
[0015] The active metal is one or more of copper, iron, silver, cerium, lanthanum, samarium and cobalt.
[0016] The present invention also includes a method for preparing the catalyst, which adopts ion exchange, impregnation or solid phase grinding method.
[0017] The present invention also includes an application of the catalyst described in item 1 to eliminate nitrogen oxides and ammonia.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The co-crystallized molecular sieve of the present invention contains a variety of topological structures. The molecular sieve pores between the topological structures are staggered and stacked, which can effectively limit the removal of aluminum species. During the hydrothermal aging process, the aluminum atoms in the molecular sieve framework will be converted into Al(OH) 3 The form is removed from the framework and enters the molecular sieve pores. The dislocation of the molecular sieve pores makes the removed Al(OH) 3 It will be confined in the molecular sieve pores. During the cooling process after hydrothermal aging, the removed Al(OH) 3It will return to the molecular sieve framework, thereby effectively preventing the molecular sieve from dealumination and achieving higher hydrothermal stability.
[0020] The present invention constructs a molecular sieve with a co-crystallization structure by regulating the molecular sieve synthesis ratio and method, and prepares a corresponding catalyst using the molecular sieve as a carrier. The catalyst not only maintains the good denitration performance of the fresh sample, but also significantly inhibits the dealumination phenomenon during the hydrothermal aging process of the molecular sieve catalyst, improves the hydrothermal stability of the catalyst, and can meet the more stringent hydrothermal environment in actual working conditions, and has a longer service life. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 XRD patterns of Examples 1, 3, 4, 7, and 10;
[0022] Figure 2 is the SEM image of Example 1;
[0023] Figure 3 is the SEM image of Example 7;
[0024] Figure 4-6 Catalyst activity diagram. DETAILED DESCRIPTION
[0025] In order to enable those skilled in the art to better understand the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and the best embodiments.
[0026] Example 1
[0027] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0028] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of structure directing agent SDA and continue to stir until it is evenly mixed; S3: Add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S4: Finally, load the gel into a reactor and crystallize it at 150°C for 6 days; After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of CHA / OFF-ERI co-crystallized molecular sieve.
[0029] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :K 2 O:SrO:18-crown ether-6:N,N,N-trimethyl-1-adamantanammonium hydroxide:H 2 O=1:0.1:0.23:0.1:0.8:0.2:160, and its dominant crystal form is shown in Table 1.
[0030] Example 2
[0031] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0032] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of SDA and continue to stir until it is evenly mixed; S3: Add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S4: Finally, the gel is loaded into a reactor and crystallized at 160°C for 3 days. After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of AEI / KFI co-crystallized molecular sieve.
[0033] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :Na 2 O: 18-crown-6: N,N-dimethyl-3,5-dimethylpiperidinium hydroxide: H 2 O=1:0.2:0.4:0.3:0.5:100, and its dominant crystal form is shown in Table 1.
[0034] Example 3
[0035] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0036] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of SDA and continue to stir until it is evenly mixed; add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S3: Finally, the gel is loaded into a reactor and crystallized at 140°C for 4 days. After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of KFI / CHA co-crystallized molecular sieve.
[0037] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :Na 2 O: 18-crown ether-6: N,N,N-trimethyl-1-adamantanammonium hydroxide: H 2 O=1:0.05:0.1:0.5:0.5:80, and its dominant crystal form is shown in Table 1.
[0038] Example 4
[0039] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0040] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of SDA and continue to stir until it is evenly mixed; add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S3: Finally, put the gel into a reactor and crystallize it at 100°C for 6 days. After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of LEV / CHA co-crystallized molecular sieve.
[0041] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :Na 2 O: Diethyldimethylamine: N,N,N-trimethyl-1-adamantanammonium hydroxide: H 2 O=1:0.02:0.1:0.5:0.5:200, and its dominant crystal form is shown in Table 1.
[0042] Example 5
[0043] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0044] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of SDA and continue to stir until it is evenly mixed; add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S3: Finally, the gel is loaded into a reactor and crystallized at 180°C for 3 days. After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of LTA / AEI co-crystallized molecular sieve.
[0045] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :Na 2 O: 1,2-dimethyl-3-(4-methylbenzyl)-imidazole hydroxide: N,N-dimethyl-3,5-dimethylpiperidinium hydroxide: H 2 O=1:0.05:0.15:0.1:0.1:50, and its dominant crystal form is shown in Table 1.
[0046] Example 6
[0047] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0048] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of SDA and continue to stir until it is evenly mixed; add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S3: Finally, load the gel into a reactor and crystallize it at 180°C for 1 day. After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of LTA / LEV co-crystallized molecular sieve.
[0049] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :Na 2 O: 1,2-dimethyl-3-(4-methylbenzyl)-imidazolium hydroxide: diethyldimethylamine: H 2 O=1:0.05:0.1:0.75:0.75:80.
[0050] Example 7
[0051] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0052] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of structure directing agent SDA and continue to stir until it is evenly mixed; S3: Add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S4: Finally, load the gel into a reactor and crystallize it at 140°C for 6 days; After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of AEI / OFF-ERI co-crystallized molecular sieve.
[0053] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :Na 2 O:SrO:18-crown-6:N,N-dimethyl-3,5-dimethylpiperidinium hydroxide:H 2 O=1:0.1:0.2:0.1:0.7:0.3:200, and its dominant crystal form is shown in Table 1.
[0054] Example 8
[0055] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0056] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of structure directing agent SDA and continue to stir until it is evenly mixed; S3: Add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S4: Finally, load the gel into a reactor and crystallize it at 160°C for 4 days; After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of LEV / OFF-ERI co-crystallized molecular sieve.
[0057] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :Na 2 O:SrO:18-crown-6:diethyldimethylamine:H 2 O=1:0.15:0.2:0.1:0.5:0.5:100, and its dominant crystal form is shown in Table 1.
[0058] Example 9
[0059] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0060] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of SDA and continue to stir until it is evenly mixed; add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S3: Finally, the gel is loaded into a reactor and crystallized at 100°C for 6 days. After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of AEI / CHA / LEV co-crystallized molecular sieve.
[0061] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :Na 2 O: N,N-dimethyl-3,5-dimethylpiperidinium hydroxide: diethyldimethylamine: N,N,N-trimethyl-1-adamantanammonium hydroxide: H 2 O=1:0.1:0.1:0.5:0.5:0.5:200, and its dominant crystal form is shown in Table 1.
[0062] Example 10
[0063] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0064] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of SDA and continue to stir until it is evenly mixed; add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S3: Finally, load the gel into a reactor and crystallize it at 100°C for 6 days. After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of KFI / LEV / CHA co-crystallized molecular sieve.
[0065] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :Na 2 O: 18-crown ether-6: diethyldimethylamine: N,N,N-trimethyl-1-adamantanammonium hydroxide: H 2 O=1:0.1:0.01:0.5:0.5:0.5:200, and its dominant crystal form is shown in Table 1.
[0066] Embodiment 11
[0067] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0068] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of SDA and continue to stir until it is evenly mixed; add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S3: Finally, put the gel into a reactor and crystallize it at 100°C for 6 days. After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of AEI / KFI / CHA co-crystallized molecular sieve.
[0069] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :Na 2 O: N,N-dimethyl-3,5-dimethylpiperidinium hydroxide: 18-crown-6: N,N,N-trimethyl-1-adamantanammonium hydroxide: H 2 O=1:0.15:0.1:0.5:0.2:0.5:200, and its dominant crystal form is shown in Table 1.
[0070] Example 12
[0071] A method for preparing a co-crystallized molecular sieve, the main steps of which are as follows:
[0072] S1: Weigh a certain proportion of alkali source and dissolve it in distilled water. After it is completely dissolved, add a certain amount of aluminum source and continue to stir until the solution is evenly mixed; S2: Then add a certain proportion of SDA and continue to stir until it is evenly mixed; add an appropriate amount of silicon source and continue to stir until it is evenly mixed; S3: Finally, the gel is loaded into a reactor and crystallized at 100°C for 6 days. After the crystallization is completed, the solid is washed, dried and calcined to obtain the powder of AEI / KFI / LEV co-crystallized molecular sieve.
[0073] The molar ratio of each substance in the gel is SiO 2 :Al 2 O 3 :Na 2 O:K 2 O: N,N-dimethyl-3,5-dimethylpiperidinium hydroxide: 18-crown-6: diethyldimethylamine: H 2 O=1:0.1:0.1:0.5:0.3:0.5:200, and its dominant crystal form is shown in Table 1.
[0074] Table 1
[0075]
[0076]
[0077] Figure 1 is the XRD diagram of Examples 1, 3, 4, 7, and 10, Figure 2 is the SEM picture of Example 1, Figure 3 This is the SEM image of Example 7. The results show that a variety of co-crystallized molecular sieves can be prepared by adopting the implementation means of the present application.
[0078] Embodiment 13
[0079] The preparation steps of a co-catalyst are as follows:
[0080] Step 1: Use the molecular sieve obtained in Example 1-12 as a carrier, mix it with ammonium nitrate at a ratio of 1g / 100ml, exchange ammonia at 80°C for 4h, wash, filter and dry, and repeat 3 times to obtain an ammonium type molecular sieve.
[0081] Step 2: Mix the obtained ammonium molecular sieve with copper nitrate in a ratio of 1 / 100 ml, with a copper content of 1 wt%, exchange at 80° C. for 1-2 h, wash, filter, dry and calcine to obtain a Cu-based co-crystallized molecular sieve catalyst.
[0082] Step 3: The simulated gas composition: NO is 500ppm, NH 3 500ppm, water vapor volume fraction 5%, O 2 Volume fraction is 5%, N 2As balance gas, total gas flow rate 500ml / min, gas volume space velocity 120,000h -1 The hydrothermal aging treatment conditions and gas composition are as follows: temperature 800°C, water vapor volume fraction 10%, O 2 The volume fraction is 21%, N 2 As the balance gas, the total gas flow rate is 500ml / min.
[0083] Step 4: Test As shown in Table 1, the catalyst has a denitration activity of more than 90% at 200-600°C, especially the catalyst obtained in Example 1, which has a denitration activity of more than 95% at 200-600°C; at the same time, the catalysts prepared in different embodiments, after hydrothermal aging at 800°C for 16h, the denitration activity of the catalyst exceeds 80% only in the temperature range of 225-500°C. Figure 4-6 They are the activity diagrams of the catalysts obtained in Examples 1, 5 and 11 respectively.
[0084] In summary, the co-crystallized molecular sieve of the present invention contains a variety of topological structures. The molecular sieve pores between the topological structures are staggered and stacked, which can effectively limit the removal of aluminum species. During the hydrothermal aging process, the aluminum atoms in the molecular sieve framework will be converted into Al(OH) 3 The form is removed from the framework and enters the molecular sieve pores. The dislocation of the molecular sieve pores makes the removed Al(OH) 3 It will be confined in the molecular sieve pores. During the cooling process after hydrothermal aging, the removed Al(OH) 3 It will return to the molecular sieve framework, thereby effectively preventing the molecular sieve from dealumination and achieving higher hydrothermal stability.
[0085] The present invention constructs a molecular sieve with a co-crystallization structure by regulating the molecular sieve synthesis ratio and method, and prepares a corresponding catalyst using the molecular sieve as a carrier. The catalyst not only maintains the good denitration performance of the fresh sample, but also significantly inhibits the dealumination phenomenon during the hydrothermal aging process of the molecular sieve catalyst, improves the hydrothermal stability of the catalyst, and can meet the more stringent hydrothermal environment in actual working conditions, and has a longer service life.
[0086] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A co-crystallized molecular sieve, It is characterized in that The topological structure includes any two or more of CHA, AEI, LTA, ERI, OFF, KFI, LEV, etc.; preferably, it is a mixed crystal form of CHA / OFF-ERI.
2. A method for preparing the cocrystallized molecular sieve according to claim 1, It is characterized in that The method comprises the following steps: S1: dissolving an alkali source in water, adding an aluminum source, and continuing to stir until the solution is evenly mixed; S2: subsequently adding a structure directing agent, and continuing to stir until the solution is evenly mixed; S3: adding a silicon source, and continuing to stir until the solution is evenly mixed; S4: loading into a reaction kettle, crystallizing, and after the crystallization is completed, washing, drying, and roasting to obtain powder of the co-crystallized molecular sieve.
3. The preparation method according to claim 2, It is characterized in that The structure directing agent includes any two or more of 18-crown ether-6, strontium oxide, strontium nitrate, N,N,N-trimethyl-1-adamantanammonium hydroxide, N,N-dimethyl-3,5-dimethylpiperidinium hydroxide, 1,2-dimethyl-3-(4-methylbenzyl)-imidazole hydroxide, and diethyldimethylamine.
4. The preparation method according to claim 2, It is characterized in that The molar ratio of silicon source, aluminum source, alkali source, structure directing agent and water is 1: (0.02-0.20): (0.075-0.4): (0.2-1.5): (50-200); preferably: 1: 0.1: 0.23: 1.1:
160.
5. The preparation method according to claim 2, It is characterized in that The alkali source includes one or more of potassium hydroxide, sodium hydroxide, and cesium hydroxide; Preferably, the aluminum source includes one or more of aluminum powder, aluminum hydroxide, and sodium aluminate; Preferably, the silicon source includes one or more of sodium silicate, white carbon black, and silica sol.
6. A catalyst, It is characterized in that It comprises the co-crystallized molecular sieve as claimed in claim 1 and an active metal loaded on the co-crystallized molecular sieve.
7. The catalyst according to claim 6, It is characterized in that The mass content of the active metal is 0.5-7.0% of the catalyst content; preferably 1.5-4.5%.
8. The catalyst according to claim 6, It is characterized in that The active metal is one or more of copper, iron, silver, cerium, lanthanum, samarium and cobalt.
9. A method for preparing the catalyst according to any one of claims 6 to 8, It is characterized in that Prepared by ion exchange, impregnation or solid phase grinding method.
10. Use of the catalyst according to any one of claims 6 to 8, It is characterized in that Applied to the elimination of nitrogen oxides and ammonia.
Citation Information
Patent Citations
Preparation method and application of active component of SCR (Selective Catalytic Reduction) catalyst
CN109759128A
Preparation method of silicon-aluminum-type AEI / CHA symbiotic molecular sieve catalyst and application of catalyst in selective catalytic reduction (SCR) catalysis
CN110422856A
Symbiotic composite molecular sieve with AEI / KFI structure as well as preparation method and SCR application thereof
CN111001436A
CHA-OFF-ERI symbiotic structure molecular sieve, preparation method thereof, catalyst thereof and application of catalyst