Porous ionic liquid containing supported high-entropy metal oxide as well as preparation method and application of porous ionic liquid

By combining the supported high-entropy metal oxide with room temperature ionic liquid, a porous ionic liquid with high active sites and high porosity was prepared, which solved the problem of uneven exposure of active sites of high-entropy alloy oxide catalysts, and achieved the goal of The efficient removal of aromatic sulfides and the improvement of catalytic activity.

CN118874535AActive Publication Date: 2024-11-01JIANGSU UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410900794.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-05
Publication Date
2024-11-01
Estimated Expiration
2044-07-05

AI Technical Summary

Technical Problem

Uneven exposure of active sites of high-entropy alloy oxide catalysts and difficulty in molecular mass transfer leads to insufficient catalytic activity of the oxidation reaction.

Method used

The loaded high-entropy metal oxide is combined with room temperature ionic liquid, and porous ionic liquid is prepared through high-temperature calcination and magnetic stirring. The high specific surface area of ​​SBA-15 molecular sieve and the hydrophilic properties of the ionic liquid are used to form high-active sites. and porous ionic liquids with high porosity.

Benefits of technology

It significantly improves catalytic activity, overcomes the problem of insufficient exposure of active sites, and shows excellent removal ability and good cycling performance when extracting coupled catalytic oxidation to remove organic sulfides in fuel oil.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874535A_ABST
    Figure CN118874535A_ABST
Patent Text Reader

Abstract

The invention discloses a supported high-entropy metal oxide-containing porous ionic liquid and a preparation method and application thereof, five subgroup non-noble metal salts are dissolved in water to obtain a mixed aqueous solution of metal salts; adding a molecular sieve SBA-15 into the mixed aqueous solution, and fully stirring to obtain a turbid liquid; heating the turbid liquid at a constant temperature, evaporating to dryness, grinding, washing with deionized water, centrifuging and drying to obtain loose solid powder; carrying out high-temperature calcination treatment on the solid powder in a protective atmosphere to obtain a supported high-entropy metal oxide; and finally, uniformly dispersing the obtained supported high-entropy metal oxide into the ionic liquid to obtain the catalyst. The porous ionic liquid is not only an extraction agent, but also a catalyst. The barrier that only the steric hindrance among molecules is utilized to construct the porous ionic liquid is broken through, and the porous ionic liquid shows excellent removal capacity on aromatic sulfides and good cycle performance of the catalyst in an ECODS system.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of catalytic material preparation, and in particular to a porous ionic liquid containing a supported high-entropy metal oxide, and a preparation method and application thereof. Background Art

[0003] There are many aromatic sulfides in fuel oil, such as thiophene, benzothiophene, dibenzothiophene and its derivatives, which have stable conjugated structures and are difficult to remove using traditional hydrodesulfurization (HDS) processes. At present, the existing new desulfurization methods include adsorption desulfurization (ADS), extraction desulfurization (EDS), oxidation desulfurization (ODS) and biological desulfurization (BDS). Among them, ODS has been favored by many scientists because it can more effectively remove aromatic sulfides. However, there are oil oxidation side reactions in the oxidation desulfurization reaction, and it is difficult to separate the oil from the catalyst. Therefore, the extraction coupled catalytic oxidation (ECODS) process combines the extraction and oxidation desulfurization two-phase system, extracts the oil phase sulfides into the extractant through a liquid extractant, and uses a catalyst in an oxygen-containing environment to accelerate the oxidation desulfurization rate. This is considered to be a promising method. The key lies in designing a catalyst that has both extraction and oxidation desulfurization capabilities.

[0004] Ionic liquids (ILs) are organic molten salts composed of organic cations and organic (inorganic) anions with high ionic conductivity, solubility and stability, and exist in liquid form at room temperature. It is worth noting that ionic liquids are also key materials for preparing porous liquids using readily available porous solid materials. Porous ionic liquids (PILs) have obvious advantages in gas capture. Since the molecular size of ILs is too large to enter the voids of porous materials, the solute molecules are dried in the micropores and gas molecules can enter. It relies on sterics to create permanent micropores and gas capture capabilities. The use of different hydrophilic and hydrophobic properties of solvent molecules and porous solute molecules to construct PILs has also been proven to be a feasible and creative method in the present invention.

[0005] High entropy alloy oxides (HEOs) are composed of five or more metal cations and have the characteristics of high temperature stability. The ability to generate and control oxygen defects in various HEOs structures can improve the catalytic activity of various oxidation reactions. However, due to the diverse structures of HEOs and the difficulty in adjusting the morphology, the active sites of HEOs are exposed unevenly, and the catalytic advantages of HEOs as catalysts in oxidation reactions cannot be fully utilized. Summary of the invention

[0006] Purpose of the invention: The technical problem to be solved by the present invention is to provide a new method for constructing porous ionic liquids in view of the shortcomings of existing high entropy alloy oxide catalysts such as uneven exposure of active sites and difficulty in molecular mass transfer. A porous ionic liquid based on thermodynamics is designed using supported high entropy metal oxides and room temperature ionic liquids to significantly improve the catalytic activity.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:

[0008] A method for preparing a porous ionic liquid containing a supported high entropy metal oxide comprises the following steps:

[0009] (1) dissolving five sub-group non-noble metal salts in water to obtain a mixed aqueous solution of metal salts;

[0010] (2) adding molecular sieve SBA-15 to the mixed aqueous solution of step (1) and stirring thoroughly to obtain a suspension;

[0011] (3) heating the suspension in step (2) at a constant temperature to evaporate to dryness, grinding, washing with deionized water, centrifuging, and drying to obtain a loose solid powder;

[0012] (4) calcining the solid powder obtained in step (3) at high temperature in a protective atmosphere to obtain a supported high entropy metal oxide;

[0013] (5) uniformly dispersing the supported high entropy metal oxide obtained in step (4) into the ionic liquid to obtain.

[0014] Specifically, in step (1), the five sub-group non-noble metal salts are cobalt salt, iron salt, molybdenum salt, nickel salt and copper salt, and the total mass percentage of the five sub-group non-noble metal salts in the mixed aqueous solution is 1 to 15 wt%.

[0015] Specifically, in step (2), the molecular sieve SBA-15 is a commercial grade ordered hexagonal mesoporous silica molecular sieve with a pore size between 7 and 11 nm; the molecular sieve SBA-15 is mixed with the mixed aqueous solution in step (1) at a mass volume ratio of 0.1 to 0.5 g / ml.

[0016] Preferably, in step (2), the stirring speed is set to 500-800 rpm, and the mixture is stirred at 30-60° C. for 6-12 hours to obtain a suspension.

[0017] Preferably, in step (3), the temperature of the constant temperature heating evaporation is 80-100° C., the time is 24-48 hours, stirring is continuously performed during the evaporation process, and the stirring speed is set to 500-800 rpm.

[0018] Preferably, in step (3), every 0.01 to 0.05 g of solid powder is washed with 30 mL of deionized water, and after washing, the solid powder is centrifuged at a speed of 8000 to 10000 rpm, and the centrifugation time is set to 1 to 5 minutes.

[0019] Specifically, in step (4), the calcination treatment refers to heating to 500-800° C. at a rate of 2-10° C. / min in air or a protective atmosphere containing 1-30% oxygen, and calcining for 2-4 hours.

[0020] Preferably, in step (5), the ionic liquid is an ionic liquid containing a hydrophobic side chain, selected from any one of 1-butyl-3-trimethylimidazolium tetrafluoroborate, 1-octyl-3-trimethylimidazolium tetrafluoroborate, 1-butyl-3-trimethylimidazolium hexafluoroborate, and 1-octyl-3-trimethylimidazolium hexafluoroborate; the supported high entropy metal oxide and the ionic liquid containing a hydrophobic side chain are mixed in a mass ratio of 1:2 to 5, and the dispersion is performed by magnetic stirring, and the speed is set to 400 to 800 rpm.

[0021] Furthermore, the porous ionic liquid containing supported high entropy metal oxide prepared by the above preparation method is also within the protection scope of the present invention.

[0022] Furthermore, the present invention also claims to protect the use of the above-mentioned porous ionic liquid containing supported high entropy metal oxides in the removal of organic sulfides in fuel by extraction-coupled catalytic oxidation.

[0023] Beneficial effects:

[0024] (1) The supported high entropy metal oxide prepared by the present invention, on the one hand, utilizes the efficient activation ability of HEOs active sites for oxygen to enhance the molecular mass transfer rate, and on the other hand, utilizes the high specific surface area of ​​SBA-15 to highly disperse the characteristics of HEOs, thereby overcoming the defect of insufficient exposure of HEOs active sites.

[0025] (2) The present invention obtains a novel porous ionic liquid with high active sites, high porosity and high oxygen storage capacity based on the difference in hydrophilicity of the functional groups of the ionic liquid and the supported high entropy metal oxide. The obtained porous ionic liquid is both an extractant and a catalyst. It not only breaks through the barrier of constructing porous ionic liquids using only the steric hindrance between molecules, but also shows excellent removal ability for aromatic sulfides and good catalyst cycle performance in the ECODS system. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments, and the above and / or other advantages of the present invention will become more clear.

[0027] Figure 1 It is a schematic diagram of the synthesis of the supported high entropy metal oxide of the present invention.

[0028] Figure 2 1 are scanning electron microscope (SEM) and transmission electron microscope (TEM) images of the materials in Example 1. Among them, a is the SEM image of SBA-15, b is the SEM image of the supported high entropy metal oxide, c and d are TEM images of the supported high entropy metal oxide; e and f are element distribution images of the supported high entropy metal oxide.

[0029] Figure 3 It is the nitrogen adsorption-desorption curve and pore size distribution diagram of the material in Example 1.

[0030] Figure 4 1 is a Fourier transform infrared spectrum (FT-IR) graph and a thermogravimetric (TG) curve graph of the porous ionic liquid prepared in Example 1. DETAILED DESCRIPTION

[0031] The present invention can be better understood with reference to the following examples.

[0032] Example 1

[0033] (1) Weighing cobalt nitrate, iron nitrate, ammonium molybdate, nickel nitrate and copper nitrate, all metal salts are used in an amount of 0.01 mol, and mixing and dissolving all metal salts in deionized water to obtain a mixed aqueous solution of metal salts, so that the mass percentage of the metal salts in the mixed aqueous solution is 5 wt %;

[0034] (2) Add 1 g of molecular sieve SBA-15 to 10 mL of a mixed aqueous solution of metal salts, stir at 30 ° C for 6 hours, and set the rotation speed to 600 rpm to obtain a light yellow suspension;

[0035] (3) heating the suspension to dryness at 80° C., with the rotation speed set to 600 rpm, and grinding the evaporated solid to obtain a light yellow solid powder;

[0036] (4) washing the solid powder with deionized water and centrifuging, repeating this step three times to obtain a white suspension and drying to obtain a white loose solid powder;

[0037] (5) calcining the reaction mixture in air for 2 hours at a temperature of 550° C. and a heating rate of 5° C. / min to obtain a supported high entropy metal oxide.

[0038] (6) Take 0.05 g of the above-mentioned supported high entropy metal oxide and add it to 4 mL of ionic liquid 1-butyl-3-methylimidazolium tetrafluoroborate, and use a magnetic stirrer to evenly disperse it in the ionic liquid to obtain a porous ionic liquid.

[0039] Figure 1 It is a schematic diagram of the synthesis of the supported high entropy metal oxide of the present invention.

[0040] Figure 2 The following are scanning electron microscope (SEM) and transmission electron microscope (TEM) photos of the materials in Example 1.

[0041] Figure 2 a is a SEM image of the untreated molecular sieve SBA-15 in Example 1. It can be seen from the figure that the macroscopic morphology of SBA-15 is a rod-like structure with a radial size of 50 to 200 μm.

[0042] Figure 2 b is a SEM image of the molecular sieve after adding high entropy oxide in Example 1. It can be seen that the loading does not affect the morphology of the carrier molecular sieve.

[0043] Figure 2 cd are the lattice fringes of the loaded high entropy metal oxide under HRTEM. It can be seen from the figure that the loading has no effect on the pore structure of SBA-15.

[0044] Figure 2 ef is the element distribution diagram of the supported high entropy metal oxide in Example 1. It can be seen that the five metal elements are evenly distributed on SBA-15, indicating the formation of high entropy metal oxide.

[0045] Figure 3 is the nitrogen adsorption-desorption curve and pore size distribution diagram of the material in Example 1. Wherein:

[0046] Figure 3 a is the nitrogen adsorption-desorption curve and pore size distribution curve of SBA-15 before and after loading in Example 1. It can be seen that the loop of SBA-15 shows obvious H1 hysteresis loop in the relative pressure range of 0.6-0.9, indicating that SBA-15 has an ordered mesoporous structure. The isotherm of the supported high entropy metal oxide shows a typical mesoporous structure, which is the same as the information obtained from the isotherm of SBA-15.

[0047] Figure 3 b is the pore size distribution curve of Example 1, which shows that there are abundant mesopores in SBA-15 before and after loading, and the pore sizes are mostly in the range of 6-8 nm, which is consistent with the pore size range of the selected SBA-15.

[0048] Figure 4 1 is a Fourier transform infrared spectrum (FT-IR) and a thermogravimetric (TG) curve of the porous ionic liquid prepared in Example 1.

[0049] Figure 4a is a Fourier transform infrared spectrum (FT-IR) of the porous ionic liquid in Example 1. It can be seen from the figure that the addition of the supported high entropy metal oxide does not change the structure of the ionic liquid, proving that the supported high entropy metal oxide exists stably and uniformly in the ionic liquid after physical dispersion, and does not chemically react with the ionic liquid.

[0050] Figure 4 b is a thermogravimetric (TG) curve of the porous ionic liquid in Example 1. The results show that below 330°C, neither the ionic liquid nor the supported high entropy metal oxide has a significant mass loss, proving that they have good thermal stability within the temperature range. In addition, the addition of supported high entropy metal oxide has a very small effect on the thermal stability of the ionic liquid, which also confirms the excellent structural stability of the constructed porous ionic liquid environment.

[0051] Example 2

[0052] (1) Weighing cobalt nitrate, iron nitrate, ammonium molybdate, nickel nitrate and copper nitrate, all metal salts are used in an amount of 0.01 mol, and mixing and dissolving all metal salts in deionized water to obtain a mixed aqueous solution of metal salts, so that the mass percentage of the metal salts in the mixed aqueous solution is 5 wt %;

[0053] (2) Add 1 g of molecular sieve SBA-15 to 10 mL of a mixed aqueous solution of metal salts, stir at 30 ° C for 6 hours, and set the rotation speed to 600 rpm to obtain a light yellow suspension;

[0054] (3) heating the suspension to dryness at 80° C., with the rotation speed set to 600 rpm, and grinding the evaporated solid to obtain a light yellow solid powder;

[0055] (4) washing the solid powder with deionized water and centrifuging, repeating this step three times to obtain a white suspension and drying to obtain a white loose solid powder;

[0056] (5) calcining at a high temperature of 650° C. in an air atmosphere for 2 hours at a heating rate of 5° C. / min to obtain a supported high entropy metal oxide.

[0057] (6) Take 0.05 g of the above-mentioned supported high entropy metal oxide and add it to 4 mL of ionic liquid 1-butyl-3-methylimidazolium tetrafluoroborate, and use a magnetic stirrer to evenly disperse it in the ionic liquid to obtain a porous ionic liquid.

[0058] Example 3

[0059] (1) Weighing cobalt nitrate, iron nitrate, ammonium molybdate, nickel nitrate and copper nitrate, all metal salts are used in an amount of 0.01 mol, and mixing and dissolving all metal salts in deionized water to obtain a mixed aqueous solution of metal salts, so that the mass percentage of the metal salts in the mixed aqueous solution is 3 wt %;

[0060] (2) Add 1 g of molecular sieve SBA-15 to 10 mL of a mixed aqueous solution of metal salts, stir at 30 ° C for 6 hours, and set the rotation speed to 600 rpm to obtain a light yellow suspension;

[0061] (3) heating the suspension to dryness at 80° C., with the rotation speed set to 600 rpm, and grinding the evaporated solid to obtain a light yellow solid powder;

[0062] (4) washing the solid powder with deionized water and centrifuging, repeating this step three times to obtain a white suspension and drying to obtain a white loose solid powder;

[0063] (5) calcining the reaction mixture in air for 2 hours at a temperature of 550° C. and a heating rate of 5° C. / min to obtain a supported high entropy metal oxide.

[0064] (6) Take 0.05 g of the above-mentioned supported high entropy metal oxide and add it to 4 mL of ionic liquid 1-butyl-3-methylimidazolium tetrafluoroborate, and use a magnetic stirrer to evenly disperse it in the ionic liquid to obtain a porous ionic liquid.

[0065] Example 4

[0066] (1) Weighing cobalt nitrate, iron nitrate, ammonium molybdate, nickel nitrate and copper nitrate, all metal salts are used in an amount of 0.01 mol, and mixing and dissolving all metal salts in deionized water to obtain a mixed aqueous solution of metal salts, so that the mass percentage of the metal salts in the mixed aqueous solution is 10 wt%;

[0067] (2) Add 1 g of molecular sieve SBA-15 to 10 mL of a mixed aqueous solution of metal salts, stir at 30 ° C for 6 hours, and set the rotation speed to 600 rpm to obtain a light yellow suspension;

[0068] (3) heating the suspension to dryness at 80° C., with the rotation speed set to 600 rpm, and grinding the evaporated solid to obtain a light yellow solid powder;

[0069] (4) washing the solid powder with deionized water and centrifuging, repeating this step three times to obtain a white suspension and drying to obtain a white loose solid powder;

[0070] (5) calcining the reaction mixture in air for 2 hours at a temperature of 550° C. and a heating rate of 5° C. / min to obtain a supported high entropy metal oxide.

[0071] (6) Take 0.05 g of the above-mentioned supported high entropy metal oxide and add it to 4 mL of ionic liquid 1-butyl-3-methylimidazolium tetrafluoroborate, and use a magnetic stirrer to evenly disperse it in the ionic liquid to obtain a porous ionic liquid.

[0072] Example 5

[0073] (1) Weighing cobalt nitrate, iron nitrate, ammonium molybdate, nickel nitrate and iron nitrate, with the amount of all metal salts being 0.01 mol, and mixing and dissolving all metal salts in deionized water to obtain a mixed aqueous solution of metal salts, such that the mass percentage of the metal salts in the mixed aqueous solution is 5 wt %;

[0074] (2) Add 1 g of molecular sieve SBA-15 to 10 mL of a mixed aqueous solution of metal salts, stir at 30 ° C for 6 hours, and set the rotation speed to 600 rpm to obtain a light yellow suspension;

[0075] (3) heating the suspension to dryness at 80° C., with the rotation speed set to 600 rpm, and grinding the evaporated solid to obtain a light yellow solid powder;

[0076] (4) washing the solid powder with deionized water and centrifuging, repeating this step three times to obtain a white suspension and drying to obtain a white loose solid powder;

[0077] (5) calcining the reaction mixture in air for 2 hours at a temperature of 550° C. and a heating rate of 5° C. / min to obtain a supported high entropy metal oxide.

[0078] (6) 0.05 g of the above-mentioned supported high entropy metal oxide was added to 4 mL of ionic liquid 1-octyl-3-methylimidazolium tetrafluoroborate, and a magnetic stirrer was used to evenly disperse it in the ionic liquid to obtain a porous ionic liquid.

[0079] Examples 6-12

[0080] The porous ionic liquid obtained in Examples 1-5 was used in an extraction coupled catalytic oxidation process to remove sulfides from oil products. The following are the types of oil products simulating diesel and the set-up of the oxidation desulfurization experimental device:

[0081] The model oil is prepared by dissolving dibenzothiophene (DBT), 4,6-dimethyldibenzothiophene (4,6-DMDBT), and 4-methyldibenzothiophene (4-MDBT) in n-dodecane, and adding n-hexadecane as an internal standard.

[0082] 20 mL of a certain amount of simulated oil was transferred into a three-necked flask, 4 mL of the porous ionic liquid synthesized in the embodiment was added thereto, and the flask was placed in a 120°C constant temperature oil bath and connected to a condensation reflux device. Oxygen was continuously introduced into the system at an oxygen flow rate of 150 mL / min, and magnetic stirring was turned on at the same time. During the reaction, the sulfur content in the oil was quantitatively detected by a gas chromatograph, and the desulfurization rate was calculated according to the following formula.

[0083]

[0084] The experimental results are shown in Table 1.

[0085] Table 1

[0086]

[0087] It can be seen from Table 1 that the porous ionic liquids synthesized in all examples have good removal effects on sulfides in the model oil. Among them, the porous ionic liquid synthesized in Example 1 has the highest removal efficiency for dibenzothiophene (DBT) under the same conditions, and the removal efficiency is DBT>4-MDBT>4,6-DMDBT.

[0088] The present invention provides a porous ionic liquid containing a supported high entropy metal oxide and a preparation method and application thereof. There are many methods and approaches to implement the technical solution. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principles of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention. All components not specified in this embodiment can be implemented using existing technologies.

Claims

1. A method for preparing a porous ionic liquid containing a supported high entropy metal oxide, characterized in that: The steps include: (1) dissolving five sub-group non-noble metal salts in water to obtain a mixed aqueous solution of metal salts; (2) adding molecular sieve SBA-15 to the mixed aqueous solution of step (1) and stirring thoroughly to obtain a suspension; (3) heating the suspension in step (2) at a constant temperature to evaporate to dryness, grinding, washing with deionized water, centrifuging, and drying to obtain a loose solid powder; (4) calcining the solid powder obtained in step (3) at high temperature in a protective atmosphere to obtain a supported high entropy metal oxide; (5) uniformly dispersing the supported high entropy metal oxide obtained in step (4) into the ionic liquid to obtain.

2. The method for preparing a porous ionic liquid containing a supported high entropy metal oxide according to claim 1, characterized in that: In step (1), the five sub-group non-noble metal salts are cobalt salt, iron salt, molybdenum salt, nickel salt and copper salt respectively, and the total mass percentage of the five sub-group non-noble metal salts in the mixed aqueous solution is 1 to 15 wt%.

3. The method for preparing a porous ionic liquid containing a supported high entropy metal oxide according to claim 1, characterized in that: In step (2), the molecular sieve SBA-15 is a commercial grade ordered hexagonal mesoporous silica molecular sieve with a pore size between 7 and 11 nm; the molecular sieve SBA-15 is mixed with the mixed aqueous solution in step (1) at a mass volume ratio of 0.1 to 0.5 g / ml.

4. The method for preparing a porous ionic liquid containing a supported high entropy metal oxide according to claim 1, characterized in that: In step (2), the stirring speed is set to 500-800 rpm, and the mixture is stirred at 30-60° C. for 6-12 hours to obtain a suspension.

5. The method for preparing a porous ionic liquid containing a supported high entropy metal oxide according to claim 1, characterized in that: In step (3), the temperature of the constant temperature heating evaporation is 80-100° C., the time is 24-48 hours, and stirring is continuously performed during the evaporation process, and the stirring speed is set to 500-800 rpm.

6. The method for preparing a porous ionic liquid containing a supported high entropy metal oxide according to claim 1, characterized in that: In step (3), every 0.01 to 0.05 g of solid powder is washed with 30 mL of deionized water. After washing, the solid powder is centrifuged at a speed of 8000 to 10000 rpm, and the centrifugation time is set to 1 to 5 minutes.

7. The method for preparing a porous ionic liquid containing a supported high entropy metal oxide according to claim 1, characterized in that: In step (4), the calcination treatment refers to heating to 500-800° C. at a rate of 2-10° C. / min in air or a protective atmosphere containing 1-30% oxygen, and calcining for 2-4 hours.

8. The method for preparing a porous ionic liquid containing a supported high entropy metal oxide according to claim 1, characterized in that: In step (5), the ionic liquid is an ionic liquid containing a hydrophobic side chain, selected from any one of 1-butyl-3-trimethylimidazolium tetrafluoroborate, 1-octyl-3-trimethylimidazolium tetrafluoroborate, 1-butyl-3-trimethylimidazolium hexafluoroborate, and 1-octyl-3-trimethylimidazolium hexafluoroborate; the supported high entropy metal oxide and the ionic liquid containing a hydrophobic side chain are mixed in a mass ratio of (1:2 to 5), and the dispersion is performed by magnetic stirring, and the rotation speed is set to 400 to 800 rpm.

9. A porous ionic liquid containing a supported high entropy metal oxide prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the porous ionic liquid containing a supported high entropy metal oxide according to claim 9 for removing organic sulfides from fuel oil.

Citation Information

Patent Citations

  • Homogeneous catalyst and heterogeneous catalyst based on ionic liquid, and preparation methods and application thereof

    CN111804331A

  • Catalyst for preparing methylacrolein as well as preparation method and application of catalyst

    CN113828346A

  • Preparation and application of doped composite oxide catalyst

    CN114054100A

  • Homogeneous catalyst and heterogeneous catalyst based on ionic liquid, and preparation method therefor and use thereof

    WO2021114091A1