Wind power main shaft extrusion forming device and process

Through the perforation and extrusion process and pretreatment before and after forging, the loosening and shrinkage defects of the wind power spindle in the continuous casting billet are solved, the quality and production efficiency of the finished product are improved, and the production cost is reduced.

CN118875192APending Publication Date: 2024-11-01TONGYU HEAVY IND +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411093108.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

When the wind power spindle is used for continuous casting, metallurgical defects such as loosening and shrinkage holes are prone to occur when the diameter reaches more than 1000mm, resulting in low material yield and high production cost.

Method used

Using perforation and extrusion processes, the inner hole forming of the wind power spindle is achieved through molds and perforation needles. The perforation needle flows the material to the lower end of the mold under pressure, reducing internal hole defects, and inspects and seals the cracks and shrinkage holes before forging. Upsetting and WHF method are drawn to ensure welding of internal defects of the blank.

Benefits of technology

It effectively reduces the metallurgical defects of the raw materials of continuous casting billets, improves production efficiency, avoids meat shortage, and corrects the deformation of the flange and shaft body through corrective measures, improving the quality of the finished product.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118875192A_ABST
    Figure CN118875192A_ABST
Patent Text Reader

Abstract

The invention discloses a wind power main shaft extrusion forming device and process, and the forming device comprises a mold, the overall length of a mold cavity is larger than that of a wind power main shaft, the upper part of the mold cavity is provided with a part which is the same as the outer circumference of the wind power main shaft, and the lower part is used as a reserved space; the perforating needle is used for punching in the blank of the wind power main shaft and achieving the purpose of forming the wind power main shaft; the forming process comprises the following steps: forging a blank of the wind power main shaft into a cylindrical shape, putting the blank into a mold cavity, upsetting the blank by using an upsetting plate, and forcing the blank material to fill a flange part cavity; after the flange part is formed, a piercing needle is used for punching in the blank, and under the action of punching pressure, materials in an inner hole of the wind power spindle flow to the length direction of a shaft body at the lower end of the die, so that the wind power spindle is formed; the inner hole of the wind power main shaft is formed by adopting the perforating and extruding processes, the metallurgical defects of a continuous casting blank raw material are reduced, and the production efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of mechanical manufacturing, and in particular to a wind turbine main shaft extrusion forming device and process. Background Art

[0002] At present, wind turbine main shafts are mostly formed by forging steel ingots. When forging steel ingots, the water risers at both ends need to be cut off, resulting in a low yield rate of raw materials for wind turbine main shafts.

[0003] The continuous casting billet has no water riser, so all the materials can be used when forging the main shaft. In addition, the production cost of the continuous casting billet is lower than that of the steel ingot, so the use of the continuous casting billet to forge the main shaft can reduce the production cost. However, when the continuous casting billet is used to extrude the wind turbine main shaft, when the diameter of the continuous casting billet reaches more than 1000mm, the large-sized continuous casting billet is prone to defects such as looseness and shrinkage holes in the core during solidification and crystallization. Summary of the invention

[0004] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a wind turbine main shaft extrusion forming device and process, which realizes the inner hole forming of the wind turbine main shaft by using perforation and extrusion process, reduces the metallurgical defects of the raw materials of the continuous casting billet, and improves the production efficiency. In order to achieve the above purpose, the present invention is implemented by the following technical solutions:

[0005] In a first aspect, the present invention provides a wind turbine main shaft extrusion forming device, comprising:

[0006] The mold cavity is provided with an overall length greater than the wind turbine main shaft, the upper portion of the mold cavity has a portion identical to the outer circumference of the wind turbine main shaft, and the lower portion is used as a reserved space;

[0007] The punching needle is used to punch holes in the blank of the wind turbine main shaft and achieve the purpose of forming the wind turbine main shaft.

[0008] As a further implementation, the taper of the mold cavity and the taper of the piercing needle are both greater than 3°.

[0009] As a further implementation, the length of the reserved space at the lower portion of the mold cavity is 100 to 150 mm greater than the length of the wind turbine main shaft.

[0010] In a second aspect, the present invention provides a wind turbine main shaft extrusion forming process, which is processed by using a wind turbine main shaft extrusion forming device as described in the first aspect, and includes the following steps:

[0011] The blank of the wind turbine main shaft is forged into a cylindrical shape, placed in the mold cavity, and the blank is upset with an upset plate to force the blank material to fill the flange cavity;

[0012] After the flange part is formed, a punching needle is used to punch a hole in the blank. Under the punching pressure, the material in the inner hole of the wind turbine main shaft flows toward the length direction of the shaft body at the lower end of the mold, thereby forming the wind turbine main shaft.

[0013] As a further implementation method, before the billet is forged into a cylindrical shape, it is loaded into a furnace for heating. After being fully kept warm according to the ingot heating regulations based on the billet size, the ingot is subjected to one or more upsetting and WHF method elongation with a free forging press to ensure that the internal defects of the forged billet are eliminated.

[0014] As a further implementation method, before loading into the furnace, check whether there are any leaking cracks or shrinkage holes on both end surfaces of the billet. If there are any, the leaking cracks or shrinkage holes are sealed by spot welding.

[0015] As a further implementation method, if there is excess material after the blank material fills the flange cavity, it can be pressed down with narrow anvils one by one, first pressing the flange edge and finally pressing the flange center, forcing the material to flow to the lower end of the mold.

[0016] As a further implementation method, if the downward flow resistance of the material is large during punching, part of the material will flow back to the upper part, causing deformation of the flange and the shaft body. At this time, the wind turbine main shaft formed part is placed in a finishing mold for correction.

[0017] As a further implementation method, the bottom of the mold is formed last during punching, and the portion of the bottom that extends beyond the length of the wind turbine main shaft is cut off.

[0018] As a further implementation method, the weight of the tail of the blank after being placed in the mold should be greater than 20-30% of the weight of the wind turbine main shaft flange.

[0019] The beneficial effects of the present invention are as follows:

[0020] 1. The present invention adopts the perforation and extrusion process to realize the inner hole forming of the wind turbine main shaft. Since the perforation needle has a small effective area when punching, the material is more easily deformed under the condition of a certain pressure of the press, and the equivalent stress of the core is large, and the deformation is severe, which is conducive to the welding of defects. The core of the billet is a frequent site of shrinkage and cracks. When the perforation needle punches, the internal defects of the billet can be forged to the maximum extent, thereby reducing the metallurgical defects of the raw materials of the continuous casting billet.

[0021] 2. Before loading the billet into the furnace, check whether there are leaking cracks or shrinkage holes on both ends of the billet. If there are any, spot weld them to prevent further oxidation of the inner wall of the crack or shrinkage hole from contacting the air during heating, which will affect the effect of forging, compacting and welding defects. In addition, after the billet is heated and fully kept warm after loading into the furnace, the steel ingot is upset and stretched by the WHF method once or multiple times by a free forging press to ensure that the internal defects of the billet are forged.

[0022] 3. The bottom of the mold is formed last during punching. Due to the low temperature, the fluidity of the material deteriorates, and it is difficult to completely fill the mold, which is prone to lack of meat. The length of the mold cavity of the present invention is greater than the length of the wind turbine main shaft blank. During extrusion, part of the material enters the reserved space. After the extrusion forming is completed, the excess part can be cut off, which solves the problem of lack of meat.

[0023] 4. When punching, if the material has a large downward flow resistance, some of the material will flow back to the upper part of the blank, causing the flange and the shaft body to deform. If deformation occurs, the present invention puts the wind turbine main shaft forming part into a finishing mold for correction. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0025] Figure 1 It is a schematic diagram of the extrusion forming die for the wind turbine main shaft in an embodiment of the present invention.

[0026] Figure 2 Schematic diagram of placing blank into a mold in an embodiment of the present invention.

[0027] Figure 3 It is a schematic diagram of the formation of the flange of the wind turbine main shaft in an embodiment of the present invention.

[0028] Figure 4 It is a schematic diagram of the final formation of the wind turbine main shaft in an embodiment of the present invention.

[0029] Figure 5 It is a schematic diagram of cutting the bottom of the wind turbine main shaft in an embodiment of the present invention.

[0030] Figure 6 It is a schematic diagram of the deformation of the wind turbine main shaft flange in an embodiment of the present invention.

[0031] Figure 7 It is a schematic diagram of the wind turbine main shaft flange trimming in an embodiment of the present invention.

[0032] In the figure: the distances or sizes between parts are exaggerated to show the positions of various parts, and the schematic diagram is for reference only.

[0033] Among them: 1. Press working platform; 2. Die; 3. Blank; 4. Upsetting plate; 5. Punching needle; 6. Wind turbine main shaft forming part; 7. Finishing lower die; 8. Finishing upper die. DETAILED DESCRIPTION

[0034] It should be noted that the following detailed descriptions are illustrative and intended to provide further explanation of the present invention. Unless otherwise specified, all technical and scientific terms used in the present invention have the same meanings as those commonly understood by those skilled in the art to which the present invention belongs.

[0035] Embodiment 1

[0036] In a typical embodiment of the present invention, reference is made to Figure 1 and Figure 4 As shown, a wind turbine main shaft extrusion forming device comprises:

[0037] The mold 2 has a mold cavity whose overall length is greater than the wind turbine main shaft. The upper portion of the mold cavity has a portion that is the same as the outer circumference of the wind turbine main shaft, and the lower portion is used as a reserved space. The mold 2 is placed on the press working platform 1 when working.

[0038] The length of the reserved space at the bottom of the mold cavity is 100-150mm longer than the length of the wind turbine main shaft. The bottom of the mold 2 is formed last during punching. Due to the low temperature, the material fluidity becomes poor, it is not easy to fill the mold completely, and it is easy to have a lack of meat. The length of the lower part of the mold cavity needs to be 100-150mm longer than the length of the wind turbine main shaft blank 3. This part is cut off after forging is completed.

[0039] The punching needle 5 is used to punch holes in the blank of the wind turbine main shaft and achieve the purpose of forming the wind turbine main shaft. Under the punching pressure, the material in the inner hole of the wind turbine main shaft flows in the length direction of the shaft body at the lower end of the mold 2, so that the wind turbine main shaft is formed to form a wind turbine main shaft formed part. Since the punching area of ​​the punching needle 5 is small, under the condition of a certain press pressure, the material is more easily deformed, the equivalent stress in the core is large, and the deformation is severe, which is conducive to the welding of defects. The core of the blank 3 is a frequent site of shrinkage holes and cracks. When the punching needle 5 is punched, the internal defects of the blank 3 can be forged to the maximum extent.

[0040] In this embodiment, the taper of the mold cavity and the taper of the piercing needle 5 are both greater than 3°, so as to facilitate the removal of the piercing needle 5 and the demoulding of the wind turbine main shaft formed part.

[0041] In this embodiment, the mold 2 and the punching needle 5 are both made of H13, 5CrN i Mo or higher quality hot working die steel, and are subjected to corresponding heat treatment to ensure that the comprehensive performance meets the requirements.

[0042] Embodiment 2

[0043] The present invention provides a wind turbine main shaft extrusion forming process, which is processed by using a wind turbine main shaft extrusion forming device as described in the first aspect, and comprises the following steps:

[0044] Before loading into the furnace, check whether there are any leaking cracks or shrinkage holes on both end surfaces of the billet 3 (the ingredients in this embodiment are continuous casting billets). If there are leaking cracks or shrinkage holes, they are spot welded and sealed to prevent further oxidation of the cracks or shrinkage holes when the inner wall is in contact with the air during heating, which affects the effect of forging, compacting and welding defects.

[0045] After the billet 3 is loaded into the furnace, it is heated to 1250°C. After being fully kept warm according to the ingot heating regulations according to the size of the billet 3, the ingot is subjected to one or more upsetting and WHF (Wide Die Heavy Blow Forging) stretching by a free forging press, that is, upper and lower wide flat anvils are used for forging during stretching, and the length of the billet pressed down each time is 0.6 to 0.1 times the thickness of the billet, and the amount of each pressing down is 20% of the thickness of the billet, so as to ensure that the internal defects of the billet 3 are forged.

[0046] The blank 3 is forged into a cylindrical shape, such as Figure 1 As shown, the diameter of the cylinder is smaller than the inner diameter D1 of the lower cone hole of the die, and larger than the inner diameter D2. If the blank 3 is too slender, a step can be forged according to the shape of the die cavity to ensure that the blank fits the inner wall of the die cavity as closely as possible, and prevent the blank 3 from tilting after being placed in the forging die.

[0047] like Figure 2 , it is necessary to ensure that the weight of part A after the blank is placed in the mold 2 is greater than 20-30% of the weight of the wind turbine main shaft flange.

[0048] like Figure 3 As shown, the blank 3 after blanking is reheated to 1250℃ and fully kept warm before being put into the mold 2, and the blank 3 is upset with the upsetting plate 4. If the pressure of the press is not enough, narrow anvils can be used to press down one by one. Since the inner diameter of the lower end gradually decreases from top to bottom, the downward flow resistance of the blank 3 material is large, forcing the blank 3 material to fill the flange part cavity.

[0049] If there is excess material after the blank 3 material fills the flange part cavity, it can be pressed down with narrow anvils one by one, first pressing the flange edge and finally pressing the flange center, forcing the blank 3 material to flow to the lower end of the mold.

[0050] like Figure 4 As shown, after the flange part of the wind turbine main shaft is formed, a punching needle 5 is used to punch a hole in the blank 3. Under the punching pressure, the material in the inner hole of the wind turbine main shaft flows toward the length direction of the shaft body at the lower end of the mold 2, thereby forming the wind turbine main shaft to form a wind turbine main shaft formed part 6.

[0051] If the blank 3 is long, it can be punched twice or more times to prevent the punching depth from being too deep at one time. If the punch is too long, the punch will be affected by the high temperature, the strength will be reduced, and it will become unstable, bent, and deformed. Since the punching area of ​​the punching needle 5 is small, under the condition of a certain press pressure, the material is more likely to deform, the equivalent stress in the core is large, and the deformation is severe, which is conducive to the welding of defects. The core of the blank 3 is a frequent location for shrinkage holes and cracks. When punching, the punching needle 5 can forge the internal defects of the blank 3 to the maximum extent.

[0052] The bottom of the die 2 is formed last during punching. Due to the low temperature, the material fluidity is poor, and it is not easy to fill the mold completely, which is prone to lack of meat. The length of the lower part of the die cavity is 100-150mm longer than the length of the wind turbine main shaft blank 3. This part is cut off after forging is completed. Figure 5 shown.

[0053] like Figure 6 As shown in the figure, when punching, if the material has a large downward flow resistance, some of the material will flow back to the upper part of the blank 3, causing the flange and the shaft to deform. Figure 7 As shown, if there is deformation after forming, the wind turbine main shaft formed part 6 is placed in a finishing mold for correction. The finishing mold includes a finishing lower mold 7 and a finishing upper mold 8.

[0054] In this embodiment, conventional forging measures such as applying lubricant and release agent to the mold 2 and the piercing needle 5 and adding carbon powder under the piercing needle during punching can be taken to reduce the difficulty of demolding and extracting the piercing needle after forming.

[0055] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A wind turbine main shaft extrusion forming device, characterized in that: include: The mold cavity is provided with an overall length greater than the wind turbine main shaft, the upper portion of the mold cavity has a portion identical to the outer circumference of the wind turbine main shaft, and the lower portion is used as a reserved space; The punching needle is used to punch holes in the blank of the wind turbine main shaft and achieve the purpose of forming the wind turbine main shaft.

2. A wind turbine main shaft extrusion forming device according to claim 1, characterized in that: The taper of the mold cavity and the taper of the piercing needle are both greater than 3°.

3. The wind turbine main shaft extrusion forming device according to claim 1, characterized in that: The length of the reserved space at the bottom of the mold cavity is 100 to 150 mm greater than the length of the wind turbine main shaft.

4. A wind turbine main shaft extrusion forming process, characterized in that: The wind turbine main shaft extrusion forming device according to any one of claims 1 to 3 is used for processing, comprising the following steps: The blank of the wind turbine main shaft is forged into a cylindrical shape, placed in the mold cavity, and the blank is upset with an upset plate to force the blank material to fill the flange cavity; After the flange part is formed, a punching needle is used to punch a hole in the blank. Under the punching pressure, the material in the inner hole of the wind turbine main shaft flows toward the length direction of the shaft body at the lower end of the mold, thereby forming the wind turbine main shaft.

5. A wind turbine main shaft extrusion forming process according to claim 4, characterized in that: Before the billet is forged into a cylindrical shape, it is loaded into a furnace for heating. After being fully kept warm according to the ingot heating regulations based on the billet size, the ingot is subjected to one or more upsetting and WHF method elongation with a free forging press to ensure that the internal defects of the forged billet are eliminated.

6. A wind turbine main shaft extrusion forming process according to claim 5, characterized in that: Before loading into the furnace, check whether there are any leaking cracks or shrinkage holes on both ends of the billet. If so, seal them by spot welding.

7. A wind turbine main shaft extrusion forming process according to claim 4, characterized in that: If there is excess material after the blank material fills the flange cavity, it can be pressed down with narrow anvils, first pressing the flange edge and finally the flange center, forcing the material to flow to the lower end of the mold.

8. The wind turbine main shaft extrusion forming process according to claim 4, characterized in that: When punching, if the downward flow resistance of the material is large, some of the material will flow back to the upper part, causing deformation of the flange and the shaft body. At this time, the wind turbine main shaft formed part is placed in the finishing mold for correction.

9. A wind turbine main shaft extrusion forming process according to claim 4, characterized in that: The bottom of the mold is formed last during punching, and the part of the bottom that extends beyond the length of the wind turbine main shaft is cut off.

10. The wind turbine main shaft extrusion forming process according to claim 4, characterized in that: After the blank is placed in the mold, the weight of the tail should be 20-30% greater than the weight of the wind turbine main shaft flange.