High-wear-resistance self-lubricating aluminum alloy extrusion die and preparation method
By using ductile iron materials and WC/Ni coatings in aluminum alloy extrusion molds, the problem of insufficient wear resistance and toughness of the mold is solved, high hardness, low friction and self-lubricating properties are achieved, and mold life is extended and reduced. Production cost.
Patent Information
- Application Number
- CN202410944961.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
AI Technical Summary
The wear resistance and toughness of existing aluminum alloy extrusion molds are insufficient, resulting in a short service life at high temperatures and cannot meet the production needs of aluminum alloy thermoforming.
Using ductile iron material, the tissue structure is regulated by adding alloy elements such as Ni, Mo, Cr and Mn, combined with heat treatment, to form carbides with high hardness and wear resistance, and apply WC/Ni coating on the surface of the mold to improve the anti-adhesion Aluminum, low friction and self-lubricating properties.
It significantly extends the service life of aluminum alloy extrusion molds, improves the hardness, wear resistance and toughness of the molds, reduces production costs, and improves the quality and production efficiency of aluminum alloy molded parts.
Smart Images

Figure CN118875650A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of thermal deformation die preparation, and in particular relates to a highly wear-resistant, self-lubricating aluminum alloy extrusion die, and also relates to a preparation method of the highly wear-resistant, self-lubricating aluminum alloy extrusion die. Background Art
[0002] Since the extrusion of aluminum alloy also belongs to the hot deformation forming of metal materials, the materials and manufacturing of the existing aluminum alloy extrusion dies follow the materials and manufacturing process of steel hot deformation dies, that is, aluminum alloy extrusion dies are all made of hot deformation die steel. However, due to the large differences between aluminum and steel in many properties, such as the hardness of Al is much lower than the hardness of steel at the same temperature, Al and Fe may form compounds at high temperatures, and the friction coefficient between aluminum alloy parts and the die surface is large, the failure form of the mold made of hot deformation die steel for hot extrusion of Al alloy is fundamentally different from that of hot forming steel; when the mold made of hot deformation die steel is used for hot forming steel parts, its failure is mainly caused by thermal fatigue leading to cracking of the mold surface and cracking of the mold; and when used for forming aluminum alloy parts, its failure is mainly caused by aluminum sticking to the mold surface, resulting in poor surface quality of aluminum products and size and shape not meeting the requirements, resulting in mold failure. The service life of the mold caused by this is also very different: the service life of aluminum alloy extrusion dies made of hot deformation die steel is much lower than that of forming steel. For example, when a mold made of hot-deformed die steel is used to form steel products, its service life can reach more than 100,000 times / set, while when the mold is used to form aluminum alloy products, its service life is even less than 20,000 times / set. Therefore, the development of molds and manufacturing technologies specifically for aluminum alloy hot forming has important practical significance and economic value for improving the service life of aluminum alloy hot deformation molds and reducing the production cost of aluminum alloy hot forming.
[0003] Ductile iron contains a large number of graphite balls. Under the drag of friction, the graphite balls will spread along the working surface, forming a graphite isolation layer between the contact surface of the mold and the workpiece, significantly reducing the friction and friction between the mold and the workpiece. At the same time, the formation of the graphite isolation layer can also significantly reduce the adhesion of the mold-molded aluminum alloy products to the mold. Therefore, aluminum alloy extrusion molds made of ductile iron are expected to solve the problem of premature failure of steel mold extrusion molding aluminum alloys due to aluminum adhesion. However, there is a contradiction between hardness and toughness in ductile iron, so that it has not been able to meet the requirements of hot extrusion molds in terms of high mechanical properties as a mold material. As a mold material, the most basic properties are high hardness and high wear resistance. In steel materials, high hardness and high wear resistance are generally achieved by regulating its organization, so that there are a large number of fine, dispersed carbides in the organization and the metal matrix is high-carbon martensite. Ductile iron is brittle and has poor toughness due to the presence of a large number of graphite nodules. If its metal matrix is a high-carbon martensite structure + a large amount of carbides, it will be even more brittle and cannot meet the toughness requirements of hot extrusion dies. By adjusting the properties of its metal matrix through heat treatment, the metal matrix is made of troostite or troostite. At this time, although ductile iron can meet the toughness requirements of hot extrusion dies, the hardness and wear resistance of troostite or troostite are worse than those of high-carbon martensite, so its hardness and wear resistance cannot meet the wear resistance and hardness requirements of extrusion dies. Therefore, the current aluminum alloy extrusion dies are basically not made of ductile iron materials.
[0004] Based on the above analysis, in order to use ductile iron with anti-adhesive aluminum, low friction and self-lubricating properties for the manufacture of aluminum alloy extrusion dies, how to overcome the contradiction between its high hardness, high wear resistance and toughness in mechanical properties, and achieve both high hardness, high wear resistance and appropriate toughness, is the key to making high-performance and long-life aluminum alloy extrusion dies with ductile iron materials. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing a highly wear-resistant, self-lubricating aluminum alloy extrusion die, which has excellent anti-adhesive aluminum performance, self-lubricating performance and toughness.
[0006] Another object of the present invention is to provide a highly wear-resistant, self-lubricating aluminum alloy extrusion die.
[0007] The technical solution adopted by the present invention is a method for preparing a highly wear-resistant, self-lubricating aluminum alloy extrusion die, which is specifically implemented according to the following steps:
[0008] Step 1: Casting aluminum alloy extrusion die blank;
[0009] Step 2: subjecting the aluminum alloy extrusion die blank to homogenization annealing treatment;
[0010] Step 3: machining the aluminum alloy extrusion die blank after homogenization annealing into an aluminum alloy extrusion die semi-finished product;
[0011] Step 4: quenching and tempering the machined aluminum alloy extrusion die semi-finished product;
[0012] Step 5: Grinding the quenched and tempered aluminum alloy extrusion die semi-finished product into an aluminum alloy extrusion die;
[0013] Step 6: Applying WC / Ni coating on the concave die working belt of the processed aluminum alloy extrusion die;
[0014] Step 7: The size and shape of the concave die of the aluminum alloy extrusion die coated with the WC / Ni coating are refined to obtain a highly wear-resistant, self-lubricating aluminum alloy extrusion die.
[0015] The present invention is also characterized in that:
[0016] In step 1, specifically:
[0017] The bread iron and scrap steel are heated to above 1500° C. to melt and obtain molten iron; according to the component requirements, 2.0%-2.5% nickel plate, 0.5%-1.0% ferrochrome, 2.5%-3.0% ferromolybdenum and 1.0%-1.5% ferrovanadium are weighed and added into the molten iron; the molten iron is inoculated and spheroidized with an inoculant and a spheroidizing agent; after the inoculation and spheroidization are completed, the molten iron is poured into a mold to cast an aluminum alloy extrusion die blank;
[0018] The cast aluminum alloy extrusion die blank includes the following components according to mass percentage: 2.4-3.0% Si, 3.3-3.7% C, 1.0-2.0% Ni, 1.50-2.50% Mo, 0.30-0.50% Cr, 0.50-0.80% V, 0.40-0.60% Mn, ≤0.1% P, 0.03-0.05% Mg 残留 , ≤0.02% S, the rest is Fe and unavoidable impurities.
[0019] In step 2, specifically:
[0020] The aluminum alloy extrusion die blank is heated to 1000-1050°C at a rate of 300-350°C / h and kept warm for 6-8h, then cooled to 500°C in the furnace, and then air-cooled to room temperature after being taken out of the furnace.
[0021] In step 4, the quenching process is: heating the machined aluminum alloy extrusion die semi-finished product to 900-950°C at a rate of 300-350°C / h and keeping it warm for 2-3h, and then air-cooling it to room temperature; the tempering process is: keeping it warm at 550-570°C for 2h, and repeating it twice.
[0022] In step 6, the coating thickness is 0.4-0.6 mm, and the coating width is 2-4 mm.
[0023] In step 6, during the WC / Ni coating process, the coating position of the mold needs to be heated to 550°C first, and then the coating is applied. After the coating is applied, the coated mold needs to be immediately placed in a heating furnace at 500°C for stress relief annealing for 4-6 hours.
[0024] Another technical solution adopted by the present invention is that a highly wear-resistant, self-lubricating aluminum alloy extrusion die is prepared by the above-mentioned preparation method.
[0025] The beneficial effects of the present invention are as follows: by designing the composition of ductile iron, adding alloy elements Ni, Mo, Cr and Mn that improve hardenability, and alloy elements Mo and V that can improve its hardness and wear resistance, firstly, a large number of fine graphite balls are realized in the cast structure, and the excellent anti-adhesive aluminum, low friction and self-lubricating properties of the ductile iron aluminum alloy extrusion die blank are ensured; then, by combining the regulation of the structure with heat treatment, the primary carbide in the cast structure is completely decomposed, and the carbide-forming elements Cr, Mo and V that can achieve high hardness and wear resistance of the material are completely dissolved in the metal matrix, and a large number of graphite balls are decomposed at the same time, further improving the anti-adhesive aluminum, low friction and self-lubricating properties of the material. Cr, Mo and V dissolved in the matrix are precipitated from the matrix again in the form of fine and dispersed carbides during the subsequent quenching and tempering process, improving the hardness and wear resistance of the mold, and significantly improving the toughness of the mold, so that the mold has excellent anti-adhesive aluminum, low friction, good self-lubricating properties and high hardness, good wear resistance and good toughness. Finally, a high-hardness WC / Ni coating with excellent wear resistance is applied to the working belt of the mold. By controlling the coating process, it is ensured that after the brittle ductile iron mold is coated with the coating, the mold and the coating will not produce cracks due to the stress generated in the mold by the heating and cooling of the mold during the coating process; and it is ensured that the coating is firmly combined with the ductile iron mold, so that the working surface of the mold has excellent wear resistance and high hardness, and finally the aluminum alloy extrusion mold is given the high hardness, excellent wear resistance, good toughness, high strength, excellent anti-adhesive aluminum ability, low friction coefficient and good self-lubricating performance required for service, which significantly extends the service life of the mold when extruding aluminum alloy products, improves the quality of aluminum alloy products extruded by the mold, and reduces the production cost of aluminum alloy products. It has significant economic benefits for the development of the aluminum alloy extrusion molding industry, and at the same time promotes the advancement of aluminum alloy extrusion molding technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is the cast metallographic structure diagram of the uncorroded mold blank;
[0027] Figure 2 It is the cast metallographic structure diagram of the corroded mold blank;
[0028] Figure 3 It is the metallographic structure diagram of the aluminum alloy extrusion die blank after pretreatment;
[0029] Figure 4 This is the metallographic structure diagram of the semi-finished aluminum alloy extrusion die after quenching;
[0030] Figure 5 This is the metallographic structure diagram of the semi-finished aluminum alloy extrusion die after quenching and then tempering twice;
[0031] Figure 6 This is the SEM image of the semi-finished aluminum alloy extrusion die after quenching and tempering twice.
[0032] Figure 7 It is a physical picture of the aluminum alloy extrusion die and the location of its coating. DETAILED DESCRIPTION
[0033] The present invention is described in detail below in conjunction with specific implementation modes and accompanying drawings.
[0034] The method for preparing the highly wear-resistant, self-lubricating aluminum alloy extrusion die of the present invention is specifically implemented according to the following steps:
[0035] Step 1: Casting aluminum alloy extrusion die blank: heating bread iron and scrap steel to above 1500°C to melt, and obtaining molten iron; weighing 2.0%-2.5% nickel plate, 0.5%-1.0% ferrochrome, 2.5%-3.0% ferromolybdenum, and 1.0%-1.5% ferrovanadium in mass fraction according to component requirements and adding them into the molten iron, and then adding 1.0%-1.5% inoculant (silicon-barium inoculant) and spheroidizer (silicon-iron rare earth magnesium alloy) in mass fraction to inoculate and spheroidize the molten iron, and after the inoculation and spheroidization is completed, pouring the treated molten iron into the mold to cast the aluminum alloy extrusion die blank;
[0036] The cast aluminum alloy extrusion die blank includes the following components according to mass percentage: 2.4-3.0% Si, 3.3-3.7% C, 1.0-2.0% Ni, 1.50-2.50% Mo, 0.30-0.50% Cr, 0.50-0.80% V, 0.40-0.60% Mn, ≤0.1% P, 0.03-0.05% Mg 残留 , ≤0.02% S, the rest is Fe and inevitable impurities; the metallographic structure of the blank is: metal matrix + a large number of fine and evenly distributed spherical graphite (graphite ball density is not less than 400 / mm 2 , ball diameter is about 20um) + coarse eutectic carbide.
[0037] Casting aluminum alloy extrusion die blanks with the above elemental composition has the following advantages compared to traditional ductile iron blanks. First, the Ni element contained in it can improve the hardenability of the die, and improve the hardness and strength of the die in the quenched state; on the other hand, Cr, Mo, and V elements can be used to improve the mechanical properties and high-temperature mechanical properties of the die through dispersion precipitation during heat treatment.
[0038] Step 2: subjecting the aluminum alloy extrusion die blank to homogenization annealing treatment;
[0039] Specifically: the aluminum alloy extrusion die blank is heated to 1000-1050℃ at a rate of 300-350℃ / h and kept warm for 6-8h, then cooled to 500℃ in the furnace, and then air-cooled to room temperature; the structure after annealing is: pearlite + a large number of fine graphite nodules.
[0040] Step 3: The aluminum alloy extrusion die blank after homogenization annealing is machined (by using a CNC machine tool according to the die size, with a size deviation of +0.5-1mm) into an aluminum alloy extrusion die semi-finished product;
[0041] Step 4: quenching and tempering the machined aluminum alloy extrusion die semi-finished product;
[0042] The quenching process is: heat the machined aluminum alloy extrusion die semi-finished product to 900-950℃ at a rate of 300-350℃ / h and keep it warm for 2-3h, then air cool it to room temperature. The structure after quenching is: high carbon martensite + a large amount of supercooled austenite + graphite nodules. The organization diagram is as follows: Figure 3 As shown;
[0043] The tempering process is: keep the temperature at 550-570℃ for 2h, repeat twice, the structure after tempering is: tempered troostite + dispersed fine alloy carbides containing (Mo, V and Cr) + graphite balls + a small amount of residual austenite, the hardness of the mold after tempering is not less than HRC48. The structure diagram after tempering is as follows Figure 4 As shown;
[0044] Step 5: Grinding the quenched and tempered aluminum alloy extrusion die semi-finished product into an aluminum alloy extrusion die (using a grinder to cut and grind the die to achieve the required size of the die, and the surface roughness Ra is required to be less than 0.8 μm);
[0045] Step 6: Applying WC / Ni coating on the concave die working belt of the processed aluminum alloy extrusion die;
[0046] When coating, laser cladding and thermal spraying methods can be used;
[0047] The coating is applied to the die working zone of the mold (such as Figure 7As shown); the coating thickness is 0.4-0.6mm, and the coating width is 2-4mm.
[0048] During the WC / Ni coating process, the coating position of the mold needs to be heated to 550°C before the coating can be applied. After the coating is applied, the coated mold needs to be immediately placed in a heating furnace at 500°C for stress relief annealing for 4-6 hours;
[0049] The advantage of WC / Ni coating is that WC can be used to improve the hardness of the coating, which is greater than 65HRC; Ni can be used to ensure the bonding strength between the coating and the mold and prevent the hardness coating from cracking. Therefore, WC / Ni coating can ensure high hardness of the coating and avoid cracking of the coating during operation. When selecting WC / Ni coating, the ratio of WC and Ni in the coating is 60%-70% by volume of WC, and the rest is Ni;
[0050] Step 7: The size and shape of the concave die of the aluminum alloy extrusion die coated with the WC / Ni coating are refined to obtain the aluminum alloy extrusion die.
[0051] The present invention achieves the goal of achieving a ductile iron material with anti-adhesive aluminum, low friction and self-lubricating properties with good toughness, high hardness and strength through component design and organizational regulation of the ductile iron material. The mold made of the ductile iron material is then surface treated (surface coated) to make its working surface have high hardness and high wear resistance. Finally, an aluminum alloy extrusion mold with excellent anti-adhesive aluminum performance, good self-lubricating performance, high wear resistance and good toughness is obtained. When the mold is used to extrude aluminum alloy materials, the service life of the mold extrusion-molded aluminum alloy is significantly extended, and the quality of aluminum alloy extrusion parts is improved, thereby significantly promoting the progress of aluminum alloy extrusion molding technology.
[0052] Figure 1 This is the cast metallographic structure diagram of the uncorroded mold blank. Figure 2 This is the cast metallographic structure diagram of the corroded mold blank. Figure 1 It can be seen that the as-cast structure contains a large amount of spheroidal graphite, and the number of spheroidal graphite is greater than 500 / mm 2 . Figure 2 It can be seen that the as-cast microstructure is mainly composed of spheroidal graphite, carbide, pearlite and ledeburite.
[0053] Example 1
[0054] The method for preparing a highly wear-resistant, self-lubricating aluminum alloy extrusion die of the present invention comprises the following steps:
[0055] Step 1: Casting of aluminum alloy extrusion die blank. The molten iron after inoculation and spheroidization treatment is poured into the mold to cast the aluminum alloy extrusion die blank first;
[0056] After step 1, the composition of the cast aluminum alloy extrusion die blank is: 2.4% Si, 3.7% C, 1.0 Ni, 1.50% Mo, 0.30% Cr, 0.50% V, 0.40% Mn, ≤0.1% P, 0.03% Mg 残留 , ≤0.02% S, the rest is Fe and unavoidable impurities; the corresponding metallographic structure of the blank is: metal matrix + a large number of fine and evenly distributed spherical graphite (graphite ball density is 480 / mm 2 , ball diameter is about 20um) + coarse eutectic carbide.
[0057] Step 2: Preheating of aluminum alloy die. Perform homogenization annealing on the aluminum alloy extrusion die blank;
[0058] The preheating treatment in step 2 is as follows: heating the blank to 1000°C at a rate of 300°C / h and keeping it at that temperature for 8h, then cooling it to 500°C in the furnace, and then air cooling it to room temperature after it is taken out of the furnace;
[0059] After step 2, the structure of the mold is: pearlite + a large number of fine graphite balls.
[0060] Step 3: Preparation of semi-finished aluminum alloy extrusion die. The aluminum alloy extrusion die blank after homogenization annealing is machined into a semi-finished aluminum alloy extrusion die;
[0061] Step 4: Final heat treatment of aluminum alloy extrusion die. The machined aluminum alloy extrusion die semi-finished product is quenched and tempered;
[0062] The heat treatment quenching process in step 4 is: heating the semi-finished mold to 900°C at a rate of 300°C / h and keeping it at that temperature for 2h, and then air cooling it to room temperature;
[0063] After quenching in step 4, the structure of the mold is: high carbon martensite + a large amount of undercooled austenite + graphite nodules;
[0064] The tempering process in step 4 is: 550°C for 2 hours, repeated twice;
[0065] After tempering in step 4, the structure of the mold is: tempered troostite + dispersed fine alloy carbides containing (Mo, V and Cr) + graphite nodules + a small amount of residual austenite. The hardness of the mold after tempering is HRC48.
[0066] Step 5: Finishing of aluminum alloy extrusion die. Grind the semi-finished aluminum alloy extrusion die that has been quenched and tempered into the final shape and size of the aluminum alloy extrusion die;
[0067] Step 6: Apply high hardness WC / Ni coating on the aluminum alloy extrusion die. Apply WC / Ni coating on the processed aluminum alloy extrusion die concave die working belt by laser coating;
[0068] In step 6, a high-hardness WC / Ni layer is applied, and various coating preparation technologies such as laser cladding and thermal spraying can be used. The coating is applied at the concave die working zone of the mold; the coating thickness is 0.4 mm and the coating width is 2 mm.
[0069] During the WC / Ni coating process in step 6, the coating position of the mold needs to be heated to 550°C before the coating can be applied. After the coating is applied, the coated mold needs to be immediately placed in a heating furnace at a temperature of 500°C for stress relief annealing for 4 hours.
[0070] Step 7: Obtaining the aluminum alloy extrusion die: The size and shape of the aluminum alloy extrusion die concave die coated with the WC / Ni coating are refined to obtain the final aluminum alloy extrusion die.
[0071] Example 2
[0072] The method for preparing the highly wear-resistant and self-lubricating aluminum alloy extrusion die of the present invention comprises the following steps:
[0073] Step 1: Casting of aluminum alloy extrusion die blank. The molten iron after inoculation and spheroidization treatment is poured into the mold to cast the aluminum alloy extrusion die blank first;
[0074] After step 1, the composition of the cast aluminum alloy extrusion die blank is: 3.0% Si, 3.3% C, 2.0% Ni, 2.50% Mo, 0.50% Cr, 0.80% V, 0.60% Mn, ≤0.1% P, 0.05% Mg 残留 , ≤0.02% S, the rest is Fe and inevitable impurities; the corresponding metallographic structure of the blank is: metal matrix + a large number of fine and evenly distributed spherical graphite (graphite ball density is 410 / mm 2 , ball diameter is about 20um) + coarse eutectic carbide.
[0075] Step 2: Preheating of aluminum alloy die. Perform homogenization annealing on the aluminum alloy extrusion die blank;
[0076] The preheating treatment in step 2 is as follows: the blank is heated to 1050°C at a rate of 350°C / h and kept at this temperature for 6 hours, then cooled to 500°C in the furnace, and then air-cooled to room temperature after being taken out of the furnace;
[0077] After step 2, the structure of the mold is: pearlite + a large number of fine graphite balls.
[0078] The metallographic structure of the mold blank after pretreatment, such as Figure 3 As shown, the black spheres are graphite spheres, and the gray matrix is pearlite;
[0079] Step 3: Preparation of semi-finished aluminum alloy extrusion die. The aluminum alloy extrusion die blank after homogenization annealing is machined into a semi-finished aluminum alloy extrusion die;
[0080] Step 4: Final heat treatment of aluminum alloy extrusion die. The machined aluminum alloy extrusion die semi-finished product is quenched and tempered;
[0081] The heat treatment quenching process in step 4 is: heating the semi-finished mold to 950°C at a rate of 350°C / h and keeping it warm for 3h, and then air cooling it to room temperature;
[0082] After quenching in step 4, the structure of the mold is: high carbon martensite + a large amount of undercooled austenite + graphite nodules;
[0083] The metallographic structure of the semi-finished mold after quenching, such as Figure 4 As shown, the black needle-shaped structure is martensite; the white block-shaped structure is supercooled austenite; the black spherical structure is graphite nodule;
[0084] The tempering process in step 4 is: 570℃ for 2h, repeated twice;
[0085] After tempering in step 4, the structure of the mold is: tempered troostite + dispersed fine alloy carbides containing (Mo, V and Cr) + graphite nodules + a small amount of residual austenite. The hardness of the mold after tempering is HRC50.
[0086] The metallographic structure diagram and SEM structure diagram of the semi-finished mold after quenching, such as Figure 5 and Figure 6 As shown, the fine white dispersed particles are carbides; the large blocks are retained austenite; the matrix is tempered troostite;
[0087] Step 5: Finishing of aluminum alloy extrusion die. Grind the semi-finished aluminum alloy extrusion die that has been quenched and tempered into the final shape and size of the aluminum alloy extrusion die;
[0088] Step 6: Apply high hardness WC / Ni coating on the aluminum alloy extrusion die. Apply WC / Ni coating on the processed aluminum alloy extrusion die concave die working belt by laser coating;
[0089] In step 6, a high-hardness WC / Ni layer is applied, and various coating preparation technologies such as laser cladding and thermal spraying can be used. The coating is applied at the concave die working zone of the mold; the coating thickness is 0.6 mm and the coating width is 4 mm.
[0090] During the WC / Ni coating process in step 6, the coating position of the mold needs to be heated to 550°C before the coating can be applied. After the coating is applied, the coated mold needs to be immediately placed in a heating furnace at a temperature of 500°C for stress relief annealing for 4 hours.
[0091] Step 7: Obtaining the aluminum alloy extrusion die: The size and shape of the aluminum alloy extrusion die concave die coated with the WC / Ni coating are refined to obtain the final aluminum alloy extrusion die.
[0092] Example 3
[0093] The method for preparing the highly wear-resistant and self-lubricating aluminum alloy extrusion die of the present invention comprises the following steps:
[0094] Step 1: Casting of aluminum alloy extrusion die blank. The molten iron after inoculation and spheroidization treatment is poured into the mold to cast the aluminum alloy extrusion die blank first;
[0095] After step 1, the composition of the cast aluminum alloy extrusion die blank is: 2.7% Si, 3.4% C, 1.5% Ni, 2.0% Mo, 0.40% Cr, 0.70% V, 0.50% Mn, ≤0.1% P, 0.04% Mg 残留 , ≤0.02% S, the rest is Fe and unavoidable impurities; the corresponding metallographic structure of the blank is: metal matrix + a large number of fine and evenly distributed spherical graphite (graphite ball density is 430 / mm 2 , ball diameter is about 20um) + coarse eutectic carbide.
[0096] Step 2: Preheating of aluminum alloy die. Perform homogenization annealing on the aluminum alloy extrusion die blank;
[0097] The preheating treatment in step 2 is: heating the blank to 1030°C at a rate of 3300°C / h and keeping it at that temperature for 7h, then cooling it to 500°C in the furnace, and then air cooling it to room temperature after it is taken out of the furnace;
[0098] After step 2, the structure of the mold is: pearlite + a large number of fine graphite balls.
[0099] Step 3: Preparation of semi-finished aluminum alloy extrusion die. The aluminum alloy extrusion die blank after homogenization annealing is machined into a semi-finished aluminum alloy extrusion die;
[0100] Step 4: Final heat treatment of aluminum alloy extrusion die. The machined aluminum alloy extrusion die semi-finished product is quenched and tempered;
[0101] The heat treatment quenching process in step 4 is: heating the semi-finished mold to 930°C at a rate of 330°C / h and keeping it warm for 2.5h, and then air cooling it to room temperature;
[0102] After quenching in step 4, the structure of the mold is: high carbon martensite + a large amount of undercooled austenite + graphite nodules;
[0103] The tempering process in step 4 is: 560℃ for 2h, repeated twice;
[0104] After tempering in step 4, the structure of the mold is: tempered troostite + dispersed fine alloy carbides containing (Mo, V and Cr) + graphite nodules + a small amount of residual austenite. The hardness of the mold after tempering is HRC49.2.
[0105] Step 5: Finishing of aluminum alloy extrusion die. Grind the semi-finished aluminum alloy extrusion die that has been quenched and tempered into the final shape and size of the aluminum alloy extrusion die;
[0106] Step 6: Apply high hardness WC / Ni coating on the aluminum alloy extrusion die. Apply WC / Ni coating on the processed aluminum alloy extrusion die concave die working belt by laser coating;
[0107] In step 6, a high-hardness WC / Ni layer is applied, and various coating preparation technologies such as laser cladding and thermal spraying can be used. The coating is applied at the concave die working zone of the mold; the coating thickness is 0.5 mm and the coating width is 3 mm.
[0108] During the WC / Ni coating process in step 6, the coating position of the mold needs to be heated to 550°C before the coating can be applied. After the coating is applied, the coated mold needs to be immediately placed in a heating furnace at a temperature of 500°C for stress relief annealing for 5 hours.
[0109] Step 7: Obtaining the aluminum alloy extrusion die: The size and shape of the aluminum alloy extrusion die concave die coated with the WC / Ni coating are refined to obtain the final aluminum alloy extrusion die.
[0110] The aluminum alloy extrusion die coated with WC / Ni coating prepared by the method of the present invention has a die base hardness greater than 50HRC, a tensile strength greater than 1000MPa, a compressive strength greater than 1900MPa, a high-temperature tensile strength greater than 900MPa at 500°C, and a high-temperature compressive strength greater than 1900MPa. The hardness of the WC / Ni coating is greater than 65HRC. In addition to having high hardness, tensile strength, and compressive strength at room temperature, the aluminum alloy extrusion die coated with WC / Ni coating still maintains a hardness greater than 65HRC, a tensile strength greater than 900MPa, and a compressive strength greater than 1900MPa at 500°C, has good high-temperature mechanical properties and mechanical property stability, and can meet the requirements of extrusion dies.
Claims
1. A method for preparing a highly wear-resistant, self-lubricating aluminum alloy extrusion die, characterized in that: Follow the steps below to implement it: Step 1: Casting aluminum alloy extrusion die blank; Step 2: subjecting the aluminum alloy extrusion die blank to homogenization annealing treatment; Step 3: machining the aluminum alloy extrusion die blank after homogenization annealing into an aluminum alloy extrusion die semi-finished product; Step 4: quenching and tempering the machined aluminum alloy extrusion die semi-finished product; Step 5: Grinding the quenched and tempered aluminum alloy extrusion die semi-finished product into an aluminum alloy extrusion die; Step 6: Applying WC / Ni coating on the concave die working belt of the processed aluminum alloy extrusion die; Step 7: The size and shape of the concave die of the aluminum alloy extrusion die coated with the WC / Ni coating are refined to obtain a highly wear-resistant, self-lubricating aluminum alloy extrusion die.
2. The method for preparing a highly wear-resistant, self-lubricating aluminum alloy extrusion die according to claim 1, characterized in that: In the step 1, specifically: The bread iron and scrap steel are heated to above 1500° C. to melt and obtain molten iron; according to the component requirements, 2.0%-2.5% nickel plate, 0.5%-1.0% ferrochrome, 2.5%-3.0% ferromolybdenum and 1.0%-1.5% ferrovanadium are weighed and added into the molten iron; the molten iron is inoculated and spheroidized with an inoculant and a spheroidizing agent; after the inoculation and spheroidization are completed, the molten iron is poured into a mold to cast an aluminum alloy extrusion die blank; The cast aluminum alloy extrusion die blank includes the following components according to mass percentage: 2.4-3.0% Si, 3.3-3.7% C, 1.0-2.0% Ni, 1.50-2.50% Mo, 0.30-0.50% Cr, 0.50-0.80% V, 0.40-0.60% Mn, ≤0.1% P, 0.03-0.05% Mg 残留 , ≤0.02% S, the rest is Fe and unavoidable impurities.
3. The method for preparing a highly wear-resistant, self-lubricating aluminum alloy extrusion die according to claim 1, characterized in that: In the step 2, specifically: The aluminum alloy extrusion die blank is heated to 1000-1050°C at a rate of 300-350°C / h and kept warm for 6-8h, then cooled to 500°C in the furnace, and then air-cooled to room temperature after being taken out of the furnace.
4. The method for preparing a highly wear-resistant, self-lubricating aluminum alloy extrusion die according to claim 1, characterized in that: In step 4, the quenching process is: heating the machined aluminum alloy extrusion die semi-finished product to 900-950°C at a rate of 300-350°C / h and keeping it warm for 2-3h, and then air-cooling it to room temperature; the tempering process is: keeping it warm at 550-570°C for 2h, and repeating it twice.
5. The method for preparing a highly wear-resistant, self-lubricating aluminum alloy extrusion die according to claim 1, characterized in that: In step 6, the coating thickness is 0.4-0.6 mm, and the coating width is 2-4 mm.
6. The method for preparing a highly wear-resistant, self-lubricating aluminum alloy extrusion die according to claim 1, characterized in that: In step 6, during the WC / Ni coating process, the coating position of the mold needs to be heated to 550°C first, and then the coating is applied. After the coating is applied, the coated mold needs to be immediately placed in a heating furnace at 500°C for stress relief annealing for 4-6 hours.
7. High wear resistance, self-lubricating aluminum alloy extrusion die, characterized by: The preparation is obtained by the preparation method according to any one of claims 1 to 6.