Air conditioner control panel waste crushing and recycling system and recycled PC resin prepared by using same
Through the multi-step processing of the air-conditioning control panel waste crushing and recycling system, the problem of low waste utilization is solved, efficient recycling and reuse is achieved, production costs are reduced, and product quality and yield rate are improved.
Patent Information
- Application Number
- CN202411237807.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-01
AI Technical Summary
The recycling of waste in automobile air conditioning control panels is low, and the utilization value of recycling waste is relatively low, resulting in increased production costs and insufficient quality.
A waste crushing and recycling system for air conditioning control panels is designed, including ultrasonic cleaning, drying, quick-cooling embrittlement, multi-roll crushing, particle size screening, batching and granulation, etc., and the waste is converted through multiple steps. It is a recycled PC resin that can be used in injection molding.
It realizes batch recycling of automobile air conditioning control panel waste, improves resource utilization, reduces production costs, and improves the processing performance and yield rate of recycled and recycled PC resin, meeting the production indicators of green factories.
Smart Images

Figure CN118876290A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of plastic recycling and reuse systems, and in particular to an air-conditioning control panel waste crushing and recycling system and a recycled PC resin prepared using the same. Background Art
[0002] The car air conditioning control panel is an important component inside the vehicle, allowing car users to easily adjust and control the various functions of the car's air conditioning system, as well as provide economical operation control and comprehensive display functions. The car air conditioning control panel can realize operating functions including temperature adjustment, wind speed control, mode selection, etc.
[0003] At present, the material of automobile air conditioning control panel is PC composite material, which is mainly made of PC resin, lubricant, antioxidant, inorganic filler and masterbatch, giving it good processability, wear resistance and impact toughness. In the process of injection molding of automobile air conditioning control panel, automobile air conditioning control panel waste will be generated due to problems such as dimensional accuracy and appearance defects.
[0004] At present, air conditioning control panel manufacturers usually deal with air conditioning control panel waste by selling them to plastic recyclers at low prices. Some air conditioning control panel manufacturers recycle the air conditioning control panel waste by extrusion, crushing and melting. However, the air conditioning control panel waste recycled by extrusion, crushing and melting is degraded by secondary thermal oxidation, resulting in a decrease in overall mechanical properties and wear resistance, which cannot meet the production requirements of standard automobile air conditioning control panels.
[0005] If the automobile air-conditioning control panel is made from the above-mentioned recycled waste, there is a certain gap in the overall quality between the automobile air-conditioning control panel and the automobile air-conditioning control panel made from new PC composite masterbatch. Not only can it not meet the patent requirements of automobile companies for automobile air-conditioning control panels, but the automobile air-conditioning control panel made from recycled waste has a low yield rate. The resulting air-conditioning control panel waste has no utilization value and can only be sold to plastic recyclers at a low price. In summary, the technical difficulties of the relevant air-conditioning control panel waste technology are: the recycling of air-conditioning control panel waste is low, and the utilization value of recycled waste is low. Summary of the invention
[0006] In order to solve the problems of low recycling of waste air-conditioning control panels and low utilization value of recycled waste in the above-mentioned prior art, the present invention provides a system for crushing and recycling waste air-conditioning control panels and regenerated recycled PC resin prepared by the system.
[0007] The present invention provides an air conditioner control panel waste crushing and recycling system, which is realized by the following scheme: A waste crushing and recycling system for air-conditioning control panel comprises an ultrasonic cleaning machine, a cleaning waste drying component, a waste rapid cooling and embrittlement component, a multi-roll crushing component, a particle size screening component, an integrated batching component, a screw extruder, a silicone oil cooling tank, and a granulator. The waste of the air-conditioning control panel is placed in the ultrasonic cleaning machine for ultrasonic cleaning to remove pollutants on the surface of the waste of the air-conditioning control panel, and then input into the cleaning waste drying component for drying treatment. The dried waste of the air-conditioning control panel is input into the waste rapid cooling and embrittlement component for rapid cooling and embrittlement treatment. The waste of the air-conditioning control panel that has been rapidly cooled and embrittled is input into the multi-roll crushing component for multi-roll crushing treatment. The crushed material is obtained by roller crushing, and the obtained crushed material is input into the particle size screening component for screening treatment, and the crushed waste A with a particle size greater than Nmm and the crushed waste B with a particle size less than Nmm are screened out. The obtained crushed waste A with a particle size greater than Nmm is input into the multi-roller crushing component for secondary crushing treatment, and the crushed waste B with a particle size less than Nmm is input into the integrated batching component for improved filler compounding to obtain a recycled composite material. The obtained recycled composite material is input into the screw extruder for melt extrusion and wire drawing treatment, input into the silicone oil cooling tank for cooling treatment, and input into the granulator for granulation treatment to obtain recycled PC resin that can be directly used for injection molding of automobile air-conditioning control panels.
[0008] The invention can recycle automobile air-conditioning control panel waste in batches, and the obtained recycled PC resin can be directly used for injection molding of automobile air-conditioning control panels, thereby improving resource utilization and reducing the production cost of automobile air-conditioning control panels.
[0009] Preferably, the cleaning waste drying component includes a first conveyor belt conveyor and a first oven, the first oven is fixedly connected to the first conveyor belt conveyor, and the first oven is reserved with an inlet and an outlet for the air-conditioning control panel waste to enter and exit; a plurality of hot air output pipes are fixedly connected inside the first oven; the input port of the hot air output pipe faces the upper surface of the conveyor belt of the first conveyor belt conveyor; the hot air input temperature of the hot air output pipe is 60-80°C, and the wind speed is 0.5-3m / s; the temperature inside the first oven is controlled to be 75-95°C, and the speed of the air-conditioning control panel waste that has completed ultrasonic cleaning transmitted by the first conveyor belt conveyor is 3-8cm / s; the length of the first oven is 6-8m.
[0010] By adopting the above technical solution, waste of air-conditioning control panels that have been ultrasonically cleaned can be dried efficiently.
[0011] Preferably, the waste rapid cooling and embrittlement component includes a second conveyor belt conveyor and an insulation box, the insulation box is fixedly connected to the second conveyor belt conveyor, and the insulation box is reserved with an inlet and an outlet for the air-conditioning control panel waste to enter and exit; a limiting protrusion frame for positioning and placing the air-conditioning control panel waste is formed on the conveyor belt of the second conveyor belt conveyor; a plurality of groups of low-temperature nitrogen output pipe groups are fixedly connected in the insulation box; the low-temperature nitrogen output pipe group includes at least three low-temperature nitrogen output pipes, and all the low-temperature nitrogen output pipes in a single low-temperature nitrogen output pipe group perform rapid cooling and embrittlement treatment on a single air-conditioning control panel waste at the same time, and the input port of the low-temperature nitrogen output pipe faces the limiting protrusion frame on the conveyor belt of the second conveyor belt conveyor; the temperature of the low-temperature nitrogen input to the low-temperature nitrogen output pipe is -80 to -40°C, and the wind speed is 1-5m / s; the speed of the air-conditioning control panel waste that has been dried and transmitted by the second conveyor belt conveyor is 2-6cm / s; the length of the insulation box is 6-12m.
[0012] By adopting the above technical solution, the air-conditioning control panel waste that has been dried can be quickly cooled and embrittled to facilitate high-quality crushing by subsequent multi-roll crushing components.
[0013] Preferably, the multi-roll crushing assembly includes a support frame, a first crushing roller group, a second crushing roller group, a pre-crushing collection tank, a high-speed crushing cutter head, and a high-speed drive motor. The first crushing roller group includes two crushing rollers A, and the vertical distance from the convex teeth on one crushing roller A to the surface of the other crushing roller A without convex teeth is X, and X is 3-8 cm; the second crushing roller group includes two crushing rollers B, and the vertical distance from the convex teeth on one crushing roller B to the surface of the other crushing roller B without convex teeth is Y, and Y is 1-5 mm and X>Y; the first crushing roller group is located at the positive side of the second crushing roller group. Above; the pre-crushing collection tank is fixedly connected to the bottom of the supporting frame; the high-speed crushing cutter head is rotatably connected to the pre-crushing collection tank; the high-speed driving motor is fixedly connected to the bottom of the pre-crushing collection tank; the rotating shaft of the high-speed driving motor is fixedly connected to the rotating shaft of the high-speed crushing cutter head through a coupling, and the high-speed driving motor drives the high-speed crushing cutter head to rotate at a high speed in the pre-crushing collection tank, and the pre-crushed particles obtained by the pre-crushing treatment of the first crushing roller group and the second crushing roller group are subjected to secondary high-speed crushing treatment, and the obtained crushed materials are input into the particle size screening component for screening treatment.
[0014] By adopting the above technical solution, the waste of air-conditioning control panel that has completed the rapid cooling and embrittlement treatment can be crushed into high-quality pieces.
[0015] Preferably, the particle size screening component includes a screening tank, a screening device, a connecting pipe, a first outlet pipe, and a second outlet pipe. The mesh size of the screening net is 3mm or 4mm or 5mm or 6mm or 7mm or 8mm or 9mm or 10mm, that is, the particle size of the crushed waste A is greater than 3mm or 4mm or 5mm or 6mm or 7mm or 8mm or 9mm or 10mm; the particle size of the crushed waste B is less than 3mm or 4mm or 5mm or 6mm or 7mm or 8mm or 9mm or 10mm; the screening net is detachable and fixedly connected to the screening tank. The screening tank is divided into a crushed waste A storage area and a crushed waste B storage area; the first outlet pipe is connected to the crushed waste A storage area of the screening tank; the second outlet pipe is connected to the crushed waste B storage area of the screening tank; the crushed waste A input by the first outlet pipe is put into a multi-roller crushing assembly for secondary crushing treatment; the second outlet pipe is connected to the integrated batching assembly; one end of the connecting pipe is connected to the top of the screening tank and the other end is connected to the bottom of the pre-crushing collection tank; the connecting pipe is provided with a control unit for controlling the output of the crushed material in the pre-crushing collection tank.
[0016] By adopting the above technical solution, the crushed waste B screened out by the particle size screening component helps to improve the processing performance, wear resistance and dimensional stability of the recycled PC resin, and improve the yield rate of injection molding products made of recycled PC resin.
[0017] Preferably, the integrated batching component includes a crushed material storage tank, a compound modifier storage tank and a mixing kettle connected to the second outlet pipe, the crushed material storage tank is connected to the top of the mixing kettle; the crushed material storage tank is connected to a first metering tank; the first metering tank is connected to the mixing kettle; the compound modifier storage tank is connected to the top of the mixing kettle; the compound modifier storage tank is connected to a second metering tank; the second metering tank is connected to the mixing kettle; the bottom of the mixing kettle is connected to the feed end of the screw extruder through a conveying pipeline, the compound modifier stored in the compound modifier storage tank and the crushed waste B stored in the crushed material storage tank are mixed uniformly in the mixing kettle according to a mass ratio of (5-30): (70-95) to obtain a recycled waste composition, and the obtained recycled waste composition is sequentially passed through a screw extruder, a silicone oil cooling tank, and a granulator for melt extrusion, wire drawing, cooling, and granulation to obtain recycled PC resin pellets.
[0018] By adopting the above technical solution, the automated batching of the recycled waste composition is achieved, thereby improving the overall production efficiency.
[0019] Preferably, the compound modifier stored in the compound modifier storage tank is a compound functional filler composition or a compound modified PC masterbatch; When the composite modifier is a composite functional filler, the composite functional filler is composed of the following raw materials in parts by weight: 0.5-2 parts of amino carbon nanotubes, 1-5 parts of zinc oxide whiskers surface-modified with methacryloxysilane, 5-25 parts of boron nitride nanosheets surface-modified with methacryloxysilane, and 5-10 parts of ultrafine silicon nitride surface-modified with methacryloxysilane; the composite functional filler and the crushed waste B stored in the crushed material storage tank are in a mass ratio of (5-10):(90-95); When the compound modifier is a compound modified PC masterbatch, the compound modified PC masterbatch is composed of the following raw materials in parts by weight: 0.5-2 parts of amino carbon nanotubes, 1-5 parts of methacryloxysilane surface-modified zinc oxide whiskers, 34-45 parts of compound functional fillers, 3-5 parts of compatibilizer-SEBS-g-MAH, 0.5-1 parts of antioxidant 1076, and 50-60 parts of PC resin; the compound modified PC masterbatch and the crushed waste B stored in the crushed material storage tank are in a mass ratio of (18-30): (70-82).
[0020] The recycled resin is modified with composite fillers during the waste recycling stage, which overcomes the problems of deviation in processing performance and wear resistance, and low yield rate of automobile air-conditioning control panels made of pure recycled PC resin. It can be directly used for injection molding of automobile air-conditioning control panels, thereby improving the utilization value of recycled PC resin and meeting the production indicators of green factories.
[0021] Preferably, the compound modifier is a compound functional filler, and the compound functional filler is composed of 1 part of amino carbon nanotubes, 3 parts of zinc oxide whiskers surface-modified with methacryloxysilane, 20 parts of boron nitride nanosheets surface-modified with methacryloxysilane, and 6 parts of ultrafine silicon nitride surface-modified with methacryloxysilane; the methacryloxysilane is at least one of γ-methacryloxypropyl triisopropoxysilane KH-571, γ-methacryloxypropyl trimethoxysilane KH-570, and γ-methacryloxypropyl methyldimethoxysilane KH-572; the mass ratio of the compound functional filler to the crushed waste B stored in the crushed material storage tank is (7-8):(92-93); When the compound modifier is a compound modified PC masterbatch, the compound modified PC masterbatch is composed of the following raw materials in parts by weight: 40 parts of a compound functional filler, 4 parts of a compatibilizer-SEBS-g-MAH, 1 part of an antioxidant 1076, and 55 parts of a PC resin; the compound modified PC masterbatch and the crushed waste B stored in the crushed material storage tank are in a mass ratio of (20-24):(76-80).
[0022] By adopting the above technical solution, it is helpful to improve the processing performance, wear resistance and dimensional stability of recycled PC resin, and improve the yield rate of injection molded products made of recycled PC resin.
[0023] Preferably, the waste formula of the air conditioner control panel is composed of the following raw materials in parts by weight: 3-6 parts of compatibilizer-SEBS-g-MAH, 1-10 parts of carbon black, 5-10 parts of barium sulfate, 1-5 parts of titanium dioxide, 0.5-1 parts of antioxidant 1076, 0.5-1 parts of siloxane coupling agent, and 75-85 parts of PC resin; the PC resin is selected from SABIC PC OQ1020L, and the melt index is 70±1g / 10min; The recycled PC resin formula is composed of the following raw materials in parts by weight: 10-20 parts of the compound modifier stored in the compound modifier storage tank, and 80-90 parts of crushed waste B with a particle size less than Nmm that has been sieved by a particle size sieve component in an air conditioner control panel waste shredding and recycling system.
[0024] A recycled PC resin prepared by utilizing an air conditioner control panel waste crushing and recycling system, and the preparation method thereof is as follows: Step 1: Place the waste of the air-conditioning control panel in an ultrasonic cleaning machine for ultrasonic cleaning to remove pollutants on the surface of the waste of the air-conditioning control panel, and then input the waste of the cleaning control panel into a drying assembly for drying. The drying parameters are as follows: the hot air temperature input into the hot air output pipe is 75-80°C, and the wind speed is 1.5-2m / s; the temperature in the first oven is controlled to be 75-80°C, and the speed of the waste of the air-conditioning control panel that has completed ultrasonic cleaning by the first conveyor belt conveyor is 4cm / s; the length of the first oven is 8m, and the waste of the air-conditioning control panel that has completed the drying process is obtained; Step 2: The dried air-conditioning control panel waste obtained in step 1 is input into the waste rapid cooling and embrittlement assembly for rapid cooling and embrittlement treatment. The rapid cooling and embrittlement treatment parameters are as follows: the temperature of the low-temperature nitrogen input into the low-temperature nitrogen output pipe is -80 to -60°C, the wind speed is 2-3m / s, the speed of the dried air-conditioning control panel waste transmitted by the second conveyor belt conveyor is 4cm / s, the length of the insulation box is 8m, and the rapid cooling and embrittlement treatment is completed to obtain the rapid cooling and embrittlement air-conditioning control panel waste; Step 3: The waste of the air-conditioning control panel that has been rapidly cooled and embrittled in step 2 is input into a multi-roll crushing assembly for multi-roll crushing treatment, wherein X in the first crushing roller group is 5 cm, Y in the second crushing roller group is 2 mm, the speed of the crushing roller A in the first crushing roller group is 120-150 r / min, the speed of the crushing roller B in the second crushing roller group is 180-240 r / min, and the speed of the high-speed crushing cutter head is 800-1200 r / min, thereby obtaining crushed material; Step 4: The crushed material obtained after the multi-roll crushing treatment is input into the particle size screening component for screening treatment. The mesh aperture of the screening net is 3 mm. The crushed waste A with a particle size greater than 3 mm and the crushed waste B with a particle size less than 3 mm are screened out. The crushed waste A with a particle size greater than 3 mm is input into the multi-roll crushing component for secondary crushing treatment, and the crushed waste B with a particle size less than 3 mm is input into the crushed material storage tank for standby; Step 5, the compound modifier stored in the compound modifier storage tank is metered into the mixing kettle through the second metering tank, and the crushed waste B in the crushed material storage tank is metered into the mixing kettle through the first metering tank. The mixing kettle rotates at a speed of 400-500r / min to mix the crushed waste B and the compound modifier evenly to obtain a regenerated recovery composite material; the mass ratio of the compound modifier to the crushed waste B is (5-30): (70-95); Step six, the obtained recycled composite material is sequentially passed through a screw extruder, a silicone oil cooling tank, and a granulator for melt extrusion, wire drawing, cooling, and granulation to obtain a recycled PC resin that can be directly used for injection molding of a car air-conditioning control panel; the obtained recycled PC resin needs to be dried before injection molding.
[0025] The preparation method provided by the present invention has relatively low difficulty in implementation and operation, and has a high degree of automated production, which is convenient for realizing batch production and preparation, thereby facilitating the reduction of the recycling cost of recycled PC resin and meeting the production indicators of green factories.
[0026] In summary, this application has the following advantages: 1. The present invention can recycle automobile air-conditioning control panel waste in batches, and the obtained recycled PC resin can be directly used for injection molding of automobile air-conditioning control panels, thereby improving resource utilization and reducing the production cost of automobile air-conditioning control panels.
[0027] 2. The present invention modifies the recycled resin with composite fillers during the waste recycling stage, thereby overcoming the problems of deviation in processing performance and wear resistance and low yield rate of automobile air-conditioning control panels prepared from pure recycled PC resin. The recycled resin can be directly used for injection molding of automobile air-conditioning control panels, thereby improving the utilization value of recycled PC resin and meeting the production indicators of green factories.
[0028] 3. The preparation method provided by the present invention has relatively low difficulty in implementation and operation, and has a high degree of automated production, which is convenient for mass production and preparation, thereby facilitating the reduction of the recycling cost of recycled PC resin and meeting the production indicators of green factories. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 It is a schematic diagram of the overall structure of the air-conditioning control panel waste crushing and recycling system in the embodiment of the present application.
[0030] Figure 2 It is a structural schematic diagram of the cleaning waste drying component in the air-conditioning control panel waste crushing and recycling system of the present application.
[0031] Figure 3 It is a structural schematic diagram of the waste rapid cooling and embrittlement component in the air-conditioning control panel waste crushing and recycling system of the present application.
[0032] Figure 4 It is a schematic diagram of the connection structure of the multi-roller crushing assembly and the particle size screening assembly in the air-conditioning control panel waste crushing and recycling system of the present application, which is used to show the connection structure of the multi-roller crushing assembly and the particle size screening assembly.
[0033] Figure 5 yes Figure 4 A partial enlarged view of point A in the middle.
[0034] Figure 6 It is a schematic diagram of the structure of the waste rapid cooling embrittlement component in Example 2 of the present application.
[0035] In the figure, 1, ultrasonic cleaning machine; 2, cleaning waste drying assembly; 21, first conveyor belt conveyor; 22, first oven; 23, hot air output pipe; 24, compressed air heater; 3, waste rapid cooling embrittlement assembly; 31, second conveyor belt conveyor; 32, insulation box; 33, low-temperature nitrogen output pipe group; 331, low-temperature nitrogen output pipe; 332, low-temperature nitrogen storage tank; 4, multi-roll crushing assembly; 41, support frame; 42, first crushing roller group; 421, crushing roller A; 43, second crushing roller group; 431, crushing roller B; 44, pre-crushing collection tank; 45 , high-speed crushing cutter head; 46, high-speed drive motor; 5, particle size screening component; 51, screening tank; 511, crushed waste storage area A; 512, crushed waste storage area B; 52, screening net; 53, connecting pipe; 54, first outlet pipe; 55, second outlet pipe; 56, control unit; 561, sealing cover; 562, electric push cylinder; 6, integrated batching component; 61, crushed material storage tank; 611, first metering tank; 612, second metering tank; 62, compound modifier storage tank; 63, mixing kettle; 7, screw extruder; 8, silicone oil cooling tank; 9, granulator. DETAILED DESCRIPTION
[0036] In order to further understand the present invention, preferred embodiments of the present invention are described below in conjunction with examples and control groups. Example
[0037] refer to Figure 1 A waste crushing and recycling system for an air-conditioning control panel includes an ultrasonic cleaning machine 1, a cleaning waste drying component 2, a waste rapid cooling and embrittlement component 3, a multi-roll crushing component 4, a particle size screening component 5, an integrated batching component 6, a screw extruder 7, a silicone oil cooling tank 8, and a granulator 9.
[0038] The formula of waste air-conditioning control panel is composed of the following raw materials in parts by weight: 3-6 parts of compatibilizer-SEBS-g-MAH, 1-10 parts of carbon black, 5-10 parts of barium sulfate, 1-5 parts of titanium dioxide, 0.5-1 parts of antioxidant 1076, 0.5-1 parts of siloxane coupling agent, and 75-85 parts of PC resin; the PC resin is selected from SABIC PC OQ1020L, and the melt index is 70±1g / 10min.
[0039] The recycled PC resin formula is composed of the following raw materials in parts by weight: 10-20 parts of the compound modifier stored in the compound modifier storage tank 62, and 80-90 parts of the crushed waste B with a particle size less than Nmm that has been sieved by the particle size screening component 5 in the air-conditioning control panel waste crushing and recycling system.
[0040] refer to Figure 2 The cleaning waste drying assembly 2 includes a first conveyor belt conveyor 21 and a first oven 22, and the first oven 22 is fixedly connected to the bracket of the first conveyor belt conveyor 21. The first oven 22 is reserved with an inlet and an outlet for the waste of the air-conditioning control panel to enter and exit. At least six hot air output pipes 23 are fixedly connected in the first oven 22. The hot air output pipes 23 are all connected to the compressed air heater 24, and the compressed air heater 24 is connected to the compressed air input pipe. The input port of the hot air output pipe 23 faces the upper surface of the conveyor belt of the first conveyor belt conveyor 21. The conveyor belt on the first conveyor belt conveyor 21 transports the waste of the air-conditioning control panel after ultrasonic cleaning to the bottom of the hot air output pipe 23, and the hot air output pipe 23 outputs hot air to dry the waste of the air-conditioning control panel after ultrasonic cleaning. The input hot air temperature of the hot air output pipe 23 is 60-80℃, and the wind speed is 0.5-3m / s. Preferably, the temperature of the hot air input to the hot air output pipe 23 is 75-80°C, and the wind speed is 1.5-2m / s. The temperature in the first oven 22 is controlled to be 75-95°C, and the speed of the waste air-conditioning control panel that has completed ultrasonic cleaning by the first conveyor belt conveyor 21 is 3-8cm / s; the length of the first oven 22 is 6-8m. Preferably, the temperature in the first oven 22 is controlled to be 75-80°C, and the speed of the waste air-conditioning control panel that has completed ultrasonic cleaning by the first conveyor belt conveyor 21 is 4cm / s; the length of the first oven 22 is 8m.
[0041] refer to Figure 3The waste rapid cooling and embrittlement assembly 3 includes a second conveyor belt conveyor 31, an insulation box 32 and several groups of low-temperature nitrogen output pipe groups 33, and the insulation box 32 is fixedly connected to the bracket of the second conveyor belt conveyor 31. The insulation box 32 is reserved with an inlet and an outlet for the waste of the air-conditioning control panel to enter and exit. In order to facilitate the rapid cooling and embrittlement treatment of the waste of the air-conditioning control panel that has been dried, a limiting protrusion frame for positioning and placing the waste of the air-conditioning control panel is formed on the conveyor belt of the second conveyor belt conveyor 31. Several low-temperature nitrogen output pipe groups 33 are fixedly connected to the inside of the insulation box 32, and the spacing between adjacent low-temperature nitrogen output pipe groups 33 is equal, and the number of low-temperature nitrogen output pipe groups 33 is 8 or more. The low-temperature nitrogen output pipe group 33 includes at least three low-temperature nitrogen output pipes 331, preferably the low-temperature nitrogen output pipe group 33 includes four low-temperature nitrogen output pipes 331 connected to the low-temperature nitrogen storage tank 332, and the angle between adjacent low-temperature nitrogen output pipes 331 is 90°. All the low-temperature nitrogen output pipes 331 in a single low-temperature nitrogen output pipe group 33 simultaneously perform rapid cooling and embrittlement treatment on a single air-conditioning control panel waste, and the input port of the low-temperature nitrogen output pipe 331 faces the limit raised frame on the conveyor belt of the second conveyor belt conveyor 31. When the conveyor belt on the second conveyor belt conveyor 31 transports the air-conditioning control panel waste that has been dried to the bottom of the low-temperature nitrogen output pipe group 33, the low-temperature nitrogen output pipe group 33 outputs low-temperature nitrogen to perform rapid cooling and embrittlement treatment on the air-conditioning control panel waste that has been dried. The temperature of the low-temperature nitrogen input to the low-temperature nitrogen output pipe 331 is -80 to -40°C, and the wind speed is 1-5m / s. Preferably, the temperature of the low-temperature nitrogen input to the low-temperature nitrogen output pipe 331 is -80 to -60°C, and the wind speed is 4m / s. The speed of the air-conditioning control panel waste that has been dried transmitted by the second conveyor belt conveyor 31 is 2-6cm / s; the length of the insulation box 32 is 6-12m. Preferably, the speed at which the dried waste air-conditioning control panel is conveyed by the second conveyor belt conveyor 31 is 4 cm / s; and the length of the heat preservation box 32 is 10 m.
[0042] refer to Figure 4The multi-roll crushing assembly 4 includes a support frame 41, a first crushing roller group 42, a second crushing roller group 43, a pre-crushing collection tank 44, a high-speed crushing cutter head 45, and a high-speed drive motor 46. Among them, the first crushing roller group 42 is located directly above the second crushing roller group 43. The first crushing roller group 42 includes two crushing rollers A421, and the vertical distance from the convex teeth on a crushing roller A421 to the surface of the other crushing roller A421 without convex teeth is X, X is 3-8cm, preferably, X is 5cm. The rotation speed of the crushing roller A421 is 120-150r / min, and the preferred rotation speed is 120 r / min. The second crushing roller group 43 includes two crushing rollers B431, and the vertical distance from the convex teeth on a crushing roller B431 to the surface of the other crushing roller B431 without convex teeth is Y, Y is 1-5mm and X>Y, preferably, Y is 2mm. The second crushing roller in the second crushing roller group 43 rotates at a speed of 180-240 r / min, preferably at 200 rpm.
[0043] refer to Figure 4 The bottom of the support frame 41 is an inverted cone opening, which is convenient for collecting pre-crushed materials. The upper port of the pre-crushing collection tank 44 is fixedly connected to the bottom of the support frame 41, so that the pre-crushed materials flow into the pre-crushing collection tank 44. The pre-crushed materials in the pre-crushing collection tank 44 will be crushed by the high-speed crushing cutter head 45 rotating at high speed to obtain crushed materials to be screened. The high-speed crushing cutter head 45 is rotatably connected to the pre-crushing collection tank 44, and the high-speed drive motor 46 is fixedly connected to the bottom of the pre-crushing collection tank 44. The rotating shaft of the high-speed drive motor 46 is fixedly connected to the rotating shaft of the high-speed crushing cutter head 45 through a coupling. The high-speed drive motor 46 drives the high-speed crushing cutter head 45 to rotate at a high speed of about 800-1200 r / min in the pre-crushing collection tank 44, and the pre-crushed particles obtained by the pre-crushing treatment of the first crushing roller group 42 and the second crushing roller group 43 are subjected to secondary high-speed crushing treatment. The crushed materials obtained after the secondary high-speed crushing treatment are input into the particle size screening component 5 for screening treatment to obtain crushed waste A and crushed waste B.
[0044] refer to Figure 4 The particle size screening component 5 includes a screening tank 51, a screening net 52, a connecting pipe 53, a first outlet pipe 54, and a second outlet pipe 55. The mesh aperture of the screening net 52 is 3mm, 4mm, 5mm, 6mm, 7mm, 8mm, 9mm, or 10mm, that is, the particle size of the crushed waste A is greater than 3mm, 4mm, 5mm, 6mm, 7mm, 8mm, 9mm, or 10mm; the particle size of the crushed waste B is less than 3mm, 4mm, 5mm, 6mm, 7mm, 8mm, 9mm, or 10mm. Preferably, the mesh aperture of the screening net 52 is 3mm, that is, the particle size of the crushed waste A is greater than 3mm, and the particle size of the crushed waste B is less than 3mm.
[0045] refer to Figure 4The screening net 52 is detachably and fixedly connected to the inside of the screening tank 51, dividing the screening tank 51 into a crushed waste A storage area 511 and a crushed waste B storage area 512. The screening net 52 and the screening tank 51 are detachably and fixedly connected in a manner that a limiting ring is fixedly connected to the inside of the screening tank 51, and the screening net 52 and the limiting ring are detachably and fixedly connected by bolts.
[0046] refer to Figure 4 The first outlet pipe 54 is connected to the crushed waste material A storage area 511 of the screening tank 51, and the crushed waste material A discharged from the first outlet pipe 54 is put into the multi-roller crushing assembly 4 for secondary crushing. One end of the second outlet pipe 55 is connected to the crushed waste material B storage area 512 of the screening tank 51, and the other end of the second outlet pipe 55 is connected to the integrated batching assembly 6.
[0047] refer to Figure 4-5 One end of the connecting pipe 53 is fixedly connected to the top of the screening tank 51 and the other end is fixedly connected to the bottom of the pre-crushing collection tank 44, so that the crushed materials obtained from the secondary high-speed crushing process can be controllably introduced into the screening tank 51 for screening. The connecting pipe 53 is provided with a control unit 56 for controlling the output of the crushed materials in the pre-crushing collection tank 44. The control unit 56 includes a cover 561 hinged to the discharge port at the bottom of the pre-crushing collection tank 44 and an electric push cylinder 562 for controlling the opening and closing of the cover 561. The electric push cylinder 562 is fixedly connected to the outer wall of the connecting pipe 53. The push rod of the electric push cylinder 562 slides and seals through the connecting pipe 53, extends into the interior of the connecting pipe 53, and is hinged to the cover 561, so that the electric push cylinder 562 can control the opening and closing of the cover 561 and automatically control the output of the crushed materials.
[0048] refer to Figure 1 The integrated batching component 6 includes a crushed material storage tank 61 connected to the second outlet pipe 55. The bottom of the crushed material storage tank 61 is fixedly connected to a first metering tank 611 through a pipeline. The end of the first metering tank 611 facing away from the crushed material storage tank 61 is fixedly connected to a mixing kettle 63 through a pipeline. The bottom of the mixing kettle 63 is connected to the feed end of the screw extruder 7 through a conveying pipeline. The top of the mixing kettle 63 is also connected to a second metering tank 621 through a pipeline. The end of the second metering tank 621 facing away from the mixing kettle 63 is fixedly connected to a compound modifier storage tank 62 through a pipeline. The compound modifier stored in the compound modifier storage tank 62 is a compound functional filler composition or a compound modified PC masterbatch.
[0049] refer to Figure 1The compound modifier stored in the compound modifier storage tank 62 and the crushed waste B stored in the crushed material storage tank 61 are mixed uniformly in a mixing kettle 63 according to a mass ratio of (5-30):(70-95) to obtain a recycled waste composition. The obtained recycled waste composition is sequentially passed through a screw extruder 7, a silicone oil cooling tank 8, and a granulator 9 for melt extrusion, wire drawing, cooling, and granulation to obtain recycled PC resin pellets.
[0050] In the process of regenerating and recovering PC resin configuration, compound modifier is particularly critical. The determination of compound modifier is obtained through experiments. For example, firstly, crushed waste B is used to prepare air-conditioning control panel sample a, and the mechanical properties, wear resistance and aging resistance of air-conditioning control panel sample a are tested; then new material (crushed waste B formula) is used to prepare air-conditioning control panel sample b, and the mechanical properties, wear resistance and aging resistance of air-conditioning control panel sample b are tested; crushed waste B is compounded with compound modifier to prepare air-conditioning control panel sample c, and the mechanical properties, wear resistance and aging resistance of air-conditioning control panel sample c are tested. If the mechanical properties, wear resistance and aging resistance of air-conditioning control panel sample c are close to or slightly better than those of air-conditioning control panel sample b, then the compound modifier composite configuration modification requirements are met.
[0051] When the compound modifier is a compound functional filler, the compound functional filler is composed of the following raw materials in parts by weight: 0.5-2 parts of amino carbon nanotubes, 1-5 parts of methacryloxysilane surface-modified zinc oxide whiskers, 5-25 parts of methacryloxysilane surface-modified boron nitride nanosheets, and 5-10 parts of methacryloxysilane surface-modified ultrafine silicon nitride; the compound functional filler and the crushed waste B stored in the crushed material storage tank 61 are in a mass ratio of (5-10): (90-95). The methacryloxysilane is at least one of γ-methacryloxypropyl triisopropoxysilane KH-571, γ-methacryloxypropyl trimethoxysilane KH-570, and γ-methacryloxypropyl methyldimethoxysilane KH-572.
[0052] The test preferred compound functional filler formula: 1 part of amino carbon nanotubes, 3 parts of zinc oxide whiskers surface-modified by methacryloxysilane, 20 parts of boron nitride nanosheets surface-modified by methacryloxysilane, and 6 parts of ultrafine silicon nitride surface-modified by methacryloxysilane. The methacryloxysilane is γ-methacryloxypropyltrimethoxysilane KH-570. The compound functional filler and the crushed waste B are in a mass ratio of (7-8): (92-93).
[0053] When the compound modifier is a compound modified PC masterbatch, the compound modified PC masterbatch is composed of the following raw materials in parts by weight: 34-45 parts of a compound functional filler, 3-5 parts of a compatibilizer-SEBS-g-MAH, 0.5-1 parts of an antioxidant 1076, and 50-60 parts of a PC resin; the compound modified PC masterbatch and the crushed waste B are in a mass ratio of (18-30):(70-82).
[0054] Preferably, when the compound modifier is a compound modified PC masterbatch, the compound modified PC masterbatch is composed of the following raw materials in parts by weight: 40 parts of compound functional filler, 4 parts of compatibilizer-SEBS-g-MAH, 1 part of antioxidant 1076, and 55 parts of PC resin; the compound modified PC masterbatch and the crushed waste B stored in the crushed material storage tank 61 are in a mass ratio of (20-24): (76-80).
[0055] A recycled PC resin prepared by utilizing an air conditioner control panel waste crushing and recycling system, and the preparation method thereof is as follows: Step 1: Place the waste of the air-conditioning control panel in an ultrasonic cleaning machine 1 for ultrasonic cleaning to remove pollutants on the surface of the waste of the air-conditioning control panel, and then input the waste of the cleaning into the drying component 2 for drying. The drying parameters are as follows: the hot air temperature input into the hot air output pipe 23 is 80° C., and the wind speed is 2 m / s; the temperature in the first oven 22 is controlled to be 80° C., and the speed of the waste of the air-conditioning control panel that has completed ultrasonic cleaning transmitted by the first conveyor belt conveyor 21 is 4 cm / s; the length of the first oven 22 is 8 m, and the waste of the air-conditioning control panel that has completed the drying process is obtained; Step 2: The dried air-conditioning control panel waste obtained in step 1 is input into the waste rapid cooling and embrittlement component 3 for rapid cooling and embrittlement treatment. The rapid cooling and embrittlement treatment parameters are as follows: the temperature of the low-temperature nitrogen input into the low-temperature nitrogen output pipe 331 is -75±1°C, the wind speed is 2m / s, the speed of the dried air-conditioning control panel waste transmitted by the second conveyor belt conveyor 31 is 4cm / s, the length of the insulation box 32 is 10m, and the rapid cooling and embrittlement treatment is completed to obtain the rapid cooling and embrittlement air-conditioning control panel waste; Step 3: The waste of the air-conditioning control panel that has been rapidly cooled and embrittled in step 2 is input into the multi-roll crushing assembly 4 for multi-roll crushing treatment, X in the first crushing roller group 42 is 5 cm, Y in the second crushing roller group 43 is 2 mm, the speed of the first crushing roller in the first crushing roller group 42 is 120 r / min, the speed of the second crushing roller in the second crushing roller group 43 is 200 r / min, and the speed of the high-speed crushing cutter head 45 is 1000 r / min, so as to obtain crushed material; Step 4: The crushed material obtained after the multi-roll crushing treatment is input into the particle size screening component 5 for screening treatment. The mesh aperture of the screening net 52 is 3 mm. The crushed waste A with a particle size greater than 3 mm and the crushed waste B with a particle size less than 3 mm are screened out. The crushed waste A with a particle size greater than 3 mm is input into the multi-roll crushing component 4 for secondary crushing treatment, and the crushed waste B with a particle size less than 3 mm is input into the crushed material storage tank 61 for standby; Step 5: the compound modifier stored in the compound modifier storage tank 62 is metered into the mixing kettle 63 through the second metering tank 621, and the crushed waste B in the crushed material storage tank 61 is metered into the mixing kettle 63 through the first metering tank 611. The mixing kettle 63 rotates at a speed of 400-500 r / min to mix the crushed waste B and the compound modifier evenly to obtain a regenerated recovery composite material; the mass ratio of the compound modifier to the crushed waste B is (5-30): (70-95); Step six, the obtained recycled composite material is sequentially passed through a screw extruder 7, a silicone oil cooling tank 8, and a granulator 9 for melt extrusion, wire drawing, cooling, and granulation to obtain a recycled PC resin that can be directly used for injection molding of a car air-conditioning control panel; the obtained recycled PC resin needs to be dried before injection molding.
[0056] Example 1: The method for preparing recycled PC resin using the air conditioner control panel waste crushing and recycling system is as follows: The preparation method of the JH11 air-conditioning control panel shell is as follows: firstly dry the SABIC PC OQ1020L at 120°C for 3h and set it aside; then prepare the masterbatch of the JH11 air-conditioning control panel shell: 250g of compatibilizer-SEBS-g-MAH (Coais W1G-4), 200g of carbon black (Mitsubishi Carbon Black MA100), 400g of barium sulfate (YF-1250 ultrafine barium sulfate of Yufeng brand), 200g of titanium dioxide (rutile titanium dioxide core R-215), 50g of antioxidant 1076, 50g of siloxane coupling agent KH570, 3850g of SABIC PC OQ1020L (melt index of 70±1g / 10min) was placed in a high-speed dispersion kettle, mixed and dispersed at 400rpm for 1h to obtain a mixed resin, and the obtained resin was placed in a twin-screw extruder, the screw speed was 440rpm, the screw aspect ratio was 32, the extrusion temperature was divided into seven heating zones, the first heating zone was set at 215°C, the second heating zone was set at 225°C, the first heating zone was set at 230°C, the third heating zone was set at 235°C, the fourth heating zone was set at 240°C, the fifth heating zone was set at 240°C, the sixth heating zone was set at 240°C, the seventh heating zone was set at 240°C, the die head temperature was 240.1°C, and the obtained molten extrudate was drawn, cooled with silicone oil, and granulated to obtain JH11 air conditioning control panel shell masterbatch with a particle size of 2-3mm; then the JH11 air conditioning control panel shell masterbatch is placed in a twin-screw extruder, the screw speed is 400rpm / min, the screw aspect ratio is 40, the extrusion temperature is divided into seven heating zones, the first heating zone is set at 220°C, the second heating zone is set at 230°C, the first heating zone is set at 240°C, the third heating zone is set at 245°C, the fourth heating zone is set at 250°C, the fifth heating zone is set at 250°C, the sixth heating zone is set at 250°C, and the seventh heating zone is set at 250°C, the die head temperature is 249.8°C, the molten extrudate is injected into a molding die, the injection pressure is 165MPa, the holding pressure is 45%, the back pressure is 13. 5MPa, and the JH11 air conditioning control panel shell is obtained after cooling and opening the mold. The JH11 air conditioning control panel shells of the same batch are quality inspected, and the JH11 air conditioning control panel shells with dimensional accuracy and appearance defects are waste air conditioning control panels; Step 1: placing the waste of the air-conditioning control panel in an ultrasonic cleaning machine 1 for ultrasonic cleaning, with an ultrasonic cleaning time of 5 minutes and an ultrasonic cleaning frequency of 40kHz, to remove pollutants on the surface of the waste of the air-conditioning control panel, and then placing the waste of the air-conditioning control panel on the conveyor belt of the first conveyor belt conveyor 21 and inputting it into the first oven 22 for drying treatment, and the drying treatment parameters are as follows: the input hot air temperature of the hot air output pipe 23 is 80°C, and the wind speed is 2m / s; the temperature in the first oven 22 is controlled to be 80°C, and the speed of the waste of the air-conditioning control panel that has completed ultrasonic cleaning transmitted by the first conveyor belt conveyor 21 is 4cm / s; the length of the first oven 22 is 8m, and the waste of the air-conditioning control panel that has completed drying treatment is obtained by inputting it into the first oven 22; Step 2: The dried air-conditioning control panel waste obtained in step 1 is placed in the limiting raised frame of the conveyor belt of the second conveyor belt conveyor 31, and the input air-conditioning control panel waste is quickly cooled and embrittled by the low-temperature nitrogen output pipe group 33 in the heat preservation box 32. The parameters of the rapid cooling and embrittlement treatment are as follows: the temperature of the low-temperature nitrogen input to the low-temperature nitrogen output pipe 331 is -75±1°C, the wind speed is 2m / s, the speed of the dried air-conditioning control panel waste transmitted by the second conveyor belt conveyor 31 is 4cm / s, the length of the heat preservation box 32 is 10m, and the rapid cooling and embrittlement treatment is completed to obtain the rapidly cooled and embrittled air-conditioning control panel waste; Step three, the waste of the air-conditioning control panel that has been rapidly cooled and embrittled in step two is input into the support frame 41 of the multi-roller crushing assembly 4 for multi-roller crushing treatment in the first crushing roller group 42 and the second crushing roller group 43, wherein X in the first crushing roller group 42 is 5 cm, Y in the second crushing roller group 43 is 2 mm, the speed of the first crushing roller in the first crushing roller group 42 is 120 r / min, and the speed of the second crushing roller in the second crushing roller group 43 is 200 r / min, and the pre-crushed material obtained by pre-crushing the first crushing roller group 42 and the second crushing roller group 43 is collected into the pre-crushing collection tank 44, and the high-speed driving motor 46 in the pre-crushing collection tank 44 drives the high-speed crushing cutter head 45 to rotate at a high speed of 1000 r / min for 15 minutes in the pre-crushing collection tank 44 for secondary high-speed crushing treatment; Step 4: The crushed material obtained after the secondary high-speed crushing treatment is input into the screening tank 51 in the particle size screening component 5 for screening treatment. The mesh aperture of the screening net 52 is 3 mm. The crushed waste A with a particle size greater than 3 mm and the crushed waste B with a particle size less than 3 mm are screened out. The obtained crushed waste A with a particle size greater than 3 mm is input into the multi-roll crushing component 4 for secondary crushing treatment, and the crushed waste B with a particle size less than 3 mm is input into the crushed material storage tank 61 for standby; Step 5: 5 kg of compound modifier is stored in the compound modifier storage tank 62. The compound modifier is a compound functional filler. The compound functional filler formula is composed of 1 part of amino carbon nanotubes (Xianfeng Nano's XFM62 amino multi-walled carbon nanotubes, outer diameter 8-15 nanometers and length 50 microns), 3 parts of KH570 surface modified zinc oxide whiskers (four-needle zinc oxide whiskers with a diameter of 0.5-5 microns and a length of 10-50 microns, brand Chaotai), 20 parts of KH570 surface modified boron nitride nanosheets (KMick, average thickness: <100nm, sheet diameter: 1-3 microns, specific surface area: 30m 2 / g), 6 parts of KH570 surface-modified ultrafine silicon nitride (Si3N4-AY500, average particle size 500nm, 99.5%, brand Chaotai), the compound functional filler is metered into the mixing kettle 63 through the second metering tank 621, the crushed waste B in the crushed material storage tank 61 is metered into the mixing kettle 63 through the first metering tank 611, the mass ratio of the compound modifier to the crushed waste B is 7:93, and the mixing kettle 63 rotates at a speed of 500r / min to evenly mix the crushed waste B and the compound modifier to obtain a regenerated recovery composite material; Step six, the obtained recycled composite material is melt-extruded in the screw extruder 7 in sequence, the screw speed is 440 rpm / min, the screw aspect ratio is 32, the extrusion temperature is divided into seven heating zones, the first heating zone is set to 215°C, the second heating zone is set to 225°C, the first heating zone is set to 230°C, the third heating zone is set to 235°C, the fourth heating zone is set to 240°C, the fifth heating zone is set to 240°C, the sixth heating zone is set to 240°C, the seventh heating zone is set to 240°C, the die head temperature is 240.1°C, the obtained molten extrudate is drawn and placed in a silicone oil cooling tank 8 for cooling, and after cooling, the wire is input into a granulator 9 for granulation to obtain a recycled PC resin that can be directly used for injection molding of an automobile air-conditioning control panel, and the particle size is 3-4mm; the obtained recycled PC resin needs to be dried at 120°C / 3h before injection molding.
[0057] The recycled PC resin prepared in the above Example 1 has a company brand number of JH11-RPC / CM-A.
[0058] The difference between Example 2 and Example 1 is: Figure 6In order to improve the efficiency of rapid cooling and embrittlement, several groups of hot air output pipe groups 34 are fixedly connected in the insulation box 32, specifically four groups of hot air output pipe groups 34 and five groups of low-temperature nitrogen output pipe groups 33. The hot air output pipe group 34 is located between adjacent low-temperature nitrogen output pipe groups 33, so as to realize the high-efficiency embrittlement treatment of the waste of the air-conditioning control panel by alternating hot and cold. The hot air output pipe group 34 includes at least three hot air output pipes 341, preferably the number of hot air output pipes 341 is four, and the angle formed by adjacent hot air output pipes 341 is 90°. The input hot air temperature of the hot air output pipe 341 is 40-60°C, and the wind speed is 1-4m / s. Preferably, the input hot air temperature is 45°C, and the wind speed is 2-2.5m / s.
[0059] The recycled PC resin prepared in the above Example 2 has a company brand number of JH11-RPC / CM-B.
[0060] refer to Figure 6 When the conveyor belt on the second conveyor belt conveyor 31 transports the waste of the air-conditioning control panel that has completed ultrasonic cleaning to the bottom of the low-temperature nitrogen output pipe group 33, the low-temperature nitrogen output pipe group 33 outputs low-temperature nitrogen to quickly cool the waste of the air-conditioning control panel that has completed drying; when the conveyor belt on the second conveyor belt conveyor 31 transports the waste of the air-conditioning control panel that has completed ultrasonic cleaning to the bottom of the hot air output pipe group 34, the hot air output pipe group 34 outputs hot air to heat-treat the waste of the air-conditioning control panel that has completed drying, thereby realizing efficient embrittlement treatment of the waste of the air-conditioning control panel by alternating cold and hot.
[0061] The difference of the method for preparing recycled PC resin by using the air-conditioning control panel waste crushing and recycling system is that: step 2, the dried air-conditioning control panel waste obtained in step 1 is placed in the limiting raised frame of the conveyor belt of the second conveyor belt conveyor 31, and the low-temperature nitrogen output pipe group 33 in the input insulation box 32 is used for rapid cooling and embrittlement treatment of the input air-conditioning control panel waste. The rapid cooling and embrittlement treatment parameters are as follows: the low-temperature nitrogen temperature input by the low-temperature nitrogen output pipe 331 is -75±1℃, the wind speed is 2m / s, the hot air output pipe group 34 performs heat treatment on the input air-conditioning control panel waste, the input hot air temperature is 45℃, the wind speed is 2m / s, a single air-conditioning control panel waste is staggered through eight low-temperature nitrogen output pipe groups 33 and seven hot air output pipe groups 34, and the cold and hot alternating efficient embrittlement treatment is carried out, the speed of the dried air-conditioning control panel waste transmitted by the second conveyor belt conveyor 31 is 4cm / s, the length of the insulation box 32 is 10m, and the rapid cooling and embrittlement treatment is completed to obtain the rapid cooling and embrittlement air-conditioning control panel waste. Except for step 2, the other steps are the same.
[0062] The difference between Example 3 and Example 1 is that the method for preparing recycled PC resin using the air-conditioning control panel waste crushing and recycling system is different in that: Step 5, the 5 kg of compound modifier stored in the compound modifier storage tank 62, the compound modifier is a compound modified PC masterbatch, and the compound modified PC masterbatch is composed of the following raw materials in parts by weight: 40 parts of compound functional filler [the compound functional filler formula is composed of the following raw materials in parts by weight: 1 part of amino carbon nanotubes (Xianfeng Nano's XFM62 amino multi-walled carbon nanotubes, outer diameter 8-15 nanometers and length 50 microns), 3 parts of KH570 surface-modified zinc oxide whiskers (four-needle zinc oxide whiskers with a diameter of 0.5-5 microns and a length of 10-50 microns, brand Chaotai), 20 parts of KH570 surface-modified boron nitride nanosheets (KMick, average thickness: <100nm, sheet diameter: 1-3 microns, specific surface area: 30m 2 / g), 6 parts of KH570 surface-modified ultrafine silicon nitride (Si3N4-AY500, average particle size 500nm)】, 4 parts of compatibilizer-SEBS-g-MAH (Coais W1G-4), 1 part of antioxidant 1076, 55 parts of PC resin SABIC PC OQ1020L; the compounded modified PC masterbatch and the crushed waste B stored in the crushed material storage tank 61 are input into the mixing kettle 63 according to the mass ratio of 2:8, the compounded modified PC masterbatch is metered into the mixing kettle 63 through the second metering tank 621, and the crushed waste B in the crushed material storage tank 61 is metered into the mixing kettle 63 through the first metering tank 611, that is, the mass ratio of the compounded modified PC masterbatch and the crushed waste B in the mixing kettle 63 is 2:8, and the crushed waste B and the compounded modifier are evenly mixed at a speed of 500r / min in the mixing kettle 63 to obtain the regeneration and recovery composite material. Except for step 5, the other steps are the same.
[0063] The preparation method of the compound modified PC masterbatch is as follows: firstly dry the SABIC PC OQ1020L at 120°C for 3h and set it aside; configure the compound functional filler: 4g of amino carbon nanotubes (Xianfeng Nano's XFM62 amino multi-walled carbon nanotubes, outer diameter 8-15nm length 50μm), 12g of KH570 surface modified zinc oxide whiskers (four-needle zinc oxide whiskers with a diameter of 0.5-5μm and a length of 10-50μm, brand Chaotai), 80g of KH570 surface modified boron nitride nanosheets (KMick, average thickness: <100nm, sheet diameter: 1-3μm, specific surface area: 30m 2 / g), 24g of KH570 surface-modified ultrafine silicon nitride (Si3N4-AY500, average particle size 500nm) were placed in a dispersion kettle and dispersed at 300rpm for 15min to obtain a composite functional filler; then 80g of the composite functional filler, 8g of compatibilizer-SEBS-g-MAH (Coais W1G-4), 2g of antioxidant 1076, 110g of SABIC PC OQ1020L was placed in a high-speed dispersion kettle and mixed and dispersed at 400 rpm for 1 h to obtain a mixed resin. The obtained resin was placed in a twin-screw extruder with a screw speed of 400 rpm / min, a screw aspect ratio of 40, and an extrusion temperature of seven heating zones. The first heating zone was set at 220°C, the second heating zone was set at 230°C, the first heating zone was set at 240°C, the third heating zone was set at 240°C, the fourth heating zone was set at 245°C, the fifth heating zone was set at 245°C, the sixth heating zone was set at 245°C, and the seventh heating zone was set at 245°C. The die head temperature was 244.8°C. The obtained molten extrudate was subjected to wire drawing, silicone oil cooling, and granulation to obtain a JH11 air-conditioning control panel shell masterbatch with a particle size of 2-3 mm.
[0064] The recycled PC resin prepared in the above Example 3 has a company brand number of JH11-RPC / CM-C.
[0065] Control group 1 is the JH11 air conditioning control panel shell masterbatch, and its preparation method is as follows: 250g of compatibilizer-SEBS-g-MAH (Coais W1G-4), 200g of carbon black (Mitsubishi Carbon Black MA100), 400g of barium sulfate (YF-1250 ultrafine barium sulfate of Yufeng brand), 200g of titanium dioxide (rutile titanium dioxide core R-215), 50g of antioxidant 1076, 50g of siloxane coupling agent KH570, 3850g of SABIC PC OQ1020L (melt index of 70±1g / 10min) was placed in a high-speed dispersion kettle and mixed and dispersed at 400rpm for 1h to obtain a mixed resin. The obtained resin was placed in a twin-screw extruder with a screw speed of 440rpm / min and a screw aspect ratio of 32. The extrusion temperature was divided into seven heating zones, with the first heating zone set at 215°C, the second heating zone set at 225°C, the first heating zone set at 230°C, the third heating zone set at 235°C, the fourth heating zone set at 240°C, the fifth heating zone set at 240°C, the sixth heating zone set at 240°C, and the seventh heating zone set at 240°C. The die head temperature was 240.1°C. The obtained molten extrudate was drawn, cooled with silicone oil, and granulated to obtain a JH11 air-conditioning control panel shell masterbatch with a particle size of 2-3mm.
[0066] The difference between the control group 2 and the embodiment 1 is that the method for preparing the recycled PC resin by using the air conditioner control panel waste crushing and recycling system is different in that: in step 5, only the crushed waste B in the crushed material storage tank 61 is metered into the mixing kettle 63 through the first metering tank 611, and the crushed waste B is mixed at a speed of 500r / min in the mixing kettle 63 to obtain the recycled composite material. Except for step 5, the other steps are the same.
[0067] The difference between the control group 3 and the embodiment 1 is that: the difference between the method for preparing the recycled PC resin by using the air conditioner control panel waste crushing and recycling system is that: step 5, the 5kg compound modifier stored in the compound modifier storage tank 62, the compound modifier is a compound functional filler, and the compound functional filler formula is 20 parts of KH570 surface modified boron nitride nanosheets (grams, average thickness: <100nm sheet diameter: 1-3 microns, specific surface area: 30m 2 / g), 10 parts of KH570 surface-modified ultrafine silicon nitride (Si3N4-AY500, average particle size 500nm), the compound functional filler is metered into the mixing kettle 63 through the second metering tank 621, the crushed waste B in the crushed material storage tank 61 is metered into the mixing kettle 63 through the first metering tank 611, the mass ratio of the compound modifier to the crushed waste B is 7:93, and the mixing kettle 63 rotates at a speed of 500r / min to evenly mix the crushed waste B and the compound modifier to obtain the regenerated recovery composite material. Except for step 5, the other steps are the same.
[0068] Control group 4 is a recycled PC resin obtained by conventional hydraulic crushing and melt extrusion granulation. The specific preparation method is as follows: the air conditioning control panel waste is loaded into a cast iron crushing barrel (inner diameter 30 cm, depth 40 cm, outer diameter 38 cm), and crushed by a hydraulic press. The hydraulic crushing obtains 0.2-3 cm of crushed material and is placed in a twin-screw extruder. The screw speed is 400 rpm / min, the screw aspect ratio is 40, and the extrusion temperature is divided into seven heating zones. The first heating zone is set at a temperature of 220°C, the second heating zone is set at a temperature of 230°C, the first heating zone is set at a temperature of 240°C, the third heating zone is set at a temperature of 240°C, the fourth heating zone is set at a temperature of 245°C, the fifth heating zone is set at a temperature of 245°C, the sixth heating zone is set at a temperature of 245°C, and the seventh heating zone is set at a temperature of 245°C. The die head temperature is 245.0°C, and the obtained melt extrudate is drawn, cooled with silicone oil, and granulated to obtain a recycled PC resin masterbatch with a particle size of 2-3 mm.
[0069] Table 1: Method parameter test table for recycled PC resin prepared by air conditioner control panel waste crushing and recycling system
[0070] As shown in Table 1, the test parameters of test group E can obtain relatively more broken waste B and the production cost is relatively economical.
[0071] Performance test: 1. Notched impact strength at 23°C is measured according to ASTM D-256. 2. Heat deformation temperature at 1.8MPa is measured according to ASTM D-648. 3. Tensile strength (yield point) is measured according to ASTM D-638. 4. Tensile fracture rate (fracture point) is measured according to ASTM D-638. 5. Wear resistance is measured according to GB / T 3960-2016 Plastic Sliding Friction and Wear Test Method. 6. Mold shrinkage is calculated by the formula: α = (D - M) / D, where D represents the mold size and M represents the size of the product after molding.
[0072] Table 2: Test parameters of automotive air conditioning control panel resin masterbatch in Examples 1-3 and Control Groups 1-4
[0073] The JH11 air conditioning control panel was produced using the automobile air conditioning control panel resin masterbatch in Examples 1-3 and Control Groups 1-4. The number of JH11 air conditioning control panels produced in the same batch was 50. The 50 JH11 air conditioning control panels were quality inspected to determine whether the dimensional error of the JH11 air conditioning control panel met the standard and whether there were defects (cracks, pits, etc.) on the shell appearance surface. The yield rate of the JH11 air conditioning control panels produced in the same batch was calculated.
[0074] Table 3: Test parameter table of the same batch of JH11 air conditioning control panels produced using the automotive air conditioning control panel resin masterbatch in Examples 1-3 and Control Groups 1-4
[0075] It can be seen from Examples 1-3, Control Groups 1-4 and Tables 2-3 that automobile air-conditioning control panel waste can be recycled in batches through the air-conditioning control panel waste crushing and recycling system combined with the corresponding production process, and the obtained recycled PC resin can be directly used for the injection molding of automobile air-conditioning control panels, thereby improving resource utilization and reducing the production cost of automobile air-conditioning control panels.
[0076] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed. However, as long as it is within the scope of the claims of the present application, it shall be protected by the patent law.
Claims
1. An air conditioner control panel waste crushing and recycling system, characterized in that: The invention comprises an ultrasonic cleaning machine (1), a cleaning waste drying component (2), a waste rapid cooling and embrittlement component (3), a multi-roll crushing component (4), a particle size screening component (5), an integrated batching component (6), a screw extruder (7), a silicone oil cooling tank (8), and a granulator (9). The air conditioning control panel waste is placed in the ultrasonic cleaning machine (1) for ultrasonic cleaning to remove pollutants on the surface of the air conditioning control panel waste, and then is input into the cleaning waste drying component (2) for drying treatment. The air conditioning control panel waste that has been dried is input into the waste rapid cooling and embrittlement component (3) for rapid cooling and embrittlement treatment. The air conditioning control panel waste that has been rapidly cooled and embrittled is input into the multi-roll crushing component (4) for multi-roll crushing treatment. The crushed material is obtained by multi-roll crushing treatment, and the obtained crushed material is input into the particle size screening component (5) for screening treatment, and the crushed waste A with a particle size greater than Nmm and the crushed waste B with a particle size less than Nmm are screened out. The obtained crushed waste A with a particle size greater than Nmm is input into the multi-roll crushing component (4) for secondary crushing treatment, and the crushed waste B with a particle size less than Nmm is input into the integrated batching component (6) for improved filler compounding to obtain a recycled composite material. The obtained recycled composite material is input into the screw extruder (7) for melt extrusion and wire drawing treatment, input into the silicone oil cooling tank (8) for cooling treatment, and input into the granulator (9) for granulation treatment to obtain recycled PC resin that can be directly used for injection molding of automobile air-conditioning control panels.
2. The air conditioner control panel waste crushing and recycling system according to claim 1 is characterized in that: The cleaning waste drying component (2) comprises a first conveyor belt conveyor (21) and a first oven (22), wherein the first oven (22) is fixedly connected to the first conveyor belt conveyor (21), and the first oven (22) is reserved with an inlet and an outlet for the air conditioning control panel waste to enter and exit; a plurality of hot air output pipes (23) are fixedly connected inside the first oven (22); the input ports of the hot air output pipes (23) face the upper surface of the conveyor belt of the first conveyor belt conveyor (21); the input hot air temperature of the hot air output pipes (23) is 60-80° C., and the wind speed is 0.5-3 m / s; the temperature inside the first oven (22) is controlled to be 75-95° C., and the speed of the air conditioning control panel waste that has been ultrasonically cleaned and is transmitted by the first conveyor belt conveyor (21) is 3-8 cm / s; and the length of the first oven (22) is 6-8 m.
3. The air conditioner control panel waste crushing and recycling system according to claim 1 is characterized in that: The waste rapid cooling and embrittlement assembly (3) comprises a second conveyor belt conveyor (31) and a heat preservation box (32); the heat preservation box (32) is fixedly connected to the second conveyor belt conveyor (31); the heat preservation box (32) is reserved with an inlet and an outlet for the waste of the air-conditioning control panel to enter and exit; a limiting protrusion frame for positioning and placing the waste of the air-conditioning control panel is formed on the conveyor belt of the second conveyor belt conveyor (31); a plurality of groups of low-temperature nitrogen output pipe groups (33) are fixedly connected in the heat preservation box (32); the low-temperature nitrogen output pipe group (33) comprises at least three low-temperature nitrogen output pipes (331), each of which has a plurality of low-temperature nitrogen output pipes (331). All low-temperature nitrogen output pipes (331) in a low-temperature nitrogen output pipe group (33) simultaneously perform rapid cooling and embrittlement treatment on a single waste air-conditioning control panel, the input port of the low-temperature nitrogen output pipe (331) faces a limit protrusion frame on the conveyor belt of the second conveyor belt conveyor (31); the temperature of the low-temperature nitrogen input to the low-temperature nitrogen output pipe (331) is -80 to -40°C, and the wind speed is 1-5m / s; the speed of the dried waste air-conditioning control panel transmitted by the second conveyor belt conveyor (31) is 2-6cm / s; and the length of the insulation box (32) is 6-12m.
4. The air conditioner control panel waste crushing and recycling system according to claim 3 is characterized in that: The multi-roll crushing assembly (4) comprises a support frame (41), a first crushing roller group (42), a second crushing roller group (43), a pre-crushing collection tank (44), a high-speed crushing cutter head (45), and a high-speed drive motor (46). The first crushing roller group (42) comprises two crushing rollers A (421), and the vertical distance from the protruding teeth on one crushing roller A (421) to the surface of the other crushing roller A (421) where the protruding teeth are not formed is X, and X is 3-8 cm. The second crushing roller group (43) comprises two crushing rollers B (431), and the vertical distance from the protruding teeth on one crushing roller B (431) to the surface of the other crushing roller B (431) where the protruding teeth are not formed is Y, and Y is 1-5 mm and X>Y. The first crushing roller group (42) is located at the second crushing roller The pre-crushing collection tank (44) is fixedly connected to the bottom of the support frame (41); the high-speed crushing cutter head (45) is rotatably connected to the pre-crushing collection tank (44); the high-speed drive motor (46) is fixedly connected to the bottom of the pre-crushing collection tank (44); the rotating shaft of the high-speed drive motor (46) is fixedly connected to the rotating shaft of the high-speed crushing cutter head (45) through a coupling, and the high-speed drive motor (46) drives the high-speed crushing cutter head (45) to rotate at a high speed in the pre-crushing collection tank (44), and performs a secondary high-speed crushing process on the pre-crushed particles obtained by the pre-crushing process of the first crushing roller group (42) and the second crushing roller group (43), and the obtained crushed materials are input into the particle size screening component (5) for screening.
5. The air conditioner control panel waste crushing and recycling system according to claim 4 is characterized in that: The particle size screening component (5) comprises a screening tank (51), a screening net (52), a connecting pipe (53), a first outlet pipe (54), and a second outlet pipe (55). The screen mesh diameter of the screening net (52) is 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, or 10 mm, that is, the particle size of the crushed waste A is greater than 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, or 10 mm; the particle size of the crushed waste B is less than 3 mm, 4 mm, 5 mm, 6 mm, 7 mm, 8 mm, 9 mm, or 10 mm; the screening net (52) is detachably and fixedly connected to the inside of the screening tank (51), dividing the screening tank (51) into the crushed waste A storage area (52); 11) and a crushed waste B storage area (512); the first outlet pipe (54) is connected to the crushed waste A storage area (511) of the screening tank (51); the second outlet pipe (55) is connected to the crushed waste B storage area (512) of the screening tank (51); the crushed waste A input by the first outlet pipe (54) is put into the multi-roll crushing assembly (4) for secondary crushing; the second outlet pipe (55) is connected to the integrated batching assembly (6); one end of the connecting pipe (53) is connected to the top of the screening tank (51) and the other end is connected to the bottom of the pre-crushing collection tank (44); the connecting pipe (53) is provided with a control unit (56) for controlling the output of the crushed material in the pre-crushing collection tank (44).
6. The air conditioner control panel waste crushing and recycling system according to claim 5 is characterized in that: The integrated batching assembly (6) comprises a crushed material storage tank (61), a compound modifier storage tank (62), and a mixing kettle (63) which are connected to the second outlet pipe (55); the crushed material storage tank (61) is connected to the top of the mixing kettle (63); the crushed material storage tank (61) is connected to a first metering tank (611); the first metering tank (611) is connected to the mixing kettle (63); the compound modifier storage tank (62) is connected to the top of the mixing kettle (63); the compound modifier storage tank (62) is connected to a second metering tank (621); the second metering tank (621) is connected to the mixing kettle (63); the bottom of the mixing kettle (63) is connected to the feed end of the screw extruder (7) through a conveying pipeline, and the compound modifier stored in the compound modifier storage tank (62) and the crushed waste B stored in the crushed material storage tank (61) are mixed in the mixing kettle (63) in a mass ratio of (5-30):(70-95) to obtain a recycled waste composition, and the obtained recycled waste composition is sequentially passed through the screw extruder (7), the silicone oil cooling tank (8), and the granulator (9) for melt extrusion, wire drawing, cooling, and granulation to obtain recycled PC resin pellets.
7. The air conditioner control panel waste crushing and recycling system according to claim 5 is characterized in that: The compound modifier stored in the compound modifier storage tank (62) is a compound functional filler composition or a compound modified PC masterbatch; When the composite modifier is a composite functional filler, the composite functional filler is composed of the following raw materials in parts by weight: 0.5-2 parts of amino carbon nanotubes, 1-5 parts of zinc oxide whiskers surface-modified with methacryloxysilane, 5-25 parts of boron nitride nanosheets surface-modified with methacryloxysilane, and 5-10 parts of ultrafine silicon nitride surface-modified with methacryloxysilane; the composite functional filler and the crushed waste B stored in the crushed material storage tank (61) are in a mass ratio of (5-10):(90-95); When the compound modifier is a compound modified PC masterbatch, the compound modified PC masterbatch is composed of the following raw materials in parts by weight: 0.5-2 parts of amino carbon nanotubes, 1-5 parts of methacryloxysilane surface-modified zinc oxide whiskers, 34-45 parts of compound functional fillers, 3-5 parts of compatibilizer-SEBS-g-MAH, 0.5-1 parts of antioxidant 1076, and 50-60 parts of PC resin; the compound modified PC masterbatch and the crushed waste B stored in the crushed material storage tank (61) are in a mass ratio of (18-30):(70-82).
8. The air conditioner control panel waste crushing and recycling system according to claim 7 is characterized in that: When the composite modifier is a composite functional filler, the composite functional filler is composed of 1 part of amino carbon nanotubes, 3 parts of zinc oxide whiskers surface-modified with methacryloxysilane, 20 parts of boron nitride nanosheets surface-modified with methacryloxysilane, and 6 parts of ultrafine silicon nitride surface-modified with methacryloxysilane; the methacryloxysilane is at least one of γ-methacryloxypropyl triisopropoxysilane KH-571, γ-methacryloxypropyl trimethoxysilane KH-570, and γ-methacryloxypropyl methyldimethoxysilane KH-572; the composite functional filler and the crushed waste B stored in the crushed material storage tank (61) are in a mass ratio of (7-8):(92-93); When the compound modifier is a compound modified PC masterbatch, the compound modified PC masterbatch is composed of the following raw materials in parts by weight: 40 parts of a compound functional filler, 4 parts of a compatibilizer-SEBS-g-MAH, 1 part of an antioxidant 1076, and 55 parts of a PC resin; the compound modified PC masterbatch and the crushed waste B stored in the crushed material storage tank (61) are in a mass ratio of (20-24):(76-80).
9. The air conditioner control panel waste crushing and recycling system according to claim 7, characterized in that: The waste formula of the air conditioner control panel is composed of the following raw materials in parts by weight: 3-6 parts of compatibilizer-SEBS-g-MAH, 1-10 parts of carbon black, 5-10 parts of barium sulfate, 1-5 parts of titanium dioxide, 0.5-1 parts of antioxidant 1076, 0.5-1 parts of siloxane coupling agent, and 75-85 parts of PC resin; the PC resin is selected from SABIC PC OQ1020L, and the melt index is 70±1g / 10min; The recycled PC resin formula is composed of the following raw materials in parts by weight: 10-20 parts of the compound modifier stored in the compound modifier storage tank (62), and 80-90 parts of crushed waste B with a particle size less than Nmm that has been sieved by a particle size sieve component (5) in the air-conditioning control panel waste shredding and recycling system.
10. A recycled PC resin prepared by using the air conditioner control panel waste crushing and recycling system according to any one of claims 1 to 9, characterized in that: The preparation method of the regenerated PC resin comprises the following steps: Step 1: placing the waste of air-conditioning control panel in an ultrasonic cleaning machine (1) for ultrasonic cleaning to remove pollutants on the surface of the waste of air-conditioning control panel, and then inputting the waste of cleaning into a drying assembly (2) for drying. The drying parameters are as follows: the temperature of the hot air input into the hot air output pipe (23) is 75-80° C., and the wind speed is 1.5-2 m / s; the temperature in the first drying oven (22) is controlled to be 75-80° C., and the speed of the waste of air-conditioning control panel that has been ultrasonically cleaned and transmitted by the first conveyor belt conveyor (21) is 4 cm / s; the length of the first drying oven (22) is 8 m, and the waste of air-conditioning control panel that has been dried after the drying process is completed; Step 2: The dried waste air-conditioning control panel obtained in step 1 is input into the waste rapid cooling and embrittlement component (3) for rapid cooling and embrittlement treatment. The rapid cooling and embrittlement treatment parameters are as follows: the temperature of the low-temperature nitrogen input into the low-temperature nitrogen output pipe (331) is -80 to -60°C, the wind speed is 2-3m / s, the speed of the dried waste air-conditioning control panel transmitted by the second conveyor belt conveyor (31) is 4cm / s, the length of the heat preservation box (32) is 8m, and the rapid cooling and embrittlement treatment is completed to obtain the rapid cooling and embrittlement waste air-conditioning control panel; Step 3, the waste of the air-conditioning control panel that has undergone the rapid cooling and embrittlement treatment in step 2 is input into the multi-roller crushing assembly (4) for multi-roller crushing treatment, wherein X in the first crushing roller group (42) is 5 cm, Y in the second crushing roller group (43) is 2 mm, the rotation speed of the crushing roller A in the first crushing roller group (42) is 120-150 r / min, the rotation speed of the crushing roller B in the second crushing roller group (43) is 180-240 r / min, and the rotation speed of the high-speed crushing cutter head (45) is 800-1200 r / min, thereby obtaining crushed material; Step 4: The crushed material obtained after the multi-roll crushing process is input into the particle size screening component (5) for screening process. The mesh size of the screening net (52) is 3 mm. The crushed waste A with a particle size greater than 3 mm and the crushed waste B with a particle size less than 3 mm are screened out. The crushed waste A with a particle size greater than 3 mm is input into the multi-roll crushing component (4) for secondary crushing process. The crushed waste B with a particle size less than 3 mm is input into the crushed material storage tank (61) for standby use. Step 5: the compound modifier stored in the compound modifier storage tank (62) is metered into the mixing kettle (63) through the second metering tank (621); the crushed waste B in the crushed material storage tank (61) is metered into the mixing kettle (63) through the first metering tank (611); the crushed waste B and the compound modifier are evenly mixed at a rotation speed of 400-500 r / min in the mixing kettle (63) to obtain a regenerated recovery composite material; the mass ratio of the compound modifier to the crushed waste B is (5-30):(70-95); Step 6, the obtained recycled composite material is sequentially passed through a screw extruder (7), a silicone oil cooling tank (8), and a granulator (9) for melt extrusion, wire drawing, cooling, and granulation to obtain a recycled PC resin that can be directly used for injection molding of an automobile air-conditioning control panel; the obtained recycled PC resin needs to be dried before injection molding.
Citation Information
Cited By
Pretreatment process and device for waste plastic recovery