Laminated glass and vehicle
By adjusting the thermal expansion coefficient of the ink shielding layer to the glass plate, the problem of laminated glass prone to cracking under impact is solved, the impact strength and durability of the product are improved, and the strength and wear resistance of the shielding area are achieved.
Patent Information
- Application Number
- CN202411077684.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-08-07
AI Technical Summary
Laminated glass is prone to rupture due to impact of stones on the road during loading or driving, which is mainly related to the mechanical stress drop caused by the mismatch of the thermal expansion coefficient of the ink shielding layer and the thermal expansion coefficient of the glass plate.
By controlling the proportional relationship between the thermal expansion coefficient of the ink shielding layer and the thermal expansion coefficient of the inner and outer glass plates, it is ensured that it is between 0.9 and 1.1, and the thermal expansion coefficient of the ink shielding layer is reduced to 80×10-7~87×10-7. Increase the strength of the shielded area and reduce the thermal expansion coefficient by adjusting the ink composition and sintering temperature.
It significantly improves the ability of laminated glass to not break under impact, improves the yield and durability of the product, and ensures the impact strength and wear resistance of the shielded area.
Smart Images

Figure CN118876524A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of vehicle technology, and in particular to a laminated glass and a vehicle. Background Art
[0002] Laminated glass for vehicles is a type of safety glass that perfectly combines the hardness of glass with the flexibility of plastic by sandwiching a transparent high-toughness plastic film between multiple layers of glass, significantly enhancing the impact resistance and safety of the glass when it breaks. When this type of glass is impacted, even if it breaks, it will remain intact due to the plastic film in the middle, greatly reducing the risk of injury caused by flying glass fragments. Generally speaking, the inner and outer glass panels of laminated glass are heat-strengthened or semi-tempered glass, which is 2 to 4 times stronger than ordinary glass, which means that the glass is less likely to break under the same impact force. However, with the functional requirements of laminated glass for vehicles, in actual production, there is a problem that laminated glass is prone to glass breakage when it is hit during loading or when it is hit by stones on the road during driving. Summary of the invention
[0003] Based on this, the first aspect of the present application provides a laminated glass, and its technical solution is as follows:
[0004] A laminated glass comprises an outer glass plate, an inner glass plate, a thermoplastic interlayer and an ink shielding layer, wherein the outer glass plate has a first surface and a second surface, the inner glass plate has a third surface and a fourth surface, the thermoplastic interlayer is located between the second surface and the third surface, and the ink shielding layer is located on at least one of the second surface, the third surface and the fourth surface;
[0005] The thermal expansion coefficient of the ink shielding layer is less than 90×10 -7 ; The ratio of the thermal expansion coefficient of the ink shielding layer to the thermal expansion coefficient of the outer glass plate or the inner glass plate is 0.9~1.1.
[0006] A second aspect of the present application provides a vehicle, which includes the laminated glass as described above.
[0007] Compared with the traditional solution, this application has the following beneficial effects:
[0008] The inventor of the present application has found that the problem that the laminated glass is prone to glass breakage when it is hit by stones on the road during loading or driving is related to the ink shielding layer of the laminated glass. Specifically, due to the requirement for the functionalization of laminated glass, additional materials are usually arranged on the laminated glass, such as some conductive circuits, antenna cover plates, antenna connectors, etc. These additional materials are generally fixed on the edge of the laminated glass, and the ink shielding layer is used to shield and beautify these additional materials. However, the thermal expansion coefficient of the ink shielding layer is different from the thermal expansion coefficient of the inner and outer glass plates of the laminated glass. During the cooling and forming stage, the ink shielding layer generates certain mechanical stress on the inner and outer glass plates, which will cause the strength of the area to decrease. Based on the above findings, the inventor has verified through experiments that in the actual production process, the proportional relationship between the thermal expansion coefficient of the ink shielding layer and the thermal expansion coefficient of the inner and outer glass plates is specified to improve the strength of the shielding area where the ink shielding layer is located after the laminated glass is formed, so as to improve the problem that the laminated glass is prone to glass breakage when it is hit by stones on the road during loading or driving, and improve the product yield. BRIEF DESCRIPTION OF THE DRAWINGS
[0009] In order to more clearly illustrate the technical solutions in the embodiments of the present application and to more completely understand the present application and its beneficial effects, the following is a brief introduction to the drawings required for the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can obtain other drawings based on these drawings without creative work.
[0010] Figure 1 is a schematic structural diagram of a laminated glass according to an embodiment;
[0011] Figure 2 For along Figure 1 Sectional view along line A-A'. DETAILED DESCRIPTION
[0012] The present application will be further described in detail below in conjunction with specific embodiments. The present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the disclosure of the present application more thoroughly understood.
[0013] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which this application belongs. The terms used herein in the specification of this application are only for the purpose of describing specific embodiments and are not intended to limit this application.
[0014] the term
[0015] Unless otherwise specified or incompatible herewith, the terms and phrases used herein shall have the following meanings:
[0016] In the present application, "plurality", "multiple", "multiple times", "plurality", etc., unless otherwise specified, refer to a number greater than 2 or equal to 2. For example, "one or more" means one or greater than or equal to two.
[0017] In the present application, “several” means at least one, such as one, two, etc., unless otherwise clearly defined.
[0018] In this application, "optionally", "optional" and "optional" refer to optional, that is, to any one of the two parallel schemes of "yes" or "no". If multiple "options" appear in a technical solution, unless otherwise specified and there is no contradiction or mutual restriction, each "optional" is independent.
[0019] In this application, in the "first aspect", "second aspect", "third aspect", "fourth aspect", etc., the terms "first", "second", "third", "fourth", etc. are used only for descriptive purposes and cannot be understood as indicating or implying relative importance or quantity, nor can they be understood as implicitly indicating the importance or quantity of the indicated technical features. Moreover, "first", "second", "third", "fourth", etc. only serve the purpose of non-exhaustive enumeration and description, and it should be understood that they do not constitute a closed limitation on quantity.
[0020] In the present application, when referring to a numerical interval (i.e., a numerical range), unless otherwise specified, the optional numerical distribution within the above numerical interval is deemed to be continuous and includes the two numerical endpoints of the numerical range (i.e., the minimum value and the maximum value), and every numerical value between the two numerical endpoints.
[0021] The temperature parameters in this application, unless otherwise specified, are allowed to be either constant temperature treatment or to vary within a certain temperature range. It should be understood that the constant temperature treatment allows the temperature to fluctuate within the accuracy range controlled by the instrument. Fluctuations within the range of ±5°C, ±4°C, ±3°C, ±2°C, and ±1°C are allowed.
[0022] In the present application, %(w / w) and wt% both represent weight percentage, %(v / v) refers to volume percentage, and %(w / v) refers to mass volume percentage.
[0023] The first aspect of the present application provides a laminated glass. In one embodiment, see Figure 1 and Figure 2The laminated glass 100 comprises an outer glass plate 11, an inner glass plate 12, a thermoplastic interlayer 13 and an ink shielding layer 14, wherein the outer glass plate 11 has a first surface and a second surface, the inner glass plate has a third surface and a fourth surface, the thermoplastic interlayer 13 is located between the second surface and the third surface, and the ink shielding layer 14 is located on the second surface;
[0024] The thermal expansion coefficient of the ink shielding layer is less than 90×10 -7 ; The ratio of the thermal expansion coefficient of the ink shielding layer to the thermal expansion coefficient of the outer glass plate or the inner glass plate is 0.9~1.1.
[0025] Among them, the ratio of the thermal expansion coefficient of the ink shielding layer to the thermal expansion coefficient of the outer glass plate or the inner glass plate is 0.9~1.1, which means: the ratio of the thermal expansion coefficient of the ink shielding layer to the thermal expansion coefficient of the outer glass plate is 0.9~1.1, or the ratio of the thermal expansion coefficient of the ink shielding layer to the thermal expansion coefficient of the inner glass plate is 0.9~1.1.
[0026] Further optionally, the ratio of the thermal expansion coefficient of the ink shielding layer to the thermal expansion coefficient of the outer glass plate or the inner glass plate is 0.95-1.05.
[0027] In this embodiment, the ink shielding layer 14 is located on the second surface. In other embodiments, the ink shielding layer 14 is located on the third surface or the fourth surface. In this embodiment, the number of layers of the ink shielding layer 14 is one layer, and in other embodiments, the number of layers of the ink shielding layer 14 is multiple layers. In this application, the ink shielding layer 14 is located on at least one of the second surface, the third surface, and the fourth surface.
[0028] The inventor of the present application has found that the problem that the laminated glass is prone to glass breakage when it is hit by stones on the road during loading or driving is related to the ink shielding layer of the laminated glass. Specifically, due to the requirement for the functionalization of laminated glass, additional materials are usually arranged on the laminated glass, such as some conductive circuits, antenna cover plates, antenna connectors, etc. These additional materials are generally fixed on the edge of the laminated glass, and the ink shielding layer is used to shield and beautify these additional materials. However, the thermal expansion coefficient of the ink shielding layer is different from the thermal expansion coefficient of the inner and outer glass plates of the laminated glass. During the cooling and forming stage, the ink shielding layer generates certain mechanical stress on the inner and outer glass plates, which will cause the strength of the area to decrease. Based on the above findings, the inventor has verified through experiments that in the actual production process, the proportional relationship between the thermal expansion coefficient of the ink shielding layer and the thermal expansion coefficient of the inner and outer glass plates is specified to improve the strength of the shielding area where the ink shielding layer is located after the laminated glass is formed, so as to improve the problem that the laminated glass is prone to glass breakage when it is hit by stones on the road during loading or driving, and improve the product yield.
[0029] Optionally, the area where the ink shielding layer is located is defined as the shielding area, and the breaking strength of the laminated glass in the shielding area is ≥1500N. The breaking strength refers to the force applied to the laminated glass when it breaks in the double ring test. The double ring test is used to measure the strength of glass. The laminated glass is pressed by two upper and lower devices until the laminated glass breaks.
[0030] Optionally, the area where the ink shielding layer is located is defined as a shielding area, and a stainless steel ball with a weight of 28g and a diameter of 19mm is used to perform a drop ball impact test in the shielding area, and the drop ball height is greater than or equal to 700mm. The drop ball impact test refers to a stainless steel ball with a weight of 28g and a diameter of 19mm falling freely from different heights onto the shielding area of the laminated glass, so that the shielding area of the laminated glass is subjected to the drop ball impact. The drop ball height refers to the height at which the shielding area of the laminated glass is at least not broken by the drop ball impact. For example, a drop ball height of 700mm means that the glass can be guaranteed not to break when subjected to a drop ball from a height of 700mm.
[0031] Optionally, the elastic modulus of the ink shielding layer is 8GPa~10GPa. At this time, the elastic modulus of the ink shielding layer is relatively high, and the impact strength is relatively high, which is beneficial to improve the strength of the shielding area. The elastic modulus is an index of the stiffness of a material when subjected to force, indicating the material's ability to respond to stress. It reflects the degree of deformation of the material after being subjected to force. The larger the elastic modulus, the more difficult it is for the material to deform, and it has a higher rigidity. The ink shielding layer with a large elastic modulus can protect the shielding area of the laminated glass from external impact or scratches to a certain extent. The elasticity of the ink shielding layer can absorb part of the external impact energy and reduce the impact on the surface of the laminated glass. This can improve the wear resistance and durability of the laminated glass. There is less attention paid to the elastic modulus of the ink shielding layer in the market, resulting in the elastic modulus of the ink shielding layer formed by common inks being generally low, generally averaging around 6GPa. In this embodiment, the elastic modulus of the ink shielding layer is controlled to be 8GPa~10GPa, which is beneficial to improve the strength of the shielding area.
[0032] Optionally, the thermal expansion coefficient of the ink shielding layer is controlled to be 80×10 -7 ~87×10 -7 The thermal expansion coefficient of the ink shielding layer affects the strength of the shielding area.
[0033] In this embodiment, the outer glass plate and the inner glass plate can be heat-strengthened glass plates or semi-strengthened glass plates obtained by physically heating and forming float glass and then cooling it. Optionally, the thermal expansion coefficients of the outer glass plate and the inner glass plate are independently 82×10 -7 ~89×10 -7 For example, the thermal expansion coefficient of clear glass (white glass) is 82.6×10 -7 The thermal expansion coefficient of green glass is 84.6×10 -7 The thermal expansion coefficient of gray glass (gray glass) is 88.6×10 -7 .
[0034] The thermal expansion coefficient of the common ink shielding layer on the market is 90×10 -7 ~92×10 -7 In this embodiment, the thermal expansion coefficient of the ink shielding layer is controlled to be 80×10 -7 ~87×10 -7 , so that the thermal expansion coefficient of the ink shielding layer is close to that of the outer glass plate and the inner glass plate. When the ink shielding layer, the outer glass plate and the inner glass plate are heated and thermally expanded, the thermal stress between the ink shielding layer, the outer glass plate and the inner glass plate is small when the temperature changes, which can improve the problem of glass cracking or breaking caused by large thermal stress in the shielding area. By controlling the thermal expansion coefficient of the ink shielding layer to 80×10-7 ~87×10 -7 , which is beneficial to improve the strength of the shielded area.
[0035] It can be understood that the thermal expansion coefficient of the ink shielding layer is determined by the chemical composition of the ink. As the temperature rises, the thermal motion amplitude of the particles in the ink increases, overcoming the force between the particles, and the distance between the particles becomes larger, which is externally manifested as expansion. For inks whose main components are oxides, the force between the particles is the bond force 2Z / r2 between various cations and oxygen ions. The greater the bond force, the more difficult the ink is to expand, and the smaller the thermal expansion coefficient is. On the contrary, the greater the expansion coefficient of the ink. Among the bond forces between various cations and oxygen ions, the bond strength of Si-O is relatively large, so, in general, the greater the content of quartz glass in the ink, the smaller the expansion coefficient is. However, the decrease in quartz glass in the ink composition will reduce the temperature during ink sintering, reduce the temperature difference between the ink and the glass after molding, and reduce the mechanical stress of the ink on the glass. In addition, in addition to SiO2, the content of alkali metals or alkaline earth metals in the ink will also affect the expansion coefficient of the ink. The greater the content of alkali metals or alkaline earth metals in the ink, the greater the expansion coefficient. The content of SiO2 in the ink of this application is 30wt~50wt%. Compared with the SiO2 content of 50wt%~60wt% in traditional inks, the SiO2 content in the ink of the present application is relatively low, so the minimum sintering temperature of the ink can be reduced to about 580°C.
[0036] In addition, among the bond forces between cations and oxygen ions, RO-type bonds are relatively weak, so the greater the content of alkali metals or alkaline earth metals in the ink, the greater the expansion coefficient. The proportion of alkaline earth metal oxides in the ink of the present application is within 30wt%. Compared with the content of alkaline earth metal oxides in traditional inks of 30wt% to 50wt%, although the content of SiO2 is reduced in the ink of the present application, the content of alkaline earth metal oxides is also reduced, so that the thermal expansion coefficient of the entire ink can be controlled within a range that is more conducive to the strength of the glass.
[0037] The order of influence of alkali metal or alkaline earth metal oxides on the expansion coefficient of ink is: Rb2O>Cs2O>K2O>Na2O>Li2O>Ba2O>SiO>Ca2O>ZnO>MgO>BeO. The higher the ranking, the stronger the RO type bond strength, and the less favorable it is for reducing the thermal expansion coefficient of the ink of the shielding layer. The above ranking can be referred to to select the oxides in the ink. The content of Na2O in the ink of this application is 0~15wt%. In addition, in the ink of this application, the content of Bi2O3 is 25wt%~75wt%, and the content of Al2O3 is 3wt%~4wt%. In addition, from the overall structure of the ink shielding layer, the network skeleton of the ink shielding layer plays an important role in thermal expansion. Si-O forms a three-dimensional network with high rigidity and is not easy to expand. BO forms a BO3 layered or chain network, which is easy to expand. Therefore, the thermal expansion coefficient of the ink containing B2O3 is much larger than that of the ink containing SiO2. The content of B2O3 in the ink of the present application is 15wt%~20wt%. However, when BO3 is converted into BO4, it is beneficial to reduce the thermal expansion coefficient. Therefore, it is possible to try to convert BO3 in the ink containing B2O3 into BO4. At this time, it is necessary to control the content of alkali metal or alkaline earth metal oxide in the ink to avoid disconnection of the BO4 network, which leads to an increase in the expansion coefficient. In summary, in this embodiment, the thermal expansion coefficient of the ink shielding layer can be 80×10 -7 ~87×10 -7 According to the needs, select the formula ingredients and content of the ink.
[0038] Optionally, the sintering temperature of the ink shielding layer is at least 580°C. Further optionally, the sintering temperature of the ink shielding layer is controlled to be 580°C to 620°C. The sintering temperature of the ink shielding layer affects the strength of the shielding area. The formula components and content of the ink can be selected according to the requirement that the sintering temperature of the ink shielding layer is 580°C to 620°C.
[0039] In common inks on the market, the content of SiO2 accounts for 50wt%~60wt%, and the content of alkaline earth metal oxides accounts for 30wt%~50wt%. The required sintering temperature is 620℃~640℃. In this embodiment, the content ratio of SiO2 and alkaline earth metal oxides in the ink is changed so that the content of SiO2 reaches 30wt~50wt%, and the content of alkaline earth metal oxides accounts for ≤30wt%. At this time, the range of sintering temperature can be increased to 580℃~620℃. After lowering the minimum sintering temperature of the ink, it is beneficial to lower the forming temperature of the glass, reduce the temperature difference between the ink shielding layer and the outer glass plate and / or the inner glass plate after hot forming, and reduce the mechanical stress of the ink shielding layer on the outer glass plate and the inner glass plate.
[0040] Optionally, the boron oxide content in the ink is increased to 15wt%~20wt% (the boron oxide content in common inks is less than 15wt%), and the aluminum oxide content is increased to 3wt%~4wt% (the aluminum oxide content in common inks is less than 1wt%) to increase the elastic modulus of the ink shielding layer, improve the impact strength of the ink shielding layer, and thereby improve the strength of the shielding area of the laminated glass.
[0041] Optionally, the thickness of the ink shielding layer is 14 μm to 24 μm. The above thickness can take into account both the shielding performance of the ink shielding layer and the impact strength of the shielding area. Further optionally, the thickness of the ink shielding layer is 14 μm to 18 μm.
[0042] It can be understood that the strength of the shielding area of the laminated glass is also related to the strength of the outer glass plate and the inner glass plate of the laminated glass. In this embodiment, the outer glass plate and the inner glass plate can be heat-strengthened glass plates or semi-tempered glass plates obtained by physically heating and forming float glass and then cooling it. Optionally, the surface compressive stress of the outer glass plate and the inner glass plate is independently between 8MPa and 64MPa. Among them, the surface compressive stress of the heat-strengthened glass plate is between 8MPa and 20MPa, and the surface compressive stress of the semi-tempered glass plate is between 24MPa and 64MPa. The edge tensile stress of the outer glass plate and the inner glass plate in the shielding area is independently ≤17.5MPa. Among them, the edge tensile stress of the heat-strengthened glass plate in the shielding area is ≤12MPa, and the edge tensile stress of the semi-tempered glass plate in the shielding area is ≤17.5MPa.
[0043] It can be understood that the thickness of the outer glass plate and the inner glass plate are independently between 0.5 mm and 3.0 mm, and the present application does not impose any limitation on this.
[0044] Optionally, the thickness of the thermoplastic intermediate layer is between 0.38 mm and 1.52 mm, which is not limited in the present application.
[0045] Optionally, the material of the thermoplastic intermediate layer is selected from at least one of polyvinyl butyral (PVB), ethylene vinyl acetate (EVA), polycarbonate (PC), polyvinyl chloride (PVC), polyacrylate (PA), polymethyl methacrylate (PMMA), polyurethane (PUR), and ionomer membrane (SGP).
[0046] It can be understood that the present embodiment is laminated glass.
[0047] The following is further described in conjunction with specific embodiments and comparative examples. The raw materials involved in the following specific embodiments and comparative examples, unless otherwise specified, can all be commercially available, the instruments used, unless otherwise specified, can all be commercially available, and the processes involved, unless otherwise specified, are all routinely selected by those skilled in the art.
[0048] See also Figure 1 and Figure 2 The structure of laminated glass is: 2.1mm gray glass (thermal expansion coefficient is 88.6×10 -7 , outer glass plate) + 0.76mm PVB + 2.1mm gray glass (thermal expansion coefficient is 88.6×10 -7 , inner glass plate), the ink shielding layer is sintered to form the edge of the second surface according to the parameters in Table 1 and Table 2. The thermal expansion coefficient of the ink shielding layer in the embodiment is 80×10 -7 ~87×10 -7 The thermal expansion coefficient of the ink shielding layer of the comparative example is 90×10 -7 ~92×10 -7 The thickness of the ink shielding layer is shown in Table 1 and Table 2.
[0049] The thermal expansion coefficient of the ink shielding layer was tested, and the results are shown in Tables 1 and 2.
[0050] With reference to the EN1288-5 standard, during the double ring test, the area where the ink shielding layer is located is defined as the shielding area. Pressure is applied to the shielding area of the laminated glass at a speed of 0.5 mm / min. The rupture strength and average value results are shown in Tables 1 and 2.
[0051] The area where the ink shielding layer is located is defined as the shielding area. A stainless steel ball with a weight of 28 g and a diameter of 19 mm is used to perform a drop ball impact test on the shielding area. The drop ball heights are shown in Tables 1 and 2.
[0052] Table 1
[0053]
[0054] Table 2
[0055]
[0056] It can be seen from Table 1 and Table 2 that in the embodiment, the thermal expansion coefficient of the ink shielding layer is less than 90×10 -7, and the ratio of the thermal expansion coefficient of the ink shielding layer to the thermal expansion coefficient of the inner and outer glass plates is between 0.9 and 1.1, which can improve the strength of the shielding area. In some further embodiments, the ratio of the thermal expansion coefficient of the ink shielding layer to the thermal expansion coefficient of the inner and outer glass plates is between 0.95 and 1.05, which can further improve the problem of easy glass breakage caused by the impact of stones on the road during loading or driving.
[0057] In the comparative example, the thermal expansion coefficient of the ink shielding layer exceeds 90×10 -7 When the content of SiO2 in the ink is in the range of 50wt%~60wt%, the sintering temperature is at least about 620℃. Due to the inconsistent cooling speed of the ink and the glass, the temperature difference between the ink and the glass is widened during the cooling process of the glass after high-temperature molding, which in turn causes the ink to produce mechanical stress on the glass and reduce the strength of the glass. At the same time, the content of alkaline earth metal oxide is 30wt%~50wt%, which may cause greater thermal stress between the ink and the glass during the temperature change process. This thermal stress will more easily cause the glass to crack or break.
[0058] In addition, in Table 1 and Table 2 of the present application, the ink of the embodiment has a significant improvement in the compressive resistance in the double ring test by reducing the thickness of the ink layer, compared with the ink of the comparative example. In the comparative example, the glass can only obtain an improvement of no more than 50N in resistance to rupture by reducing the thickness of the ink, while in the embodiment, the improvement of at least 150N in resistance to rupture can be achieved.
[0059] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0060] The above-mentioned embodiments only express several implementation methods of the present application, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for a person of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present application, and these all belong to the protection scope of the present application. Therefore, the protection scope of the patent of the present application shall be subject to the attached claims.
Claims
1. A laminated glass, characterized in that: The invention comprises an outer glass plate, an inner glass plate, a thermoplastic intermediate layer and an ink shielding layer, wherein the outer glass plate has a first surface and a second surface, the inner glass plate has a third surface and a fourth surface, the thermoplastic intermediate layer is located between the second surface and the third surface, and the ink shielding layer is located on at least one of the second surface, the third surface and the fourth surface; The thermal expansion coefficient of the ink shielding layer is less than 90×10 -7 ; The ratio of the thermal expansion coefficient of the ink shielding layer to the thermal expansion coefficient of the outer glass plate or the inner glass plate is 0.9~1.
1.
2. The laminated glass according to claim 1, characterized in that: The ratio of the thermal expansion coefficient of the ink shielding layer to the thermal expansion coefficient of the outer glass plate or the inner glass plate is 0.95-1.
05.
3. The laminated glass according to claim 1, characterized in that: The area where the ink shielding layer is located is defined as a shielding area, and the breaking strength of the laminated glass in the shielding area is ≥1500N.
4. The laminated glass according to claim 1, characterized in that: The area where the ink shielding layer is located is defined as the shielding area. A stainless steel ball with a weight of 28 g and a diameter of 19 mm is used to perform a drop ball impact test in the shielding area, and the drop ball height is greater than or equal to 700 mm.
5. The laminated glass according to claim 1, characterized in that: The elastic modulus of the ink shielding layer is 8 GPa to 10 GPa.
6. The laminated glass according to any one of claims 1 to 5, characterized in that: The thermal expansion coefficient of the ink shielding layer is 80×10 -7 ~87×10 -7 .
7. The laminated glass according to any one of claims 1 to 5, characterized in that: The thermal expansion coefficients of the outer glass plate and the inner glass plate are each independently 82×10 -7 ~89×10 -7 .
8. The laminated glass according to any one of claims 1 to 5, characterized in that: The ink of the ink shielding layer includes SiO2 and alkaline earth metal oxide, the proportion of SiO2 in the ink is 30wt~50wt%, and the proportion of the alkaline earth metal oxide in the ink is within 30wt%.
9. The laminated glass according to any one of claims 1 to 5, characterized in that: The ink of the ink shielding layer includes boron oxide and aluminum oxide, wherein the proportion of the boron oxide in the ink is 15wt%-20wt%, and the proportion of the aluminum oxide in the ink is 3wt%-4wt%.
10. The laminated glass according to any one of claims 1 to 5, characterized in that: The sintering temperature of the ink shielding layer is at least 580°C.
11. The laminated glass according to any one of claims 1 to 5, characterized in that: The ink shielding layer has a thickness of 14 μm to 24 μm.
12. The laminated glass according to claim 11, characterized in that: The thickness of the ink shielding layer is 14 μm to 18 μm.
13. The laminated glass according to any one of claims 1 to 5 and 12, characterized in that: The surface compressive stress of the outer glass plate and the inner glass plate is independently between 8 MPa and 64 MPa, and the edge tensile stress of the shielding area is independently ≤17.5 MPa.
14. A vehicle, characterized in that: The laminated glass comprises the laminated glass according to any one of claims 1 to 13.
Citation Information
Patent Citations
Method for screening ink for laminated glass and laminated glass
CN107512855A
High-acid-resistance anti-sticking shielding silver paste ink for automobile rear windshield and preparation method thereof
CN112125517A
Shock-resistant tempered glass ink, preparation method and application thereof, and shock-resistant tempered glass
CN115926525A
Laminated glass with low HIC value and preparation method thereof
CN116476471A
Vehicle window glass and manufacturing method therefor, vehicle laminated glass, and vehicle windshield
US20240246321A1