Preparation method of graphene-based material
Through microwave plasma continuous emission device, microwave processing of graphite oxide-based materials is achieved, high efficiency, low cost and large-scale preparation of graphene is solved, the problems of complex and high cost in the existing technology are solved, and the material weight is improved Present.
Patent Information
- Application Number
- CN202411147242.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-01
AI Technical Summary
In the existing graphene preparation methods, especially the reduction process is complex and low efficiency, and it is difficult to achieve sufficient reduction of graphite oxide or graphene oxide, resulting in poor reproducibility and high cost of graphene, making it difficult to prepare on a large scale.
Using microwave plasma continuous emission device, the continuous porous reduced graphene oxide film is used as the microwave emission source. By microwave processing of graphite oxide-based materials, it can be efficiently reduced to graphene, and can be combined with inorganic non-metallic materials to form high efficiency. Low-cost graphene-based materials.
It realizes high efficiency, low cost and large-scale preparation of graphene, and improves the reproducibility of materials, solving the problems of complex and high cost in the prior art.
Smart Images

Figure CN118877882A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of graphene preparation, and in particular to a method for preparing a graphene-based material. Background Art
[0002] Graphene is a new type of carbon material with a two-dimensional nano-plane structure. It has excellent optical, electrical, thermal, and mechanical properties, as well as a large specific surface area and excellent material compatibility. It has been widely developed and applied in electrochemical energy storage, new energy development, environmental governance, biomedicine, equipment protection, and aerospace. At present, the technical paths for preparing graphene mainly include mechanical exfoliation, chemical exfoliation, epitaxial growth, chemical synthesis, and chemical vapor deposition. Among them, the chemical exfoliation method is more widely used than other methods due to its low cost and the fact that it does not require special equipment.
[0003] The chemical exfoliation method mainly includes two basic steps: oxidizing graphite flakes to produce graphite oxide or graphene oxide, and reducing graphite oxide or graphene oxide to produce graphene. A variety of effective methods have been developed for the process of oxidizing graphite flakes to produce graphite oxide or graphene oxide, and market-based large-scale production applications have been realized, such as the Hummers method, the Standenmaier method, the Brodie method, the electrochemical oxidation exfoliation method, and the chemical method based on K2FeO4. The process of reducing graphite oxide or graphene oxide to produce graphene has currently formed methods such as high-temperature thermal reduction, chemical reduction, microwave reduction, photoreduction, plasma reduction, electrochemical reduction, and flame-induced reduction. However, the implementation process of most reduction methods is complicated and inefficient, and it is difficult to apply them on a large scale. More importantly, in the above-mentioned reduction methods, except for microwave reduction, it is almost difficult to achieve sufficient reduction of graphite oxide or graphene oxide. Although the microwave reduction method is highly energy efficient, the graphene prepared directly by microwave reduction not only has poor reproducibility, but also has a high degree of dependence on the properties of graphite oxide or graphene oxide precursors, and it is difficult to achieve efficient and reproducible reduction of graphite oxide or graphene oxide from different sources. Therefore, how to efficiently achieve sufficient reduction of graphite oxide or graphene oxide to prepare graphene is still a technical problem that needs to be solved in the current wider application of graphene.
[0004] In addition, graphene has excellent electrical conductivity, thermal conductivity, and large specific surface area, and is widely used to modify other inorganic non-metallic materials, such as non-metallic oxides, metal oxides, sulfides, hydroxides, etc., to improve the electrical conductivity and thermal conductivity of inorganic non-metallic materials. However, the current preparation methods of inorganic non-metallic materials / graphene composites mainly include hydrothermal method, solid phase high temperature heat treatment, etc. These methods have the problems of high energy consumption, low efficiency and high cost.
[0005] Therefore, it is urgent to develop a method that is low in energy consumption, low in cost, efficient and capable of large-scale preparation of graphene-based materials. Summary of the invention
[0006] The object of the present invention is to provide a method for preparing a graphene-based material. The method provided by the present invention has low energy consumption, low cost, high efficiency and can prepare graphene-based materials on a large scale.
[0007] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0008] The present invention provides a method for preparing a graphene-based material, comprising the following steps:
[0009] (1) laying a continuous porous reduced graphene oxide film on the bottom of a barrel-shaped container to obtain a microwave plasma continuous emission device;
[0010] (2) laying the graphite oxide-based material in the microwave plasma continuous emission device obtained in step (1), performing microwave treatment, and obtaining the graphene-based material.
[0011] Preferably, the thickness of the continuous porous reduced graphene oxide film in step (1) is 15 to 40 μm.
[0012] Preferably, the method for preparing the continuous porous reduced graphene oxide film in step (1) comprises: contacting the graphene oxide film with the outer flame of the flame for sintering and reduction.
[0013] Preferably, the temperature of the outer flame of the flame is 500-600°C.
[0014] Preferably, the sintering reduction time is 1 to 3 seconds.
[0015] Preferably, the graphite oxide-based material in step (2) is obtained by mixing graphite oxide and / or graphene oxide with an inorganic non-metallic material to be modified, and the mass ratio of the graphite oxide and / or graphene oxide to the inorganic non-metallic material to be modified is 1:(0-20).
[0016] Preferably, the inorganic non-metallic material to be modified in step (2) includes one or more of non-metallic oxides, metal oxides, metal sulfides, metal hydroxides and metal salts.
[0017] Preferably, the microwave treatment in step (2) is performed more than once, the duration of each microwave treatment is 3 to 10 seconds, and the time interval between two microwave treatments is 3 to 5 minutes.
[0018] Preferably, the power of the microwave treatment in step (2) is 600-800W.
[0019] The present invention provides a method for preparing a graphene-based material, comprising the following steps: laying a continuous porous reduced graphene oxide film on the bottom of a barrel-shaped container to obtain a microwave plasma continuous emission device; laying a graphene oxide-based material in the microwave plasma continuous emission device, and performing microwave treatment to obtain a graphene-based material. The present invention lays a continuous reduced graphene oxide porous film on the bottom of the container as a microwave plasma emission source. On the one hand, during microwave treatment, the reduced graphene oxide can be used to absorb a large amount of microwaves and quickly release a large amount of heat, while the generated heat is evenly distributed throughout the reduced graphene oxide film, thereby causing the entire reduced graphene oxide film to emit uniform plasma; on the other hand, the loose and porous characteristics of the reduced graphene oxide can be used to continuously absorb air and continuously ionize the air to form plasma, while preventing the strong airflow impact pressure generated by thermal expansion from causing the reduced graphene oxide film to be peeled off and destroyed, thereby causing it to be unable to continuously generate plasma; in addition, by this method, the reduction of graphene oxide-based materials, such as graphite oxide and / or graphene oxide to graphene is not affected by the source, properties, structure and other properties of the raw materials, and has good reproducibility. This method is simple to operate, has low energy consumption and high efficiency, and can be applied to the large-scale preparation of graphene and graphene-based composite materials by reducing graphene oxide and / or graphene oxide. The results of the examples show that the method provided by the present invention has low energy consumption, low cost, and can prepare graphene-based materials efficiently and on a large scale, and the obtained graphene-based materials have good reproducibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is an optical photograph of the microwave plasma continuous emission device prepared in Example 1 of the present invention;
[0021] Figure 2 This is an optical photograph of the microwave plasma continuously generated by the microwave plasma continuous emission device prepared by the present invention before adding materials;
[0022] Figure 3 This is an optical photograph of the microwave plasma continuous emission device prepared in Example 1 after adding materials;
[0023] Figure 4 This is an optical photograph of the microwave plasma continuous emission device prepared in Example 1 after microwave treatment after adding materials;
[0024] Figure 5 This is the XRD pattern of the manganese oxide / graphene composite material prepared in Example 1;
[0025] Figure 6 This is a SEM image of the manganese oxide / graphene composite material prepared in Example 1;
[0026] Figure 7 This is the XRD pattern of the hard carbon / graphene composite material prepared in Example 2;
[0027] Figure 8 SEM image of the hard carbon / graphene composite material prepared in implementation 2;
[0028] Fig. 9 This is the XRD pattern of the nickel oxide / graphene composite material prepared in Example 3;
[0029] Fig.10 This is a SEM image of the nickel oxide / graphene composite material prepared in Example 3;
[0030] Fig.11 This is the XRD pattern of the lithium cobalt oxide / graphene composite material prepared in Example 4;
[0031] Fig.12 This is a SEM image of the lithium cobalt oxide / graphene composite material prepared in Example 4;
[0032] Fig.13 This is the XRD pattern of graphene prepared in Example 6;
[0033] Fig.14 This is the SEM image of the graphene prepared in Example 6. DETAILED DESCRIPTION
[0034] The present invention provides a method for preparing a graphene-based material, comprising the following steps:
[0035] (1) laying a continuous porous reduced graphene oxide film on the bottom of a barrel-shaped container to obtain a microwave plasma continuous emission device;
[0036] (2) laying the graphite oxide-based material in the microwave plasma continuous emission device obtained in step (1), performing microwave treatment, and obtaining the graphene-based material.
[0037] The present invention lays a continuous porous reduced graphene oxide film on the bottom of a barrel-shaped container to obtain a microwave plasma continuous emission device.
[0038] The present invention has no particular limitation on the size of the barrel-shaped container, which can be adjusted according to the amount of graphene-based material to be prepared. In the present invention, the volume of the barrel-shaped container is preferably 100 to 250 mL.
[0039] In the present invention, the thickness of the continuous porous reduced graphene oxide film is preferably 15 to 40 μm, more preferably 20 to 30 μm. The present invention is more conducive to continuous emission of plasma by controlling the thickness of the continuous porous reduced graphene oxide film within the above range.
[0040] In the present invention, the method for preparing the continuous porous reduced graphene oxide film preferably comprises: contacting the graphene oxide film with the outer flame of the flame and performing sintering reduction. By adopting the above preparation method, the present invention can quickly reduce and peel the graphene oxide film into a reduced graphene oxide film, and, during the reduction process, a continuous porous structure is formed in the reduced graphene oxide film.
[0041] The present invention has no particular limitation on the source of the graphite oxide, and any graphite oxide obtained by a conventional preparation method may be used. In the present invention, the graphite oxide is preferably prepared by the Hummers method, the Standenmaier method or the Brodie method, and the graphite oxide is prepared by oxidation of flake graphite.
[0042] In the present invention, the temperature of the outer flame of the flame is preferably 500-600°C, more preferably 550-600°C; the sintering reduction time is preferably 1-3s, more preferably 1-2s. The present invention can fully reduce the graphite oxide film and form a continuous porous loose reduced graphene oxide film by controlling the above parameters.
[0043] After obtaining the microwave plasma continuous emission device, the present invention lays the graphite oxide-based material in the microwave plasma continuous emission device and performs microwave treatment to obtain the graphene-based material.
[0044] In the present invention, the graphite oxide-based material is preferably obtained by mixing graphite oxide and / or graphene oxide with an inorganic non-metallic material to be modified, and the mass ratio of the graphite oxide and / or graphene oxide to the inorganic non-metallic material to be modified is preferably 1:(0-20), and more preferably 1:(0-10). In the present invention, when the mass of the inorganic non-metallic material to be modified is 0, graphene is obtained by the method of the present invention; when the mass of the inorganic non-metallic material to be modified is not 0, a graphene / inorganic non-metallic material composite material is obtained. The present invention does not specifically limit the method for mixing the graphite oxide and / or graphene oxide with the inorganic non-metallic material to be modified, and the components can be evenly mixed using a mixing method well known to those skilled in the art.
[0045] The present invention does not specifically limit the sources of the graphite oxide and graphene oxide, and can be prepared by commercial products well known to those skilled in the art, or by well-known preparation methods. Since the present invention reduces graphite oxide or graphene oxide by plasma continuously released by a microwave plasma continuous emission device, the sources of graphite oxide and graphene oxide are not limited, and the scope of application is wide, which solves the problem that the graphene prepared by the microwave reduction method in the prior art not only has poor reproducibility, but also has a high degree of dependence on the characteristics of graphite oxide or graphene oxide precursors. In the present invention, the preparation method of the graphite oxide is preferably Hummers method, Standenmaier method or Brodie method, and graphite oxide or graphene oxide is prepared by oxidation of flake graphite.
[0046] In the present invention, the inorganic non-metallic material to be modified includes one or more of non-metallic oxides, metal oxides, metal sulfides, metal hydroxides and metal salts. In the present invention, the inorganic non-metallic material to be modified is an active material, but its thermal conductivity and electrical conductivity are poor, so the electrical conductivity and thermal conductivity of the inorganic non-metallic material are improved by using graphene with electrical conductivity and thermal conductivity.
[0047] The present invention has no special limitation on the thickness of the graphite oxide-based material laid in the microwave plasma continuous emission device, and can be adjusted as needed. In the present invention, when the volume of the barrel-shaped container is preferably 100 mL and the thickness of the continuous porous reduced graphene oxide film is 15 μm, the thickness of the graphite oxide-based material laid in the microwave plasma continuous emission device is preferably <6 cm.
[0048] In the present invention, the microwave treatment is preferably performed more than once. The number of microwave treatments is not particularly limited and can be adjusted according to the reduction of graphite oxide and / or graphene oxide, as long as the graphite oxide and / or graphene oxide can be fully reduced to graphene.
[0049] In the present invention, the time of each microwave treatment is preferably 3 to 10 seconds, more preferably 4 to 6 seconds; the time interval between two microwave treatments is preferably 3 to 5 minutes, more preferably 5 minutes. The present invention can fully reduce graphite oxide and / or graphene oxide by controlling the parameters of the above microwave treatment without destroying the structure of graphene; when the inorganic non-metallic material to be modified is added, it is also beneficial for graphene to fully combine with the inorganic non-metallic material to be modified.
[0050] In the present invention, the power of the microwave treatment is preferably 600-800W, more preferably 700-800W. The present invention has no special limitation on the temperature of the microwave treatment. The present invention is more conducive to fully reducing graphite oxide and / or graphene oxide by controlling the power of the microwave treatment to be within the above range; when the inorganic non-metallic material to be modified is added, it is also conducive to fully combining graphene with the inorganic non-metallic material to be modified. The present invention has no special limitation on the device for the microwave treatment, and a conventional microwave device can be used. In the present invention, the device for the microwave treatment is preferably a household microwave oven.
[0051] The preparation method provided by the present invention has low energy consumption, low cost, and can prepare graphene-based materials efficiently and on a large scale. The obtained graphene-based materials have good reproducibility, which solves the technical problems of high energy consumption, high cost, low efficiency and inability to prepare on a large scale in existing graphene-based materials.
[0052] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0053] Example 1
[0054] A method for preparing a graphene-based material, comprising the following steps:
[0055] (1) taking a graphite oxide film and exposing it to the outer flame of a flame for 2 seconds to obtain a continuous porous reduced graphene oxide film, and then spreading 10 mg of the flame-reduced reduced graphene oxide film on the bottom of a barrel-shaped container with a volume of 250 mL, with a thickness of 20 μm, to obtain a microwave plasma continuous emission device;
[0056] The graphite oxide film was prepared by the Hummers method in the chemical exfoliation method: 1g of flake graphite and 0.5g of sodium nitrate were weighed and placed in a 250mL round-bottom flask, 23mL of concentrated sulfuric acid with a weight percentage concentration of 98% was measured and added to the round-bottom flask, a magnet was added, the round-bottom flask was placed in an ice-water bath, and stirred for 30min, 3g of potassium permanganate was weighed and added to the reactor, and stirring was continued for 1h. After the reaction was completed, the reactor was transferred to a 35°C water bath and stirred for 30min. 50 mL of distilled water was measured and added to the round-bottom flask, and then the round-bottom flask was transferred to an oil bath at 98° C. and stirred for 15 min. 140 mL of distilled water and 10 mL of 30% H2O2 were added in sequence. After the reaction system finally turned bright yellow, it was centrifuged, and then washed with 500 mL of 5% HCl hydrochloric acid and distilled water in sequence until the solution became neutral. The solution was then placed on the surface of a watch glass and dried to obtain graphite oxide (oxygen atom content of 25 to 30 at.%) for later use.
[0057] (2) After 1 g of the graphite oxide prepared in step (1) and 100 mL of water are stirred evenly, 5 g of manganese dioxide is added, the mixture is stirred evenly, and then dried at 50° C. for 48 h. The mixture is then laid in the microwave plasma continuous emission device obtained in step (1) with a thickness of 2 cm. The microwave plasma continuous emission device is then placed in a household microwave oven, the power is set to 800 W, and microwave treatment is performed for 3 seconds to obtain a manganese oxide / graphene composite material.
[0058] Example 2
[0059] A method for preparing a graphene-based material, comprising the following steps:
[0060] (1) The graphite oxide film prepared in step (1) of Example 1 was exposed to the outer flame of a flame for 2 seconds to obtain a continuous porous reduced graphene oxide film, and then 10 mg of the flame-reduced reduced graphene oxide film was spread evenly on the bottom of a barrel-shaped container with a volume of 250 mL, with a thickness of 20 μm, to obtain a microwave plasma continuous emission device;
[0061] (2) After 1 g of the graphite oxide prepared in step (1) and 100 mL of water are stirred evenly, 5 g of hard carbon is added, and after stirring and mixing evenly, it is dried at 50°C for 48 h, and then laid in the microwave plasma continuous emission device obtained in step (1) with a thickness of 2 cm, and then the microwave plasma continuous emission device is placed in a household microwave oven, the power is set to 800 W, and microwave treatment is performed for 3 seconds to obtain a hard carbon / graphene composite material).
[0062] Example 3
[0063] A method for preparing a graphene-based material, comprising the following steps:
[0064] (1) The graphite oxide film prepared in step (1) of Example 1 was exposed to the outer flame of a flame for 2 seconds to obtain a continuous porous reduced graphene oxide film, and then 10 mg of the flame-reduced reduced graphene oxide film was spread evenly on the bottom of a barrel-shaped container with a volume of 250 mL, with a thickness of 20 μm, to obtain a microwave plasma continuous emission device;
[0065] (2) After 1 g of the graphite oxide prepared in step (1) and 100 mL of water are stirred evenly, 5 g of nickel nitrate is added, the mixture is stirred evenly, and then dried at 50° C. for 48 h. The mixture is then laid in the microwave plasma continuous emission device obtained in step (1) with a thickness of 1 cm. The microwave plasma continuous emission device is then placed in a household microwave oven, the power is set to 800 W, and microwave treatment is performed for 3 seconds to obtain a nickel oxide / graphene composite material.
[0066] Example 4
[0067] A method for preparing a graphene-based material, comprising the following steps:
[0068] (1) The graphite oxide film prepared in step (1) of Example 1 was exposed to the outer flame of a flame for 2 seconds to obtain a continuous porous reduced graphene oxide film, and then 10 mg of the flame-reduced reduced graphene oxide film was spread evenly on the bottom of a barrel-shaped container with a volume of 250 mL, with a thickness of 20 μm, to obtain a microwave plasma continuous emission device;
[0069] (2) After 1 g of the graphite oxide prepared in step (1) and 100 mL of water are stirred evenly, 5 g of lithium cobalt oxide is added, the mixture is stirred evenly, and then dried at 50° C. for 48 h. The mixture is then laid in the microwave plasma continuous emission device obtained in step (1) with a thickness of 1 cm. The microwave plasma continuous emission device is then placed in a household microwave oven, the power is set to 800 W, and microwave treatment is performed for 3 seconds to obtain a lithium cobalt oxide / graphene composite material.
[0070] Example 5
[0071] A method for preparing graphene, comprising the following steps:
[0072] (1) Preparation of graphite oxide film by Hummers method in chemical exfoliation: 1 g of flake graphite and 0.5 g of sodium nitrate were weighed and placed in a 250 mL round-bottom flask, 23 mL of 98% by weight concentrated sulfuric acid was measured and added to the round-bottom flask, a magnet was added, the round-bottom flask was placed in an ice-water bath, and stirred for 30 min, 3 g of potassium permanganate was weighed and added to the reactor, and stirring was continued for 1 h. After the reaction was completed, the reactor was transferred to a 35° C. water bath and stirred for 30 min. , 50 mL of distilled water was measured and added to the round-bottom flask, and then the round-bottom flask was transferred to an oil bath at 98° C. and stirred for 15 min. 140 mL of distilled water and 10 mL of 30% H2O2 were added in sequence. After the reaction system finally turned bright yellow, centrifugation was performed, and then 500 mL of 5% HCl hydrochloric acid and distilled water were used to wash the solution until it became neutral. The solution was then placed on the surface of a watch glass and dried to obtain graphite oxide (oxygen atom content of 25 to 30 at.%) for later use;
[0073] The prepared graphite oxide film was taken and exposed to the outer flame of the flame for 2 seconds to obtain a continuous porous reduced graphene oxide film, and then 5 mg of the flame-reduced reduced graphene oxide film was spread evenly on the bottom of a barrel-shaped container with a volume of 100 mL, with a thickness of 25 μm, to obtain a microwave plasma continuous emission device;
[0074] (2) 2 g of the graphite oxide prepared in step (1) is laid in the microwave plasma continuous emission device obtained in step (1) with a thickness of 5 cm, and then the microwave plasma continuous emission device is placed in a household microwave oven, the power is set to 800 W, first microwave treatment for 3 seconds, let it stand and cool for 5 minutes, and then microwave treatment for 3 seconds to obtain graphene.
[0075] Example 6
[0076] A method for preparing graphene, which is different from that of Example 1 in that step (1) uses the Standenmaier method in a chemical exfoliation method to prepare graphite oxide: 17.5 mL of concentrated sulfuric acid and 9 mL of concentrated nitric acid are measured in a 250 mL flask and stirred for 15 min; 1 g of graphite is weighed and slowly added to the flask; after stirring, 11 g of potassium chlorate is added and reacted for 96 h; the graphite is washed with 800 mL of distilled water, then washed with 5% dilute hydrochloric acid, and finally washed with distilled water until neutral, and then placed on the surface of a watch glass and dried to obtain graphite oxide (oxygen atom content of 25 to 30 at.%) for standby use;
[0077] The remaining steps are the same as those in Example 1.
[0078] Example 7
[0079] A method for preparing graphene, comprising the following steps:
[0080] (1) The graphite oxide film prepared in step (1) of Example 1 was exposed to the outer flame of a flame for 1 second to obtain a continuous porous reduced graphene oxide film, and then 10 mg of the flame-reduced reduced graphene oxide film was spread evenly on the bottom of a barrel-shaped container with a volume of 250 mL, with a thickness of 20 μm, to obtain a microwave plasma continuous emission device;
[0081] (2) 2 g of the graphite oxide prepared in step (1) is laid in the microwave plasma continuous emission device obtained in step (1) with a thickness of 2 cm, and then the microwave plasma continuous emission device is placed in a household microwave oven, the power is set to 700 W, first microwave treatment for 3 seconds, let it stand and cool for 3 minutes, and then microwave treatment for 3 seconds to obtain graphene.
[0082] Example 8
[0083] A method for preparing graphene, comprising the following steps:
[0084] (1) The graphite oxide film prepared in step (1) of Example 1 was exposed to the outer flame of a flame for 3 seconds to obtain a continuous porous reduced graphene oxide film, and then 10 mg of the flame-reduced reduced graphene oxide film was spread evenly on the bottom of a barrel-shaped container with a volume of 100 mL, with a thickness of 40 μm, to obtain a microwave plasma continuous emission device;
[0085] (2) 2 g of the graphite oxide prepared in step (1) is laid in the microwave plasma continuous emission device obtained in step (1) with a thickness of 5 cm, and then the microwave plasma continuous emission device is placed in a household microwave oven, the power is set to 800 W, first microwave treatment for 3 seconds, let it stand and cool for 4 minutes, and then microwave treatment for 5 seconds to obtain graphene.
[0086] Test Case
[0087] Figure 1 This is an optical photograph of the microwave plasma continuous emission device prepared in Example 1 of the present invention; Figure 2 This is an optical photograph of the microwave plasma continuously generated by the microwave plasma continuous emission device prepared by the present invention before adding materials; Figure 3 This is an optical photograph of the microwave plasma continuous emission device prepared in Example 1 after adding materials; Figure 4 This is an optical photograph of the microwave plasma continuous emission device prepared in Example 1 after microwave treatment after adding materials; Figure 5 This is the XRD pattern of the manganese trioxide / graphene composite material prepared in Example 1; Figure 6 This is a SEM image of the manganese trioxide / graphene composite material prepared in Example 1; Figure 7 This is the XRD pattern of the hard carbon / graphene composite material prepared in Example 2; Figure 8SEM image of the hard carbon / graphene composite material prepared in implementation 2; Fig. 9 This is the XRD pattern of the nickel oxide / graphene composite material prepared in Example 3; Fig.10 This is a SEM image of the nickel oxide / graphene composite material prepared in Example 3; Fig.11 This is the XRD pattern of the lithium cobalt oxide / graphene composite material prepared in Example 4; Fig.12 This is a SEM image of the lithium cobalt oxide / graphene composite material prepared in Example 4; Fig.13 This is the XRD pattern of graphene prepared in Example 5; Fig.14 This is the SEM image of the graphene prepared in Example 5.
[0088] from Figure 1 It can be seen from the figure that the assembly of the microwave plasma continuous emission device is extremely simple. It only requires laying the reduced graphene oxide film on the bottom of the container. The technical strategy is simple and can be applied on a large scale. Figure 2 It can be seen from the figure that when the microwave plasma continuous emission device is placed in a microwave oven and microwave radiation is started, plasma can be continuously generated; Figure 3 It can be seen that it is only necessary to place the reactants on the surface of the reduced graphene oxide film without any special requirements and the operation is simple; Figure 4 It can be seen that after microwave treatment, the reactant changes from a gray block to a brick red, indicating that the reactant has been successfully processed and transformed into other substances; Figure 5 It can be seen that the XRD diffraction spectrum of the prepared material is consistent with that of manganese tetraoxide and manganese ore, indicating that manganese dioxide has been successfully transformed into a composite material of manganese tetraoxide, manganese ore and graphene; Figure 6 It can be seen that the prepared manganese trioxide / graphene composite material is composed of uniform micron particles attached to the film, indicating that the material has good uniformity; Figure 7 It can be seen that the XRD diffraction spectrum of the prepared material is consistent with that of hard carbon, and the diffraction peak of graphene is observed, indicating that the hard carbon / graphene composite material has been successfully prepared; Figure 8 It can be seen that the prepared hard carbon / graphene composite material is composed of uniform nanosheets attached to the film, indicating that the material has good uniformity; Fig. 9 It can be seen that the XRD diffraction spectrum of the prepared material is consistent with that of nickel oxide, and the diffraction peak of graphene is observed, indicating that the nickel oxide / graphene composite material has been successfully prepared; Fig.10 It can be seen that the prepared nickel oxide / graphene composite material is composed of uniform micron particles attached to the film, indicating that the material has good uniformity; Fig.11 It can be seen that the XRD diffraction spectrum of the prepared material is consistent with that of lithium cobalt oxide, and the diffraction peak of graphene is observed, indicating that the lithium cobalt oxide / graphene composite material has been successfully prepared; Fig.12 It can be seen that the prepared lithium cobalt oxide / graphene composite material is composed of uniform micron particles and thin films, indicating that the material has good uniformity; Fig.13 It can be seen that the XRD diffraction spectrum of the prepared material is consistent with that of graphene, indicating that graphene has been successfully prepared; Fig.14 It can be seen that the prepared graphene presents a transparent wrinkled film structure.
[0089] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a graphene-based material, comprising the following steps: (1) laying a continuous porous reduced graphene oxide film on the bottom of a barrel-shaped container to obtain a microwave plasma continuous emission device; (2) Laying the graphite oxide-based material in the microwave plasma continuous emission device obtained in step (1), performing microwave treatment, and obtaining the graphene-based material.
2. The method for preparing a graphene-based material according to claim 1, characterized in that: The thickness of the continuous porous reduced graphene oxide film in the step (1) is 15 to 40 μm.
3. The method for preparing a graphene-based material according to claim 1 or 2, characterized in that: The method for preparing the continuous porous reduced graphene oxide film in step (1) comprises: contacting the graphene oxide film with the outer flame of the flame and performing sintering reduction.
4. The method for preparing a graphene-based material according to claim 3, characterized in that: The temperature of the outer flame of the flame is 500-600°C.
5. The method for preparing a graphene-based material according to claim 3, characterized in that: The sintering reduction time is 1 to 3 seconds.
6. The method for preparing a graphene-based material according to claim 1, characterized in that: The graphite oxide-based material in step (2) is obtained by mixing graphite oxide and / or graphene oxide with an inorganic non-metallic material to be modified, and the mass ratio of the graphite oxide and / or graphene oxide to the inorganic non-metallic material to be modified is 1:(0-20).
7. The method for preparing a graphene-based material according to claim 6, characterized in that: The inorganic non-metallic material to be modified in step (2) includes one or more of non-metallic oxides, metal oxides, metal sulfides, metal hydroxides and metal salts.
8. The method for preparing a graphene-based material according to claim 1, characterized in that: The microwave treatment in step (2) is performed more than once, the duration of each microwave treatment is 3 to 10 seconds, and the time interval between two microwave treatments is 3 to 5 minutes.
9. The method for preparing a graphene-based material according to claim 1 or 8, characterized in that: The power of the microwave treatment in step (2) is 600-800W.
Citation Information
Patent Citations
Method for quickly preparing reduced graphene by using microwaves
CN102107870A
High-efficiency catalysis macroscopic quantity preparation method for graphene oxide or compound thereof reduced and peeled based on microwaves
CN106629689A
Preparation method for high-quality reduced graphene oxide by microwave auxiliary in trigger way
CN106865529A
Method for reducing oxidized graphene through microwave heating
CN109019578A
Graphene and preparation method thereof
CN109179387A