Pegmatite dissociation method

Through the method of acid leaching, chlorination and calcining and water quenching combined with rod grinding screening, the problem of impurity residue in pegmatite is solved, complete dissociation without mechanical external force is achieved, and the purity and stability of quartz sand is improved, which is satisfactory. Preparation requirements for high purity quartz sand.

CN118877899APending Publication Date: 2024-11-01HUNAN LIHUI NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410949963.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

In the existing pegmatite cleavage method, the external force of artificial hand hammer breaks causes impurities to remain, making it difficult to completely remove mica and feldspar, affecting the stability of purity of quartz sand.

Method used

Using acid leaching, chlorination and water quenching combined with rod grinding screening, the pegmatite cracks are dissolved by mixed acid liquid, expand the cleavage surface cracks, and then the pegmatite bursts through water quenching, and finally through rod grinding and color selection. Remove impurities and achieve complete dissociation without mechanical external force.

Benefits of technology

Quickly and effectively remove impurities in pegmatite, improve the purity of quartz sand, and meet the preparation needs of high-purity quartz sand, with low impurity content and high purity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118877899A_ABST
    Figure CN118877899A_ABST
Patent Text Reader

Abstract

The invention specifically discloses a pegmatite dissociation method, and relates to the technical field of mineral processing, the dissociation method comprises the following steps: S1, pre-prepared mixed acid is added into pegmatite for acid leaching, so that fractures of the pegmatite are completely impregnated with the mixed acid; s2, transferring the pegmatite subjected to acid leaching into a roasting furnace, performing chloridizing roasting at a preset temperature, and then performing water quenching on the pegmatite subjected to chloridizing roasting; and S3, the pegmatite subjected to water quenching is subjected to rod milling screening. According to the dissociation method, the pegmatite can be dissociated rapidly and effectively, the dissociated pegmatite is low in impurity content and high in purity, and the preparation requirement of high-purity quartz sand can be met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the technical field of mineral processing, and in particular relates to a method for dissociating pegmatite. Background Art

[0002] As competition in the crucible market becomes increasingly fierce, the quality and cost control of crucible products are particularly important. In the crucible industry, the requirements for the impurity content and purity of upstream quartz sand are getting higher and higher. As the main raw material for producing high-purity quartz sand, pegmatite has a great influence on the purity of quartz sand if it is completely cleaved. At present, the production of high-purity quartz sand using pegmatite basically relies on the external force of manual hammers to break and then cleave quartz, mica, feldspar and other impurities in pegmatite. This method causes a large amount of residual feldspar, mica and other impurities to adhere to the quartz. Even if the subsequent purification technology such as acid flotation is used for reprocessing, the impurities cannot be completely removed. Therefore, the residual feldspar, mica and other impurities cause the purity of quartz produced by pegmatite to be extremely unstable. In view of this, it is extremely urgent to study a new method for cleaving pegmatite. Summary of the invention

[0003] This application is made in view of the above technical problems and aims to provide a pegmatite dissociation method for removing impurities in pegmatite and thereby improving the purity of quartz sand.

[0004] In order to solve the above technical problems, the present application provides a pegmatite dissociation method, which comprises the following steps:

[0005] S1, adding the pre-prepared mixed acid into the pegmatite for acid leaching, so that the mixed acid can penetrate through the cracks of the pegmatite;

[0006] S2, transferring the acid-leached pegmatite to a roasting furnace, and performing chlorination roasting at a preset temperature, and then water quenching the chlorination roasted pegmatite;

[0007] S3. The water-quenched pegmatite is subjected to rod mill screening.

[0008] In some embodiments, the preformulated mixed acid refers to a mixture of hydrofluoric acid and hydrochloric acid in a volume ratio of 1:4.5-5.5.

[0009] In some embodiments, in step S2, the preset temperature in the roasting furnace is 400-600°C, the heating rate is 4-5min, and the holding time is 3-5h.

[0010] In some embodiments, in step S2, the pegmatite after chlorination roasting is placed in an ice-water mixture for water quenching.

[0011] In some implementations, step S3 specifically includes:

[0012] S31, sieving out 4-10 mesh particles from the water-quenched pegmatite and performing primary color sorting to remove large particle impurities;

[0013] S32, transferring the concentrate after primary color sorting to a rod mill and grinding it to 10-16 mesh, then sieving out 10-16 mesh particles and performing secondary color sorting;

[0014] S33, transferring the fine material after the secondary color sorting to a rod mill and grinding it to 16-26 mesh, then screening out the 16-26 mesh particles and performing tertiary color sorting.

[0015] In some embodiments, in step S1, the pegmatite after acid leaching needs to be cleaned with deionized water to clean the mixed acid on the surface of the pegmatite.

[0016] Compared with the prior art, the pegmatite dissociation method provided in this application has the following beneficial technical effects:

[0017] In this dissociation method, firstly, a mixed acid solution is used to penetrate into the cracks of the pegmatite and enter the cleavage plane for dissolution, and then the cleavage plane cracks of the pegmatite dissolution and weathering can be enlarged and accelerated by chlorination roasting, and then water quenching is used to make the pegmatite burst along the cleavage plane, so that part of the pegmatite is completely dissociated without being subjected to mechanical external force; finally, the pegmatite can be ground to the required particle size based on the rod mill, and at the same time, impurities such as feldspar and mica wrapped inside the pegmatite can be dissociated, and then the impurities can be selected by the color sorter, realizing the final dissociation of the pegmatite. Therefore, this dissociation method can quickly and effectively dissociate the pegmatite, and the dissociated pegmatite has a low impurity content and high purity, which can meet the preparation requirements of high-purity quartz sand. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 It is a flow chart of a pegmatite dissociation method in the present application. DETAILED DESCRIPTION

[0019] "Scope" disclosed in the present application is limited in the form of lower limit and upper limit, and a given range is limited by selecting a lower limit and an upper limit, and the selected lower limit and upper limit define the boundary of a special range. The scope limited in this way can be including end values ​​or not including end values, and can be arbitrarily combined, that is, any lower limit can be combined with any upper limit to form a scope. For example, if the scope of 60-120 and 80-110 is listed for a specific parameter, it is understood that the scope of 60-110 and 80-120 is also expected. In addition, if the minimum range values ​​1 and 2 are listed, and if the maximum range values ​​3, 4 and 5 are listed, the following scope can be all expected: 1-3, 1-4, 1-5, 2-3, 2-4 and 2-5. In the present application, unless otherwise specified, the numerical range "ab" represents the abbreviation of any real number combination between a and b, wherein a and b are real numbers. For example, the numerical range "0-5" means that all real numbers between "0-5" are listed in this document, and "0-5" is just an abbreviation of these numerical combinations. In addition, when a parameter is expressed as an integer ≥ 2, it is equivalent to disclosing that the parameter is, for example, an integer of 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, etc.

[0020] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.

[0021] If there is no special explanation, the "include" and "comprising" mentioned in this application are open-ended or closed-ended. For example, the "include" and "comprising" may mean that other components not listed may also be included or only the listed components may be included or only the listed components may be included.

[0022] If there is no special explanation, the pressure mentioned in this application is gauge pressure, which is gauge pressure = absolute pressure - standard atmospheric pressure. For example, if the evaporation decomposition pressure is 0.2 MPa, it means that the gauge pressure of the evaporation decomposition pressure is 0.2 MPa, and the absolute pressure is (0.2 + 0.1013) MPa.

[0023] If not specifically stated, in this application, the term "or" is inclusive. For example, the phrase "A or B" means "A, B, or both A and B". More specifically, any of the following conditions satisfies the condition "A or B": A is true (or exists) and B is false (or does not exist); A is false (or does not exist) and B is true (or exists); or both A and B are true (or exist).

[0024] In order to more clearly understand the above-mentioned objects, features and advantages of the present application, the present application is further described in detail below in conjunction with the accompanying drawings and specific embodiments. The additional embodiments and advantages of the present application will be partially given in the following description, and some will become apparent from the following description, or will be understood through practice. It should be noted that, in the absence of conflict, the embodiments of the present application and the features in the embodiments can be combined with each other, and the acids in the embodiments of the present application are all concentrated sulfuric acid.

[0025] like Figure 1 As shown, a pegmatite dissociation method comprises the following steps:

[0026] S1, adding the pre-prepared mixed acid into the pegmatite for acid leaching, so that the mixed acid can penetrate through the cracks of the pegmatite;

[0027] In this step, the pre-mixed acid is a mixture of hydrofluoric acid and hydrochloric acid in a volume ratio of 1:4.5-5.5, preferably a mixture of hydrofluoric acid and hydrochloric acid in a volume ratio of 1:5, wherein both the hydrofluoric acid and the hydrochloric acid can be chemically pure, analytically pure or premium pure. The mixed acid can enter the cleavage plane through the cracks of the pegmatite, and then dissolve the cleavage plane of the pegmatite.

[0028] S2, transferring the acid-leached pegmatite to a roasting furnace, and performing chlorination roasting at a preset temperature, and then water quenching the chlorination roasted pegmatite;

[0029] In this step, the preset temperature in the roasting furnace is 400-600° C., the heating rate is 4-5 min, and the holding time at the preset temperature is 3-5 h.

[0030] The specific steps are as follows: first, the acid-leached pegmatite is transferred to a roasting furnace, and the temperature is raised to a preset temperature of 400-600°C at a heating rate of 4-5 minutes, and the temperature is kept for 3-5 hours, and then the chlorinated roasted pegmatite is sent to an ice-water mixture for water quenching;

[0031] In the above embodiment, since most of the impurities in the pegmatite will generate melts above 600°C, these melts will adhere to quartz, which will make it difficult to remove the melt impurities adhering to quartz in subsequent processes. Therefore, the chlorination roasting temperature in the roasting furnace must be strictly controlled at 400-600°C, so as to ensure that the impurities in the pegmatite will not be vitrified and melted on the quartz, providing a guarantee for the low impurity content of the product after the dissociation of the pegmatite;

[0032] It should be noted that, since the mixed acid in the acid leaching process contains hydrochloric acid, the chlorinating agent will automatically volatilize during the roasting process, so there is no need to add chlorinating agent in the roasting furnace to obtain the pegmatite chlorination roasting atmosphere;

[0033] In the above embodiment, the pegmatite after chlorination roasting is quenched with ice-water mixture. Due to the difference in contraction coefficient between impurities and quartz, the pegmatite can easily burst along the cleavage plane of acid leaching, and some pegmatites can be completely dissociated without being subjected to external mechanical force.

[0034] In other embodiments, the pegmatite after chlorination roasting may be directly quenched with water at room temperature. Compared with water at room temperature, the quenching effect of ice-water mixture is better.

[0035] S3. The water-quenched pegmatite is subjected to rod mill screening.

[0036] This step specifically includes:

[0037] S31, sieving out 4-10 mesh particles from the water-quenched pegmatite and performing primary color sorting to remove large particle impurities, that is, removing large individual impurities such as large particles of feldspar and mica from the pegmatite through primary color sorting;

[0038] S32, transferring the concentrate after the primary color sorting to a rod mill and grinding it to 10-16 mesh, then screening out the 10-16 mesh particles and performing secondary color sorting, that is, removing the single impurities such as feldspar and mica that are secondary dissociated after the rod mill from the pegmatite through the secondary color sorting;

[0039] S33, the fine material after the secondary color sorting is transferred to the rod mill and rod-milled to 16-26 mesh, and then the 16-26 mesh particles are screened out and subjected to tertiary color sorting, that is, the impurities such as feldspar and mica separated after the second rod milling are completely removed from the pegmatite through the tertiary color sorting, thereby obtaining more than 99% pure quartz.

[0040] In the above implementation, the mixed acid solution is firstly used to penetrate into the cracks of the pegmatite and enter the cleavage plane for dissolution, and then the cleavage cracks of the pegmatite dissolution and weathering can be enlarged and accelerated by chlorination roasting, and then the pegmatite is made to burst along the cleavage plane by water quenching, so that part of the pegmatite is completely dissociated without being subjected to mechanical external force; finally, the pegmatite can be ground to the required particle size based on the rod mill, and at the same time, the impurities such as feldspar and mica wrapped in the pegmatite can also be separated, and then the impurities can be selected by the color sorter, so as to achieve the final dissociation of the pegmatite. Therefore, the dissociation method can quickly and effectively dissociate the pegmatite, and the dissociated pegmatite has a low impurity content and high purity, which can meet the preparation requirements of high-purity quartz sand.

[0041] In some embodiments, in step S1, the pegmatite after acid leaching needs to be cleaned with deionized water to clean the mixed acid on the surface of the pegmatite.

[0042] In the above embodiment, since the mixed acid may cause certain corrosion to the roasting furnace, the pegmatite after acid leaching needs to be cleaned with deionized water to clean the mixed acid on the surface of the pegmatite, thereby extending the service life of the roasting furnace to a certain extent.

[0043] In order to better illustrate the working principle and technical effect of the present application, three embodiments and one comparative example are provided below.

[0044] Example 1

[0045] (1) Take a pegmatite sample and put it into a mixed acid of hydrofluoric acid and hydrochloric acid with a volume ratio of 1:4.5 for acid leaching for 1 hour;

[0046] (2) transferring the acid-leached pegmatite to a roasting furnace for chlorination roasting, with a heating rate of 4°C / min, a preset roasting temperature of 400°C, and a holding time of 5h, and then rapidly quenching the chlorination roasted pegmatite in an ice-water mixture to cause the pegmatite to burst;

[0047] (3) Screening out 4-10 mesh particles from the water-quenched pegmatite and performing primary color sorting to remove large individual impurities such as large particles of feldspar and mica;

[0048] (4) The fine material after primary color sorting is transferred to a rod mill and rod-milled to 10-16 mesh, and then the 10-16 mesh particles are screened out and subjected to secondary color sorting, thereby removing single impurities such as feldspar and mica that are secondary dissociated after rod milling from the pegmatite;

[0049] (5) The fine material after the secondary color sorting is transferred to a rod mill and rod-milled to 16-26 mesh, and then the particles of 16-26 mesh are screened out and subjected to tertiary color sorting, and then the impurities such as feldspar and mica separated three times after the second rod mill are completely removed from the pegmatite to obtain separated quartz sand.

[0050] Example 2

[0051] (1) Take a pegmatite sample and put it into a mixed acid of hydrofluoric acid and hydrochloric acid with a volume ratio of 1:5 for acid leaching for 1.5 hours;

[0052] (2) transferring the acid-leached pegmatite to a roasting furnace for chlorination roasting, with a heating rate of 4.5°C / min, a preset roasting temperature of 500°C, and a holding time of 4h, and then rapidly quenching the chlorination roasted pegmatite in an ice-water mixture to cause the pegmatite to burst;

[0053] (3) Screening out 4-10 mesh particles from the water-quenched pegmatite and performing primary color sorting to remove large individual impurities such as large particles of feldspar and mica;

[0054] (4) The fine material after primary color sorting is transferred to a rod mill and rod-milled to 10-16 mesh, and then the 10-16 mesh particles are screened out and subjected to secondary color sorting, thereby removing single impurities such as feldspar and mica that are secondary dissociated after rod milling from the pegmatite;

[0055] (5) The fine material after the secondary color sorting is transferred to a rod mill and rod-milled to 16-26 mesh, and then the particles of 16-26 mesh are screened out and subjected to tertiary color sorting, and then the impurities such as feldspar and mica separated three times after the second rod mill are completely removed from the pegmatite to obtain separated quartz sand.

[0056] Example 3

[0057] (1) Take a pegmatite sample and put it into a mixed acid of hydrofluoric acid and hydrochloric acid with a volume ratio of 1:5.5 for acid leaching for 2 hours;

[0058] (2) transferring the acid-leached pegmatite to a roasting furnace for chlorination roasting, with a heating rate of 5°C / min, a preset roasting temperature of 600°C, and a holding time of 3h, and then rapidly quenching the chlorination roasted pegmatite in an ice-water mixture to cause the pegmatite to burst;

[0059] (3) Screening out 4-10 mesh particles from the water-quenched pegmatite and performing primary color sorting to remove large individual impurities such as large particles of feldspar and mica;

[0060] (4) The fine material after primary color sorting is transferred to a rod mill and rod-milled to 10-16 mesh, and then the 10-16 mesh particles are screened out and subjected to secondary color sorting, thereby removing single impurities such as feldspar and mica that are secondary dissociated after rod milling from the pegmatite;

[0061] (5) The fine material after the secondary color sorting is transferred to a rod mill and rod-milled to 16-26 mesh, and then the particles of 16-26 mesh are screened out and subjected to tertiary color sorting, and then the impurities such as feldspar and mica separated three times after the second rod mill are completely removed from the pegmatite to obtain separated quartz sand.

[0062] Comparative Example 1

[0063] A quantitative pegmatite sample is taken, and the pegmatite sample is broken by manual hammering. Then, impurities such as feldspar and mica are sorted out from the broken pegmatite sample to obtain dissociated quartz sand.

[0064] The quartz sand obtained from the three embodiments and one comparative example was analyzed by ICP detection, and the detection data are shown in Table 1.

[0065] Table 1 ICP test results of quartz sand obtained after dissociation of Examples 1-3 and Comparative Examples

[0066]

[0067]

[0068] As can be seen from Table 1, compared with the quartz sand obtained in the comparative example, the impurity content in the quartz sand obtained in Examples 1-3 is less, especially, the potassium and sodium content in the quartz sand obtained in the comparative example is higher, wherein the potassium content is 11% and the sodium content is 9.98%, while the potassium content in the quartz sand obtained in Examples 1-3 is only 0.36%, and the sodium content is only 0.91%. It can be seen that a large amount of feldspar remains in the pegmatite in the comparative example after purification, while the feldspar content in the pegmatite in Examples 1-3 is very small after purification. Therefore, the pegmatite dissociation method provided in the present application can quickly and effectively dissociate the pegmatite, and the dissociated pegmatite has a low impurity content and high purity, which can meet the requirements of the sand in the crucible.

[0069] The above is a detailed introduction to a pegmatite dissociation method provided by the present application. Specific examples are used in this article to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the core idea of ​​the present application. It should be pointed out that for ordinary technicians in this technical field, without departing from the principles of the present application, several improvements and modifications can be made to the present application, and these improvements and modifications also fall within the scope of protection of the claims of the present application.

Claims

1. A method for dissociating pegmatite, characterized in that: The method comprises the following steps: S1, adding the pre-prepared mixed acid into the pegmatite for acid leaching, so that the mixed acid can penetrate through the cracks of the pegmatite; S2, transferring the acid-leached pegmatite to a roasting furnace, and performing chlorination roasting at a preset temperature, and then water quenching the chlorination roasted pegmatite; S3. The water-quenched pegmatite is subjected to rod mill screening.

2. The pegmatite dissociation method according to claim 1, characterized in that: The pre-mixed acid refers to a mixture of hydrofluoric acid and hydrochloric acid in a volume ratio of 1:4.5-5.

5.

3. The pegmatite dissociation method according to claim 2, characterized in that: In step S2, the preset temperature in the roasting furnace is 400-600°C, the heating rate is 4-5min, and the insulation time is 3-5h.

4. The pegmatite dissociation method according to claim 3, characterized in that: In the step S2, the pegmatite after chlorination roasting is placed in an ice-water mixture for water quenching.

5. The pegmatite dissociation method according to claim 4, characterized in that: The step S3 specifically includes: S31, sieving out 4-10 mesh particles from the water-quenched pegmatite and performing primary color sorting to remove large particle impurities; S32, transferring the concentrate after primary color sorting to a rod mill and grinding it to 10-16 mesh, then sieving out 10-16 mesh particles and performing secondary color sorting; S33, transferring the fine material after the secondary color sorting to a rod mill and grinding it to 16-26 mesh, then screening out the 16-26 mesh particles and performing tertiary color sorting.

6. The pegmatite dissociation method according to claim 5, characterized in that: In the step S1, the pegmatite after acid leaching needs to be cleaned with deionized water to clean the mixed acid on the surface of the pegmatite.

Citation Information

Patent Citations

  • High-purity quartz sand purification cleaning machine

    CN111170322A

  • Quartz sandstone high-value comprehensive utilization method

    CN111841829A

  • Method for preparing 4N8-grade high-purity quartz sand from pegmatite quartz

    CN117623320A

  • Selective crushing method of granite pegmatite and high-purity quartz sand raw material

    CN118047385A

  • Method for producing a highly pure quartz granulate

    US20120103017A1